A MOF-based polymer hollow fiber composite membrane, its preparation method and application

By introducing a SIFSIX-3-Ni layer onto a polymer hollow fiber membrane, a synergistic effect between a dense selective layer and a polyphenylsulfone support layer is achieved, solving the problem of balancing selectivity and permeability in hydrogen separation of polymer membranes. This results in high permeation flux and structural stability, while reducing preparation costs.

CN123102169APending Publication Date: 2026-11-17INNER MONGOLIA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611604491.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polymer membranes struggle to balance high selectivity and high permeability in hydrogen separation, and their stability is insufficient, making it difficult to meet demanding separation conditions.

Method used

The preparation method of MOF-based polymer hollow fiber composite membrane is adopted. By introducing a SIFSIX-3-Ni layer on the polymer hollow fiber membrane, a dense selective layer and a polyphenylsulfone support layer are formed, which can enhance the hydrogen permeation flux and improve the membrane structure stability.

Benefits of technology

It significantly improves hydrogen permeation flux, reduces mass transfer resistance, solves the trade-off between gas selectivity and permeability, enhances membrane structural stability and lifespan, and reduces preparation costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102169A_ABST
    Figure CN123102169A_ABST
Patent Text Reader

Abstract

This invention discloses a MOF-based polymer hollow fiber composite membrane, its preparation method, and its application, relating to the field of hydrogen separation membrane preparation technology. The method includes the following steps: S1: preparing a polymer spinning solution; S2: preparing an internal coagulant; S3: using the NIPS method, co-extruding the polymer spinning solution and the internal coagulant through a spinneret, then introducing them into a water bath system for phase inversion molding to obtain a polymer hollow fiber membrane; S4: introducing SIFSIX-3-Ni onto the polymer hollow fiber membrane using a coating method or in-situ growth method; S5: post-treating the SIFSIX-3-Ni-introduced polymer hollow fiber membrane to remove residual moisture, thus obtaining the final product. The MOF-based polymer hollow fiber composite membrane of this invention exhibits excellent thermal stability and long-term operational stability, and can be used for hydrogen separation at high temperatures, effectively overcoming the "permeability-selectivity" trade-off effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of hydrogen separation membrane preparation technology, specifically to a MOF-based polymer hollow fiber composite membrane, its preparation method, and its application. Background Technology

[0002] Hollow fiber membrane separation technology for hydrogen, with its advantages of high efficiency, energy saving, and modularity, has become a core process for hydrogen purification and refining. Relying on membrane materials with extremely fine pores, it rapidly and accurately separates hydrogen from impurity gases, ensuring hydrogen quality and providing a high-purity gas source for applications such as fuel cells. It is a key link in reducing costs and increasing efficiency in the hydrogen energy industry chain.

[0003] Membrane separation methods are generally classified into inorganic membranes, polymer membranes, and metal membranes. Polymer membranes are prone to plasticization, have difficulty balancing flux and selectivity, and lack stability, making them unsuitable for demanding separation conditions. Introducing MOFs can improve sieving accuracy and gas flux by utilizing their regularized channels, enhance membrane structural stability, suppress plasticization, and achieve a breakthrough in separation performance, making them suitable for high-efficiency hydrogen separation. Summary of the Invention

[0004] To address the above-mentioned problems, this invention provides a MOF-based polymer hollow fiber composite membrane, its preparation method, and its application.

[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0006] This invention provides a method for preparing a MOF-based polymer hollow fiber composite membrane, specifically including the following steps:

[0007] S1: Add polyphenylsulfone particles to N-methylpyrrolidone, stir to dissolve and disperse evenly to obtain a polymer spinning solution;

[0008] S2: Mix N-methylpyrrolidone with deionized water until homogeneous to obtain an internal coagulant;

[0009] S3: Using the NIPS method, the polymer spinning solution and the internal coagulant are extruded together through the spinning head and then enter the water bath system to undergo phase inversion and molding, thus obtaining a polymer hollow fiber membrane.

[0010] S4: SIFSIX-3-Ni is introduced onto the polymer hollow fiber membrane obtained in step S3, wherein the introduction method is either coating or in-situ growth.

[0011] S5: The polymer hollow fiber membrane with SIFSIX-3-Ni introduced is post-treated to remove residual moisture from the membrane, thus obtaining the MOF-based polymer hollow fiber composite membrane.

[0012] Further, step S1 specifically involves: adding polyphenylsulfone particles to an N-methylpyrrolidone (NMP) solution, stirring at 40°C and 300 r / min for 12 hours to disperse evenly, then sonicating for 10 minutes to defoam, obtaining a polymer spinning solution, loading it into the first injection pump 1 and evacuating it for 1 hour for later use; the solid-liquid ratio of polyphenylsulfone to N-methylpyrrolidone is 6 g: 17.5 mL.

[0013] Further, step S2 specifically involves mixing deionized water and N-methylpyrrolidone (NMP) solution at a volume ratio of 1:1 to obtain an internal coagulant, which is then loaded into the second injection pump 2 for later use.

[0014] Further, step S3 specifically involves connecting a first injection pump 1 containing a polymer spinning solution and a second injection pump 2 containing an internal coagulant to the top and side of the spinning head, respectively. After being extruded through the spinning head, the solution enters the water to form a tubular hollow fiber membrane. After standing in tap water for 24 hours, the membrane is dried at room temperature for 24 hours to obtain a polymer hollow fiber membrane.

[0015] Further, in step S4, the coating method specifically includes:

[0016] S41A: Ni(BF4)2 Add 6H2O to a mixture of methanol and deionized water, and stir magnetically for 15 minutes until completely dissolved to obtain solution A; the Ni(BF4)2 The volume ratio of 6H2O to the mixed solution is 0.0004 mol: 10 mL; the volume ratio of methanol to deionized water in the mixed solution is 1:1.

[0017] S42A: Ammonium hexafluorosilicate and pyrazine are added to a mixture of methanol and deionized water, and the mixture is magnetically stirred for 15 min until completely dissolved to obtain solution B; the Ni(BF4)2 The molar ratio of 6H2O, ammonium hexafluorosilicate, and pyrazine is 1:1:2; the volume ratio of pyrazine to the mixture is 0.0008 mol: 10 mL.

[0018] S43A: Solution A was slowly added to solution B at a rate of 1 drop / second. After the addition was complete, the solution was placed at room temperature of 25°C for 24 hours, centrifuged at 9000 r / min, washed three times with methanol, and dried under vacuum at 80°C for 12 hours to obtain SIFSIX-3-Ni powder (MOF material).

[0019] S44A: SIFSIX-3-Ni powder is dissolved in deionized water to form a SIFSIX-3-Ni solution; the solid-liquid ratio of SIFSIX-3-Ni powder to deionized water is 2g:100mL;

[0020] S45A: Seal both ends of the dried polymer hollow fiber membrane with epoxy resin and dry it. Then immerse it in SIFSIX-3-Ni solution for 3 minutes and take it out for 1 minute. Repeat this process 3 times to obtain the final product.

[0021] Further, in step S4, the in-situ growth method specifically refers to:

[0022] S41B: Ni(BF4)2 Add 6H2O to a mixture of methanol and deionized water, stir magnetically for 15 minutes until completely dissolved, to obtain solution C; the Ni(BF4)2 The volume ratio of 6H2O to the mixed solution is 0.01 mol: 100 mL; the volume ratio of methanol to deionized water in the mixed solution is 1:1.

[0023] S42B: Ammonium hexafluorosilicate and pyrazine are added to a mixture of methanol and deionized water and magnetically stirred for 15 min until completely dissolved to obtain solution D; the Ni(BF4)2 The molar ratio of 6H2O, ammonium hexafluorosilicate, and pyrazine is 1:1:2; the volume ratio of pyrazine to the mixture is 0.02 mol: 100 mL.

[0024] S43B: Ni(BF4)2 6H2O, ammonium hexafluorosilicate, and pyrazine were added to a mixture of methanol and deionized water and magnetically stirred for 15 minutes until completely dissolved to obtain solution E; the Ni(BF4)2 The molar ratio of 6H2O, ammonium hexafluorosilicate, and pyrazine is 1:1:2; the volume ratio of pyrazine to the mixture is 0.015 mol: 100 mL.

[0025] S44B: After drying, seal both ends of the polymer hollow fiber membrane with epoxy resin and dry it. Then, immerse it in solution C for 4 hours and dry it overnight in an oven at 40°C. Next, immerse the dried polymer hollow fiber membrane in solution D for 2 hours. After removing the membrane, gently rinse the surface with methanol and air dry it naturally for 30 minutes. Finally, immerse the dried polymer hollow fiber membrane in solution E at room temperature for 3 hours to obtain the final product.

[0026] Further, in step S5, when the coating method is used, the post-treatment is as follows: the polymer hollow fiber membrane with SIFSIX-3-Ni introduced is soaked in anhydrous methanol solution for 24 hours and then dried at room temperature; when the in-situ growth method is used, the post-treatment is as follows: the polymer hollow fiber membrane with SIFSIX-3-Ni introduced is washed twice with methanol, then washed once with deionized water, and then dried in a vacuum drying oven at 40°C for 6 hours.

[0027] The present invention also provides a MOF-based polymer hollow fiber composite membrane, which includes an outer dense selective layer formed of SIFSIX-3-Ni and an inner polyphenylsulfone support.

[0028] The present invention also provides an application of a MOF-based polymer hollow fiber composite membrane for H2 separation.

[0029] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0030] This invention introduces the unique porous structure and designability of metal-organic frameworks (MOFs) into polymer materials, providing a MOF-based polymer hollow fiber composite membrane with high selectivity and permeability for hydrogen (H2). First, the MOF-polymer hollow fiber composite membrane prepared by this invention exhibits a synergistic effect between its outer dense MOF layer and inner polyphenylsulfone (PPSU) support layer. Compared to traditional polymer membranes, this effectively reduces hydrogen permeation mass transfer resistance and significantly increases hydrogen permeation flux, providing a new approach to breaking through the Robertson limit and solving the trade-off between gas selectivity and permeability. Second, this invention uses polyphenylsulfone (PPSU) as the support layer, fully utilizing its excellent mechanical strength, good chemical stability, and environmental friendliness to ensure the structural stability and service life of the hydrogen separation membrane in practical applications. Finally, the polymer substrate used in this invention is widely available and inexpensive, significantly reducing the overall cost of membrane material preparation and the hydrogen separation process, greatly enhancing its potential for industrial application. Attached Figure Description

[0031] Figure 1 This invention relates to a spinning device for preparing polymer hollow fiber membranes. In the figure: 1, first injection pump; 2, second injection pump; 3, spinning head; 4, tap water solution.

[0032] Figure 2 This is a diagram illustrating the separation mechanism of hydrogen using the MOF-based polymer hollow fiber composite membrane of this invention.

[0033] Figure 3 This is a diagram of the apparatus for separating hydrogen using a MOF-based polymer hollow fiber composite membrane according to the present invention. Detailed Implementation

[0034] To make the objectives and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are only for explaining the invention and are not intended to limit the invention.

[0035] Unless otherwise specified, the instruments, reagents, and materials used in the following embodiments are all conventional instruments, reagents, and materials already available in the prior art and can be obtained through legitimate commercial channels. Unless otherwise specified, the experimental methods and detection methods used in the following embodiments are all conventional experimental methods and detection methods already available in the prior art.

[0036] Example 1

[0037] This embodiment provides a MOF-based polymer hollow fiber composite membrane, which is prepared by the following method:

[0038] S1: Add 6g of polyphenylsulfone particles to 17.5mL of NMP solution, stir at 40℃ and 300r / min for 12h to disperse evenly, then sonicate for 10min to defoam, and obtain polymer spinning solution, which is then loaded into the first injection pump 1 and vacuumed for 1h.

[0039] S2: After mixing deionized water and NMP solution at a volume ratio of 1:1, an internal coagulant is obtained and loaded into the second injection pump 2.

[0040] S3: Using the NIPS method in spinning equipment (see...) Figure 1 The process includes a first injection pump 1, a second injection pump 2, a spinning head 3, and a tap water solution 4. The first injection pump 1, which contains a polymer spinning solution, and the second injection pump 2, which contains an internal coagulant, are connected to the top and side of the spinning head, respectively. After being extruded through the spinning head, the solution enters the water to form a tubular hollow fiber membrane. After standing in tap water for 24 hours, the membrane is dried at room temperature for 24 hours to obtain a polymer hollow fiber membrane.

[0041] S4: SIFSIX-3-Ni is introduced onto the polymer hollow fiber membrane using a coating method or an in-situ growth method, specifically:

[0042] S41: Add 135mg Ni(BF4)2 Add 6H2O to a mixture of 5 mL methanol and 5 mL deionized water, stir magnetically for 15 min until completely dissolved, to obtain solution A;

[0043] S42: Add 72 mg of ammonium hexafluorosilicate and 64.8 mg of pyrazine to a mixture of 5 mL of methanol and 5 mL of deionized water, and stir magnetically for 15 min until completely dissolved to obtain solution B;

[0044] S43: Using a pipette, slowly add solution A to solution B at a rate of 1 drop / second. After the addition is complete, place at room temperature of 25°C for 24 hours, centrifuge at 9000 r / min, wash three times with methanol, and vacuum dry at 80°C for 12 hours to obtain SIFSIX-3-Ni powder (MOF material).

[0045] S44: Dissolve 2g of SIFSIX-3-Ni powder in 100mL of deionized water to form a SIFSIX-3-Ni solution;

[0046] S45: Seal both ends of the dried polymer hollow fiber membrane with epoxy resin and dry it. Then immerse it in SIFSIX-3-Ni solution for 3 minutes and take it out for 1 minute. Repeat this process 3 times to obtain the final product.

[0047] S5: The polymer hollow fiber membrane with SIFSIX-3-Ni introduced is soaked in anhydrous methanol solution for 24 hours, and then dried at room temperature to remove residual moisture from the membrane, thus obtaining the MOF-based polymer hollow fiber composite membrane.

[0048] Example 2

[0049] This embodiment provides a MOF-based polymer hollow fiber composite membrane, which is prepared by the following method:

[0050] S1: Add 6g of polyphenylsulfone particles to 17.5mL of NMP solution, stir at 40℃ and 300r / min for 12h to disperse evenly, then sonicate for 10min to defoam, and obtain polymer spinning solution, which is then loaded into the first injection pump 1 and vacuumed for 1h.

[0051] S2: After mixing deionized water and NMP solution at a volume ratio of 1:1, an internal coagulant is obtained and loaded into the second injection pump 2.

[0052] S3: Using the NIPS method, a first injection pump 1 containing a polymer spinning solution and a second injection pump 2 containing an internal coagulant are connected to the top and side of the spinning head, respectively. After being extruded through the spinning head, the solution enters the water to form a tubular hollow fiber membrane. After standing in tap water for 24 hours, the membrane is dried at room temperature for 24 hours to obtain a polymer hollow fiber membrane.

[0053] S4: SIFSIX-3-Ni is introduced onto the polymer hollow fiber membrane using a coating method or an in-situ growth method, specifically:

[0054] S41: 3400mg Ni(BF4)2 Add 6H2O to a mixture of 50 mL methanol and 50 mL deionized water, stir magnetically for 15 min until clear, to obtain solution C;

[0055] S42: Add 1780 mg of ammonium hexafluorosilicate and 1602 mg of pyrazine to a mixture of 50 mL of methanol and 50 mL of deionized water, and stir magnetically for 15 min until completely dissolved to obtain solution D;

[0056] S43: 2550mg Ni(BF4)2 6H2O, 1350mg ammonium hexafluorosilicate and 1201.5mg pyrazine were added to a mixture of 50mL methanol and 50mL deionized water and magnetically stirred for 15min until transparent to obtain solution E;

[0057] S44: After drying, seal both ends of the polymer hollow fiber membrane with epoxy resin and dry it. Then, immerse it in solution C for 4 hours and dry it overnight in an oven at 40°C. Next, immerse the dried polymer hollow fiber membrane in solution D for 2 hours. After removing the membrane, gently rinse the surface with methanol and air dry it for 30 minutes to form a SIFSIX-3-Ni layer on the outer surface of the polymer hollow fiber membrane. Finally, immerse the polymer hollow fiber membrane that has undergone one growth treatment in solution E at room temperature for 3 hours to obtain the final product.

[0058] S5: The polymer hollow fiber membrane with SIFSIX-3-Ni introduced is washed twice with methanol and once with deionized water. It is then placed in a vacuum drying oven at 40°C for 6 hours to remove residual moisture from the membrane, thus obtaining the MOF-based polymer hollow fiber composite membrane.

[0059] See attached diagram for the separation mechanism of MOF-based polymer hollow fiber composite membranes. Figure 2 The separation principle of MOF-containing polymer hollow fiber membranes used for hydrogen separation is as follows: the SIFSIX-3-Ni layer generated on the surface of the polymer hollow fiber membrane has a selective effect, which allows a mixed gas containing H2 and N2 to pass through the dense layer of the SIFSIX-3-Ni layer and be sieved according to the different sizes of gas molecules, so that the smaller H2 molecules can pass through into the PPSU layer, thus achieving the effect of hydrogen separation.

[0060] Experimental Example 1

[0061] A diagram of the testing setup for MOF-based polymer hollow fiber composite membranes used for hydrogen separation is attached. Figure 3 The apparatus consists of a gas chromatograph, a horizontal tube furnace, gas supply lines, a hydrogen separation membrane, a mass flow meter, and a tail gas treatment unit. MOF-based polymer hollow fiber composite membranes prepared in Examples 1 and 2 were installed at the intermediate interface of the self-made testing apparatus and sealed with sealant to ensure overall airtightness. The testing apparatus was placed in the horizontal tube furnace and kept at room temperature without heating. A 1:1 H2-N2 mixture was used as the feed gas in this experiment, introduced into the feed side of the membrane separation device; argon gas was used as the carrier gas on the purge side. The tail gas generated on the purge side was connected to the gas chromatograph via pipeline for real-time analysis of the gas composition. During the experiment, the flow rates of both H2 and N2 were controlled at 25 mL. min -1 Ar purge gas flow rate is 50 mL min -1The flow rate of each gas stream is precisely controlled by a mass flow meter.

[0062] Experiment Example 2

[0063] The MOF-based polymer hollow fiber composite membranes prepared in Examples 1 and 2 were heated in a horizontal tube furnace at 2°C. min -1 The temperature was increased to 80°C at a heating rate, and the remaining experimental conditions were the same as in Experiment 1. The H2 separation permeability test was then conducted.

[0064] Experimental Example 3

[0065] The MOF-based polymer hollow fiber composite membranes prepared in Examples 1 and 2 were heated in a horizontal tube furnace at 2°C. min -1 The temperature was increased to 100℃ at a heating rate, and the remaining experimental conditions were the same as in Experiment 1, to test the H2 separation permeability.

[0066] Experiment Example 4

[0067] The MOF-based polymer hollow fiber composite membranes prepared in Examples 1 and 2 were heated in a horizontal tube furnace at 2°C. min -1 The temperature was increased to 120°C at a heating rate, and the remaining experimental conditions were the same as in Experiment 1. The permeability test of H2 separation was carried out for 100 hours.

[0068] Experimental Example 5

[0069] The MOF-based polymer hollow fiber composite membranes prepared in Examples 1 and 2 were heated in a horizontal tube furnace at 2°C. min -1 The temperature was increased to 140℃ at a heating rate, and the remaining experimental conditions were the same as in Experiment 1, to test the H2 separation permeability.

[0070] Table 1. H2 permeation flux and selectivity for Experiments 1-5

[0071]

[0072] The MOF-based polymer hollow fiber composite membrane prepared in this embodiment can be used for high-purity hydrogen separation. As shown in Table 1, Example 1, the composite membrane exhibits excellent hydrogen permeation flux at room temperature, indicating that the introduced MOF material effectively improves the insufficient permeation performance of the base membrane. Table 1 also shows that the hydrogen permeation flux increases with increasing temperature, confirming that the hydrogen transport process within the membrane is controlled by a thermal activation mechanism. Based on the results of Example 5, the hydrogen separation membrane can operate stably and continuously for 100 hours at a high temperature of 140°C, demonstrating the excellent thermal stability of the prepared MOF-based polymer hollow fiber composite membrane.

[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a MOF-based polymeric hollow fiber composite membrane, characterized by: Specifically, the following steps are included: S1: Add polyphenylsulfone particles to N-methylpyrrolidone, stir to dissolve and disperse evenly to obtain a polymer spinning solution; S2: Mix N-methylpyrrolidone with deionized water until homogeneous to obtain an internal coagulant; S3: Using the NIPS method, the polymer spinning solution and the internal coagulant are extruded together through the spinning head and then enter the water bath system to undergo phase inversion and molding, thus obtaining a polymer hollow fiber membrane. S4: Introduce SIFSIX-3-Ni onto the polymer hollow fiber membrane obtained in step S3 by coating or in-situ growth. S5: The polymer hollow fiber membrane with SIFSIX-3-Ni introduced is post-treated to remove residual moisture from the membrane, thus obtaining the MOF-based polymer hollow fiber composite membrane.

2. The method of claim 1, wherein: The specific steps of step S1 are as follows: polyphenylsulfone particles are added to N-methylpyrrolidone solution, stirred at 40°C and 300r / min for 12 hours to disperse evenly, and then ultrasonically defoamed for 10 minutes to obtain polymer spinning solution, which is then loaded into the first injection pump (1) and vacuumed for 1 hour for later use; the solid-liquid ratio of polyphenylsulfone to N-methylpyrrolidone is 6g:17.5mL.

3. The method of claim 1, wherein: The specific step S2 is as follows: after mixing deionized water with N-methylpyrrolidone solution at a volume ratio of 1:1, an internal coagulant is obtained and loaded into the second injection pump (2) for later use.

4. The method of claim 1, wherein: The specific steps of step S3 are as follows: the first injection pump (1) containing the polymer spinning solution and the second injection pump (2) containing the internal coagulant are connected to the top and side of the spinning head, respectively. After being extruded through the spinning head, the solution enters the water to form a tubular hollow fiber membrane. After standing in tap water for 24 hours, the membrane is dried at room temperature for 24 hours to obtain the polymer hollow fiber membrane.

5. The preparation method according to claim 1, characterized in that: Step S4, the coating method specifically includes: S41A: Ni(BF4)2 Add 6H2O to a mixture of methanol and deionized water, and stir magnetically for 15 minutes until completely dissolved to obtain solution A; the Ni(BF4)2 The volume ratio of 6H2O to the mixed solution is 0.0004 mol: 10 mL; the volume ratio of methanol to deionized water in the mixed solution is 1:

1. S42A: Ammonium hexafluorosilicate and pyrazine are added to a mixture of methanol and deionized water, and the mixture is magnetically stirred for 15 min until completely dissolved to obtain solution B; the Ni(BF4)2 The molar ratio of 6H2O, ammonium hexafluorosilicate, and pyrazine is 1:1:2; the volume ratio of pyrazine to the mixture is 0.0008 mol: 10 mL. S43A: Solution A was slowly added to solution B at a rate of 1 drop / second. After the addition was complete, the solution was placed at room temperature of 25°C for 24 hours, centrifuged at 9000 r / min, washed three times with methanol, and dried under vacuum at 80°C for 12 hours to obtain SIFSIX-3-Ni powder. S44A: SIFSIX-3-Ni powder is dissolved in deionized water to form a SIFSIX-3-Ni solution; the solid-liquid ratio of SIFSIX-3-Ni powder to deionized water is 2g:100mL; S45A: Seal both ends of the dried polymer hollow fiber membrane with epoxy resin and dry it. Then immerse it in SIFSIX-3-Ni solution for 3 minutes and take it out for 1 minute. Repeat this process 3 times to obtain the final product.

6. The preparation method according to claim 1, characterized in that: In step S4, the in-situ growth method specifically refers to: S41B: Ni(BF4)2 Add 6H2O to a mixture of methanol and deionized water, stir magnetically for 15 minutes until completely dissolved, to obtain solution C; the Ni(BF4)2 The volume ratio of 6H2O to the mixed solution is 0.01 mol: 100 mL; the volume ratio of methanol to deionized water in the mixed solution is 1:

1. S42B: Ammonium hexafluorosilicate and pyrazine are added to a mixture of methanol and deionized water and magnetically stirred for 15 min until completely dissolved to obtain solution D; the Ni(BF4)2 The molar ratio of 6H2O, ammonium hexafluorosilicate, and pyrazine is 1:1:2; the volume ratio of pyrazine to the mixture is 0.02 mol: 100 mL. S43B: Ni(BF4)2 6H2O, ammonium hexafluorosilicate, and pyrazine were added to a mixture of methanol and deionized water and magnetically stirred for 15 minutes until completely dissolved to obtain solution E; the Ni(BF4)2 The molar ratio of 6H2O, ammonium hexafluorosilicate, and pyrazine is 1:1:2; the volume ratio of pyrazine to the mixture is 0.015 mol: 100 mL. S44B: After drying, seal both ends of the polymer hollow fiber membrane with epoxy resin and dry it. Then, immerse it in solution C for 4 hours and dry it overnight in an oven at 40°C. Next, immerse the dried polymer hollow fiber membrane in solution D for 2 hours. After removing the membrane, gently rinse the surface with methanol and air dry it naturally for 30 minutes. Finally, immerse the dried polymer hollow fiber membrane in solution E at room temperature for 3 hours to obtain the final product.

7. The preparation method according to claim 1, characterized in that: In step S5, when the coating method is used, the post-treatment is as follows: the polymer hollow fiber membrane with SIFSIX-3-Ni introduced is soaked in anhydrous methanol solution for 24 hours and then dried at room temperature; when the in-situ growth method is used, the post-treatment is as follows: the polymer hollow fiber membrane with SIFSIX-3-Ni introduced is washed twice with methanol, then washed once with deionized water, and then dried in a vacuum drying oven at 40°C for 6 hours.

8. The MOF-based polymer hollow fiber composite membrane prepared by any one of the preparation methods described in claims 1-7, characterized in that: The MOF-based polymer hollow fiber composite membrane comprises an outer dense selective layer formed of SIFSIX-3-Ni and an inner polyphenylsulfone support.

9. The application of the MOF-based polymer hollow fiber composite membrane as described in claim 8, characterized in that: The MOF-based polymer hollow fiber composite membrane is used for H2 separation.