Defect-induced covalent organic framework layer-mediated polyamide composite membranes, their preparation methods and applications
By designing a multi-layered defective covalent organic framework layer-mediated polyamide composite membrane, the problem of increased mass transfer resistance caused by membrane fouling was solved, achieving a balance between anti-fouling and permeability in high-salt wastewater treatment, and making it suitable for complex high-salt wastewater and seawater desalination.
Patent Information
- Application Number
- CN202611628648.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-21
- Publication Date
- 2026-11-17
AI Technical Summary
In existing membrane distillation technologies for treating high-salinity wastewater, membrane scaling increases mass transfer resistance, affecting operational stability and permeability, making it difficult to simultaneously improve anti-scaling performance and permeability.
A multilayer defect covalent organic framework-mediated polyamide composite membrane is designed, comprising a hydrophobic PVDF microporous membrane, a pore defect covalent organic framework intermediate layer, and a dense polyamide sieved surface layer, formed through interfacial polymerization and thermal crosslinking, thereby optimizing the membrane's anti-fouling performance and permeability.
It significantly improves the membrane's anti-fouling performance and permeability, ensuring long-term stable operation of the membrane in high-salinity wastewater treatment, and is suitable for complex high-salinity wastewater and seawater desalination applications.
Smart Images

Figure CN123102175A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of membrane distillation technology, and in particular to a defect covalent organic framework layer-mediated polyamide composite membrane, its preparation method, and its application. Background Technology
[0002] Membrane distillation (MD) has become a promising technology for treating high-salinity wastewater and achieving zero discharge (ZLD) due to its excellent tolerance to high-salinity feed streams, theoretical ability to completely remove salt, and compatibility with low-grade or waste heat resources under mild operating conditions.
[0003] Currently, we have projects in severely water-scarce regions such as the Middle East and North Africa, as well as in the treatment of high-mineralization mine water and power plant wastewater in western my country.
[0004] However, high-salt wastewater is usually complex in composition, and continuous MD process evaporation and concentration will gradually increase the solute concentration at the membrane-feed interface, thereby inducing the nucleation, growth and deposition of inorganic crystals on the membrane surface and in the membrane pores.
[0005] This inorganic scale layer significantly increases the mass transfer resistance of the membrane and affects the operational stability of the MD system.
[0006] More seriously, scaling on the membrane can lead to wetting of the pores, ultimately causing degradation or even complete loss of water / salt separation performance.
[0007] Therefore, suppressing pore wetting caused by scaling is widely considered to be one of the key prerequisites for the large-scale and sustainable application of MD technology.
[0008] Composite membranes that integrate high-density polyamide functional layers with hydrophobic substrates are expected to reduce pore wetting caused by scaling during the MD process of high-salt wastewater.
[0009] However, hydrophobic porous substrates are prone to defects in polyamide layers, while introducing an intermediate layer increases mass transfer resistance.
[0010] Therefore, it is necessary to design and develop composite membranes that combine excellent anti-scaling properties with good permeability, thereby overcoming the trade-off between scaling resistance and permeability and promoting the application of MD technology in the field of high-salinity wastewater treatment. Summary of the Invention
[0011] The purpose of this invention is to address the technical problem that membrane fouling and permeability cannot be simultaneously improved in distillation membranes used for high-salt wastewater treatment in the prior art, and to provide a defect covalent organic framework layer-mediated polyamide composite membrane and its preparation method. The composite membrane has a multi-layer structure, with a bottom layer of hydrophobic polyvinylidene fluoride microporous membrane, an intermediate layer of pore defect covalent organic framework, and a surface layer of dense polyamide sieved surface layer.
[0012] Another object of the present invention is to provide the application of the composite membrane in the treatment of high-salinity wastewater.
[0013] The technical solution adopted to achieve the purpose of this invention is: A defective covalent organic framework layer-mediated polyamide composite membrane includes a PVDF hydrophobic microporous membrane and a modification layer located on one side of the PVDF hydrophobic microporous membrane. The modification layer includes a pore defective covalent organic framework intermediate layer and a dense polyamide sieve surface layer, wherein the pore defective covalent organic framework intermediate layer is located on the surface of the PVDF base membrane, and the dense polyamide sieve surface layer is located on the surface of the pore defective covalent organic framework intermediate layer. The preparation method includes the following steps: Step 1: Pre-wet the PVDF hydrophobic microporous membrane with an ethanol aqueous solution, wash it with deionized water, and then store it in deionized water to obtain a hydrophilic wetted membrane. Then, sequentially add a mixed solution obtained by mixing p-phenylenediamine aqueous solution and acetic acid, and a hexane solution containing 1,3,5-trialdehyde resorcinol. The p-phenylenediamine and 1,3,5-trialdehyde resorcinol undergo interfacial polymerization on the surface of the hydrophilic wetted membrane to obtain a defect covalent organic framework membrane composed of a PVDF hydrophobic microporous membrane and a pore defect covalent organic framework intermediate layer located on one side of it. The concentration of the p-phenylenediamine aqueous solution is 0.05-0.1 wt%; the mass of the acetic acid is 7-9 times the mass of the p-phenylenediamine; the concentration of the hexane solution containing 1,3,5-trialdehyde resorcinol is 0.0025-0.005 wt%; and the interfacial polymerization time is 100-300 s. Step 2: Piperazine and pyromellitic trimethylolpropionate chloride are interfacially polymerized and thermally crosslinked on the coating side of the defective covalent organic framework membrane obtained in Step 1 to form a dense polyamide sieve surface layer, thus obtaining a composite membrane.
[0014] In the above technical solution, the thickness of the composite membrane is 120-135 μm, wherein the thickness of the PVDF hydrophobic microporous membrane is 118-130 μm, the thickness of the pore defect covalent organic framework intermediate layer is 150-200 nm, and the thickness of the dense polyamide sieved surface layer is 90-120 nm; preferably, the liquid inlet pressure LEPw of the composite membrane is >10 bar, and the water contact angle of the composite membrane is 50-60°.
[0015] In the above technical solution, the pore size of the PVDF hydrophobic microporous membrane is 0.35-0.45 μm, the pore size of the defect covalent organic framework layer is 0.02-0.10 μm, and the pore size of the dense polyamide layer is 0.50-0.70 nm.
[0016] In the above technical solution, the specific steps of the interfacial polymerization reaction in step 1 are as follows: A hydrophilic wetting membrane was fixed in a frame mold, and a mixed solution of p-phenylenediamine aqueous solution and acetic acid, as well as a hexane solution containing 1,3,5-trialdehyde phloroglucinol, were added sequentially to carry out the reaction. After the reaction was completed, the membrane was placed in an oven for interfacial polymerization and thermal crosslinking to obtain a covalent organic framework intermediate layer with pore defects.
[0017] In the above technical solution, step 2, the specific steps of interface aggregation are as follows: The defective covalent organic framework membrane obtained in step 1 is fixed in a framework mold with the intermediate layer of the pore defective covalent organic framework facing upward. Under preset ambient temperature and humidity conditions, piperazine aqueous solution and n-hexane solution containing trimesoyl chloride are added sequentially. After inducing interfacial polymerization on the surface of the intermediate layer of the pore defective covalent organic framework, thermal crosslinking is performed to form a dense polyamide sieve surface layer.
[0018] In the above technical solution, in step 1, the PVDF hydrophobic microporous membrane is immersed in an ethanol aqueous solution for pre-wetting treatment, the concentration of the ethanol aqueous solution is 40-80% v / v; the reaction temperature is 15-20℃, and the thermal crosslinking temperature is 60-90℃.
[0019] In the above technical solution, in step 2, the preset ambient temperature is 18-22℃, the preset ambient humidity is 50-60%, the concentration of piperazine aqueous solution is 1.5-3.0 wt%, the concentration of n-hexane solution containing trimesoyl chloride is 0.15-0.30 wt%, the interfacial polymerization time is 5-10 min, and the thermal crosslinking temperature is 70-90℃.
[0020] Another aspect of the present invention includes the application of the composite membrane as a distillation membrane in wastewater treatment.
[0021] In the above technical solution, the composite membrane is used as a distillation membrane in the desalination of high-salt wastewater.
[0022] Compared with the prior art, the beneficial effects of the present invention are: 1. The composite membrane prepared by this invention has a multilayer structure. The polyamide surface layer is a dense structure with sub-nanometer pores. It can avoid inorganic mineral scale from entering the membrane pores and causing membrane wetting initiation through size sieving, thereby significantly improving the membrane's anti-fouling performance. 2. The defective covalent organic framework intermediate layer of the composite membrane of the present invention not only promotes the formation of a dense polyamide selective layer by regulating monomer diffusion kinetics, but also creates a highly efficient vapor transport channel, significantly reducing mass transfer resistance, thereby ensuring the permeation performance of the modified membrane; 3. The composite membrane of the present invention can be applied to membrane distillation processes in the fields of complex high-salt wastewater treatment and seawater desalination, and can effectively improve the overall performance of the distillation membrane.
[0023] This composite membrane has excellent anti-fouling and anti-permeation properties, making it effective for a long time during membrane distillation. Attached Figure Description
[0024] Figure 1 This is a schematic diagram of the preparation process of the composite membrane of the present invention.
[0025] Figure 2 These are scanning electron microscope images of PVDF hydrophobic microporous membrane (#PVDF), covalent organic framework membrane (#PVDF-C), polyamide membrane (#PVDF-P), and the composite membrane of this invention (#PVDF-CP).
[0026] Figure 3 These are the water contact angle and liquid ingress pressure (LEPw) on the surfaces of #PVDF, #PVDF-C, #PVDF-P, and #PVDF-CP membranes.
[0027] Figure 4 This is a DCMD anti-supersaturated gypsum scaling performance test.
[0028] Figure 5 This is a test of the long-term performance of DCMD complex mixed salts and the anti-scaling / anti-fouling / anti-wetting properties of organic matter. Detailed Implementation
[0029] The present invention will be further described in detail below with reference to specific embodiments.
[0030] It should be understood that the specific embodiments described herein are for illustrative purposes only and are not intended to limit the scope of the invention.
[0031] The PVDF hydrophobic microporous membranes used in the following examples or comparative examples were purchased from Merck Milipore (IPVH00010).
[0032] Example 1 A defective covalent organic framework layer-mediated polyamide composite film is prepared by the following method: Step 1: Immerse the PVDF hydrophobic microporous membrane (#PVDF) in a 50% v / v ethanol aqueous solution to change the wettability of the membrane. Then, wash it with deionized water to remove excess ethanol and obtain a hydrophilic wettable membrane. Store it in deionized water for later use. Next, the hydrophilic wetting membrane was fixed in the frame mold. First, a 0.05% p-phenylenediamine aqueous solution and 200 μL acetic acid were poured in as catalysts. After maintaining for 100 s, the excess solution was removed. Then, a 0.0025% 1,3,5-trialdehyde phloroglucinol hexane solution was poured in and maintained for 100 s. The membrane was then placed in an 80℃ oven and dried for 5 min to obtain a defect covalent organic framework membrane composed of a PVDF hydrophobic microporous membrane and a defect covalent organic framework layer located on one side of it, denoted as #PVDF-C.
[0033] Step 2: Fix the defect covalent organic framework intermediate layer of #PVDF-C prepared in Step 1 onto the framework mold with the defect covalent organic framework layer facing upward. Stabilize the ambient temperature and humidity at 15℃ and 65%, respectively. Pour in 2 wt% piperazine aqueous solution, keep for 10 min, remove excess solution, then pour in 0.2% trimesoyl chloride hexane solution, keep for 5 min, and dry in an 80 ℃ oven for 10 min to form a dense polyamide sieve surface layer. Finally, obtain the defect covalent organic framework layer-mediated polyamide composite film, denoted as #PVDF-CP.
[0034] The preparation process of PVDF-CP is as follows: Figure 1 As shown, the morphology of #PVDF-CP is as follows Figure 2 As shown in (D).
[0035] like Figure 2 As shown in (A), the original #PVDF exhibits a typical interconnected porous network structure, such as Figure 2 As shown in (B), defect #PVDF-C exhibits a significantly densified network framework, accompanied by numerous spherical crystalline nodules, such as... Figure 2 As shown in (C), the polyamide layer on #PVDF-P has more protrusions, the polyamide layer on the upper surface of #PVDF-CP is denser, and the polyamide layer completely covers the defective covalent organic framework intermediate layer.
[0036] Therefore, #PVDF-CP significantly enhances anti-fouling properties while ensuring good permeability, thus overcoming the trade-off between scale resistance and permeability.
[0037] Comparative Example 1 A composite membrane with a defective covalent organic framework layer is prepared by the following method: Step 1: Immerse the PVDF hydrophobic microporous membrane (#PVDF) in a 50% v / v ethanol aqueous solution to change the wettability of the membrane. Then rinse it with deionized water to remove excess ethanol and store it in deionized water for later use. Step 2: Fix the wetting film obtained in Step 1 in the frame mold. First, pour in a 0.05% p-phenylenediamine aqueous solution and 200 μL acetic acid as a catalyst. After keeping it for 100 s, remove the excess solution. Then, pour in a 0.0025% 1,3,5-trialdehyde phloroglucinol n-hexane solution and keep it for 100 s. Place it in an 80℃ oven to dry for 5 min to obtain the defect covalent organic framework membrane, denoted as #PVDF-C.
[0038] The defects are attributed to the control of monomer concentration and interfacial polymerization conditions.
[0039] If either the aqueous or oil-phase monomer at a low concentration is completely consumed, the reaction process will stop. At the same time, shortening the reaction time can also block the reaction process, thus creating defects.
[0040] The ideal, defect-free COF membrane for comparison is prepared according to the following steps: Step 1: Immerse the PVDF hydrophobic microporous membrane (#PVDF) in a 50% v / v ethanol aqueous solution to change the wettability of the membrane. Then rinse it with deionized water to remove excess ethanol and store it in deionized water for later use. Step 2: Fix the wetting film obtained in Step 1 in a frame mold. First, pour in a 0.15% p-phenylenediamine aqueous solution and 210 μL acetic acid as a catalyst. After keeping it for 600 s, remove the excess solution. Then, pour in a 0.008% 1,3,5-trialdehyde phloroglucinol hexane solution. Keep it for 4 days and dry it in an 80℃ oven for 10 min to obtain a defective covalent organic framework membrane with an ideal defect-free covalent organic material layer.
[0041] From the SEM image of the #PVDF-C surface, such as Figure 2 As shown in the middle (B) left, #PVDF-C exhibits a significantly denser network framework, accompanied by numerous spherical crystalline nodules.
[0042] This structural evolution originates from the Schiff base condensation reaction occurring at the interface, which forms a covalently cross-linked organic framework.
[0043] The dense and uniform pore structure in ideal covalent organic framework membranes ( Figure 2 Unlike the middle (B) right), the #PVDF-C membrane prepared by this artificially regulated interfacial polymerization process has a moderate degree of crystallinity and retains defect-engineered voids. It can be used as an intermediate layer to regulate the subsequent interfacial polymerization process of polyamide, and it can also be used as a vapor transport channel, thereby improving anti-fouling properties while avoiding a decrease in permeability.
[0044] Comparative Example 2 A composite film having a polyamide layer is prepared by the following method: Step 1: Immerse the PVDF hydrophobic microporous membrane (#PVDF) in a 50% v / v ethanol aqueous solution to change the wettability of the membrane. Then rinse it with deionized water to remove excess ethanol and store it in deionized water for later use. Step 2: Fix the wetted film obtained in Step 1 in a frame mold, stabilize the ambient temperature and humidity at 15℃ and 65%, pour in 2 wt% piperazine aqueous solution, keep for 10 min, remove excess solution, then pour in 0.2% trimesoyl chloride n-hexane solution, keep for 5 min, and dry in an 80 ℃ oven for 10 min to obtain a PVDF film with a polyamide layer, denoted as #PVDF-P.
[0045] From the SEM image of the #PVDF-P surface, such as Figure 2 As shown in (C), the nodular morphology characteristic of thin-film composite membranes can be observed.
[0046] The polyamide layer is continuous and completely covers the PVDF substrate, but its density is worse than that of #PVDF-CP. Because it is directly polymerized on the hydrophobic macroporous PVDF substrate, it cannot achieve effective size retention and anti-scaling.
[0047] Test Example 1 The surface wetting properties of #PVDF-CP obtained in Example 1, #PVDF-C of Comparative Example 1, #PVDF-P of Comparative Example 2, and #PVDF were tested.
[0048] like Figure 3 As shown in (A), the WCA of the original #PVDF membrane is 115.0±1.0°, while the WCA of #PVDF-C drops to 99.3±0.7°, and that of #PVDF-P drops to 12.3±1.1°.
[0049] In contrast, the WCA of #PVDF-CP is moderate, at 51.0 ± 1.3°.
[0050] In addition, such as Figure 3 As shown in (B), the LEPw values of #PVDF, #PVDF-C, #PVDF-P and #PVDF-CP are 2.8±0.2, 3.7±0.7, 5.3±0.6 and 13.7±0.9 bar, respectively.
[0051] like Figure 3 As shown in (C), the average pore size of #PVDF-P and #PVDF-CP is reduced to the sub-nanometer scale (<0.65 nm), which significantly improves the anti-wetting properties.
[0052] This indicates that the introduction of a defective covalent organic framework interlayer helps polyamides to polymerize more fully at the interface, reduces unreacted end groups, and promotes the formation of a dense, highly cross-linked, and smooth polyamide layer.
[0053] Test Example 2 Membrane distillation tests were performed on the #PVDF-CP obtained in Example 1, the #PVDF-C of Comparative Example 1, the #PVDF-P of Comparative Example 2, and the #PVDF.
[0054] Specifically, the feed solution consisted of 25 mM gypsum. Under these feed solution conditions, the feed side and the permeation side were stabilized at 60 ℃ and 20 ℃, respectively, for 10 hours of continuous testing.
[0055] The side with the modified layer faces the feed liquid, and the PVDF substrate faces the permeate.
[0056] Depend on Figure 4 The membrane distillation test results in (A) show that, compared with #PVDF, #PVDF-C and #PVDF-P, #PVDF-CP has excellent anti-fouling properties.
[0057] During a 10-hour DCMD operation, the #PVDF-CP membrane exhibited stable permeate flux and salt rejection rate. With supersaturated brine as feed, the average permeate flux of the #PVDF-CP membrane was 36.70 kg·m³. -2 ·h -1 The conductivity of the produced water remained stable at approximately 2.99 μS·cm. -1 This indicates that no membrane scaling or wetting has occurred, and the produced water is pure.
[0058] The permeation fluxes of #PVDF, #PVDF-C, and #PVDF-P eventually decreased to 11.96, 16.71, and 26.53 kg·m³, respectively. -2 ·h -1 .
[0059] like Figure 4 Images (B), (C), (D), and (E) show the scanning electron microscopy (SEM) cross-sectional morphologies of PVDF, #PVDF-C, #PVDF-P, and #PVDF-CP, respectively. These images indicate that after 10 hours of testing with a 25 mM gypsum solution, the different film cross-sections exhibit significantly differentiated gypsum crystal distribution characteristics. For example, [the images show...] Figure 4 As shown in Figure (E), #PVDF-CP exhibits the best anti-fouling performance: only a small amount of sparse crystals are attached to the upper surface, and there are no signs of crystallization in the middle and lower surfaces of the membrane. This indicates that the #PVDF-CP membrane effectively inhibits the vertical migration and lateral diffusion of crystals, and has excellent anti-fouling performance. It can be applied to membrane distillation technology for the treatment of high-salt wastewater in actual production.
[0060] Test Example 3 like Figure 5 As shown in (A), long-term performance testing was conducted on the #PVDF-CP obtained in Example 1 in a direct contact membrane distillation (DCMD) configuration, as follows: Figure 5 As shown in (B), a typical mixed feed was used, consisting of 3.5 wt% NaCl, 5.0 mM gypsum, 1.0 mM NaHCO3 and 1.5 mM Na2SiO3·5H2O, to simulate a chemically complex brine environment.
[0061] The PVDF-CP membrane maintained a stable permeation flux (35.24 kg·m³) during 120 hours of continuous operation. -2 ·h -1 With a salt rejection rate of nearly 100%, it exhibits excellent desalination stability.
[0062] To further evaluate the antifouling and antiwetting properties of #PVDF-CP, the #PVDF-CP membrane was tested by gradually adding various contaminants to a 3.5 wt% NaCl solution, including 10 mg·L⁻¹. -1 HA, 0.05 mM SDS and 6.7% v / v ethanol.
[0063] like Figure 5 As shown in (C), the addition of these contaminants did not lead to a significant deterioration in the performance of the #PVDF-CP membrane, and no decrease in flux or increase in conductivity was observed.
[0064] Compared to Figure 5 The composite membrane previously reported in (D) demonstrates its suitability for complex high-salinity wastewater scenarios involving multiple pollutant categories.
[0065] The above description is only a preferred embodiment of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A defect-covalent organic framework layer-mediated polyamide composite film, characterized in that, The invention includes a PVDF hydrophobic microporous membrane and a modification layer located on one side of the PVDF hydrophobic microporous membrane. The modification layer includes a pore defect covalent organic framework intermediate layer and a dense polyamide sieve surface layer, wherein the pore defect covalent organic framework intermediate layer is located on the surface of the PVDF base membrane, and the dense polyamide sieve surface layer is located on the surface of the pore defect covalent organic framework intermediate layer. The preparation method includes the following steps: Step 1: Pre-wet the PVDF hydrophobic microporous membrane with an ethanol aqueous solution, wash it with deionized water, and then store it in deionized water to obtain a hydrophilic wetted membrane. Then, sequentially add a mixed solution obtained by mixing p-phenylenediamine aqueous solution and acetic acid, and a hexane solution containing 1,3,5-trialdehyde resorcinol. The p-phenylenediamine and 1,3,5-trialdehyde resorcinol undergo interfacial polymerization on the surface of the hydrophilic wetted membrane to obtain a defect covalent organic framework membrane composed of a PVDF hydrophobic microporous membrane and a pore defect covalent organic framework intermediate layer located on one side of it. The concentration of the p-phenylenediamine aqueous solution is 0.05-0.1 wt%; the mass of the acetic acid is 7-9 times the mass of the p-phenylenediamine; the concentration of the hexane solution containing 1,3,5-trialdehyde resorcinol is 0.0025-0.005 wt%; and the interfacial polymerization time is 100-300 s. Step 2: Piperazine and pyromellitic trimethylolpropionate chloride are interfacially polymerized and thermally crosslinked on the coating side of the defective covalent organic framework membrane obtained in Step 1 to form a dense polyamide sieve surface layer, thus obtaining a composite membrane.
2. The defect covalent organic framework layer-mediated polyamide composite film as described in claim 1, characterized in that, The composite membrane has a thickness of 120-135 μm, wherein the PVDF hydrophobic microporous membrane has a thickness of 118-130 μm, the pore defect covalent organic framework intermediate layer has a thickness of 150-200 nm, and the dense polyamide sieved surface layer has a thickness of 90-120 nm.
3. The defect covalent organic framework layer-mediated polyamide composite film as described in claim 1, characterized in that, The liquid inlet pressure LEPw of the composite membrane is greater than 10 bar, and the water contact angle of the composite membrane is 50-60°.
4. The defect covalent organic framework layer-mediated polyamide composite film as described in claim 1, characterized in that, The PVDF hydrophobic microporous membrane has a pore size of 0.35-0.45 μm, the defect covalent organic framework layer has a pore size of 0.02-0.10 μm, and the dense polyamide layer has a pore size of 0.50-0.70 nm.
5. The defect covalent organic framework layer-mediated polyamide composite film as described in claim 1, characterized in that, In step 1, the specific steps of the interfacial polymerization reaction are as follows: A hydrophilic wetting membrane was fixed in a frame mold, and a mixed solution of p-phenylenediamine aqueous solution and acetic acid, as well as a hexane solution containing 1,3,5-trialdehyde phloroglucinol, were added sequentially to carry out the reaction. After the reaction was completed, the membrane was placed in an oven for interfacial polymerization and thermal crosslinking to obtain a covalent organic framework intermediate layer with pore defects.
6. The defect covalent organic framework layer-mediated polyamide composite film as described in claim 1, characterized in that, In step 2, the specific steps of interface aggregation are as follows: The defective covalent organic framework membrane obtained in step 1 is fixed in a framework mold with the intermediate layer of the pore defective covalent organic framework facing upward. Under preset ambient temperature and humidity conditions, piperazine aqueous solution and n-hexane solution containing trimesoyl chloride are added sequentially. After inducing interfacial polymerization on the surface of the intermediate layer of the pore defective covalent organic framework, thermal crosslinking is performed to form a dense polyamide sieve surface layer.
7. The defect covalent organic framework layer-mediated polyamide composite film as described in claim 1, characterized in that, In step 1, the PVDF hydrophobic microporous membrane is pre-wetted by immersing it in an ethanol aqueous solution with a concentration of 40-80% v / v; the reaction temperature is 15-20℃ and the thermal crosslinking temperature is 60-90℃.
8. The defect covalent organic framework layer-mediated polyamide composite film as described in claim 1, characterized in that, In step 2, the preset ambient temperature is 18-22℃, the preset ambient humidity is 50-60%, the concentration of piperazine aqueous solution is 1.5-3.0 wt%, the concentration of n-hexane solution containing trimesoyl chloride is 0.15-0.30 wt%, the interfacial polymerization time is 5-10 min, and the thermal crosslinking temperature is 70-90℃.
9. The application of the defective covalent organic framework layer-mediated polyamide composite membrane as a distillation membrane in wastewater treatment, as described in any one of claims 1-8.
10. The application as described in claim 9, characterized in that, The wastewater treatment is a high-salinity wastewater desalination treatment.