Polyurethane microporous membranes, their preparation methods and bedding textiles
By preparing polyurethane microporous membranes with specific pore sizes, the problems of excessive moisture permeability and water permeability in fitted sheets were solved, achieving high air permeability and high water pressure resistance, thus improving the thermal and humid comfort and user experience of fitted sheets.
Patent Information
- Application Number
- CN202611321268.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
When existing polyurethane microporous membranes are used in fitted sheets, they have excessive moisture permeability and water permeability, which cannot effectively block liquid water penetration, resulting in a poor user experience. In addition, their air permeability is insufficient, failing to meet the thermal and moisture comfort requirements of fitted sheets.
Thermoplastic polyurethane is used as the film-forming matrix, combined with hydrophilic modifiers, hydrophobic modified nano-inorganic fillers and surfactants. Polyurethane microporous membranes are prepared by bidirectional synchronous stretching and heat setting to form water and air permeable channels with specific pore sizes. The bonding strength of the composite fabric is improved by surface corona treatment.
It achieves high air permeability, high water pressure resistance, and high moisture permeability, ensuring that the polyurethane microporous membrane effectively blocks liquid water penetration in the fitted sheet, while maintaining a soft feel and excellent elasticity, thus improving user comfort.
Smart Images

Figure SMS_3 
Figure SMS_4
Abstract
Description
Technical Field
[0001] This application relates to the field of textile technology, and in particular to a polyurethane microporous membrane, its preparation method, and bedding textiles. Background Technology
[0002] As living standards improve, people have higher requirements for the thermal and humidity comfort and protective performance of the sleep microenvironment. For example, in everyday home settings, fitted sheets, as textiles that cover mattresses, need to be able to block liquid stains and dust mites from penetrating, while also quickly wicking away sweat and water vapor emitted by the body during sleep.
[0003] To meet the above requirements, composite fabrics formed by combining polyurethane microporous membranes with fabric substrates are typically used as the fabric for fitted sheets. Polyurethane microporous membranes are polymer films with a micro-nano-scale pore network inside. The micropore size is between that of water droplets and water vapor molecules, and the waterproof and breathable functions are achieved by relying on the sieving effect of physical pore size and surface tension.
[0004] One related technology involves adding carbon nanotubes or graphene as reinforcing fillers to a film-forming matrix such as polyurethane, and combining it with a pore-forming agent, followed by coating, drying, and biaxial stretching to prepare microporous membranes. However, this approach is geared towards the outdoor clothing industry, and the microporous membranes exhibit excessively high moisture permeability and water permeability. If used directly in fitted sheets, they are highly susceptible to liquid water penetration under the continuous pressure of a person sleeping, resulting in a poor user experience. Furthermore, this approach, geared towards the outdoor clothing industry, suffers from poor air permeability of the microporous membranes. Summary of the Invention
[0005] This application provides a polyurethane microporous membrane, its preparation method, and bedding textiles to solve the above-mentioned technical problems.
[0006] To achieve the above objectives, the technical solution of this application is as follows: This application provides a method for preparing a polyurethane microporous membrane, comprising the following steps: S1. A casting solution is prepared by mixing thermoplastic polyurethane, a hydrophilic modifier, a surfactant, a hydrophobic modified nano-inorganic filler, and an organic solvent; the thermoplastic polyurethane has a Shore A hardness of 80HA-90HA. S2. The casting solution is coated onto a support carrier and then immersed in a coagulation bath to perform phase transformation molding and obtain a shaped primary wet film. S3. Peel the nascent wet film from the support carrier, and then stretch the nascent wet film in both directions synchronously at a temperature of 40℃-60℃ and a stretching speed of 50% / min-100% / min. The longitudinal stretching ratio is 1.2 times-1.5 times and the transverse stretching ratio is 1.5 times-2.0 times. Then, perform heat setting to obtain the polyurethane microporous membrane.
[0007] In one embodiment of this application, step S1 satisfies at least one of the following requirements (1)-(3): (1) The hydrophilic modifier has a molecular weight of 10,000-50,000, preferably 15,000-50,000; (2) The mass ratio of the hydrophilic modifier to the thermoplastic polyurethane is 15-25:100, preferably 18-23:100; (3) The hydrophilic modifier includes polyvinylpyrrolidone and / or polyethylene glycol.
[0008] In one embodiment of this application, in step S1, the mass ratio of the surfactant to the thermoplastic polyurethane is 0.5-2:100, preferably 0.8-2:100.
[0009] In one embodiment of this application, in step S1, the surfactant includes a nonionic fluorinated surfactant.
[0010] In one embodiment of this application, step S1 satisfies at least one of the following requirements (4)-(6): (4) The mass ratio of the hydrophobic modified nano-inorganic filler to the thermoplastic polyurethane is 5-10:100, preferably 6-10:100; (5) The hydrophobically modified nano-inorganic filler includes hydrophobically modified nano-silica and / or hydrophobically modified nano-titanium dioxide; (6) The particle size of the hydrophobic modified nano-inorganic filler is 20nm-50nm, preferably 25nm-50nm.
[0011] In one embodiment of this application, in step S1, the organic solvent includes N,N-dimethylformamide and / or N,N-dimethylacetamide.
[0012] In one embodiment of this application, in step S1, the mass ratio of the organic solvent to the thermoplastic polyurethane is 300-500:100, preferably 350-450:100.
[0013] In one embodiment of this application, in step S2, the thickness of the liquid film is 150μm-250μm, preferably 160μm-250μm.
[0014] In one embodiment of this application, in step S2, the temperature of the coagulation bath is 25°C-40°C, preferably 25°C-35°C.
[0015] In one embodiment of this application, in step S2, the coagulation bath liquid includes a water-ethanol mixture.
[0016] In one embodiment of this application, in step S2, the coagulation bath time is 3 min-8 min, preferably 4 min-8 min.
[0017] In one embodiment of this application, in step S3, the heat setting temperature is 80℃-100℃, preferably 85℃-95℃; the time is 2min-5min, preferably 3min-5min.
[0018] In one embodiment of this application, after heat setting in step S3, the following step is further included: performing surface corona treatment on the heat-set polyurethane microporous membrane.
[0019] This application also provides a polyurethane microporous membrane prepared according to the method described above, wherein the polyurethane microporous membrane has an average pore size of 0.1 μm-0.5 μm, a porosity of 60%-75%, and a thickness of 30 μm-50 μm.
[0020] This application also provides a bedding textile product, which includes a fabric base and a polyurethane microporous membrane as described above, laminated together with the fabric base.
[0021] The technical solution provided in this application has at least the following beneficial effects: In this application, thermoplastic polyurethane is used as the film-forming matrix, a hydrophilic modifier as a hydrophilic additive, and a hydrophobic modified nano-inorganic filler as a nucleating agent and mechanical reinforcing agent. Surfactants are used to reduce the interfacial interaction between the thermoplastic polyurethane and the hydrophobic modified nano-inorganic filler, thus reducing the probability of microscopic pinhole defects during film formation. During phase transformation, the highly hydrophilic modifier dissolves and precipitates in the coagulation bath, leaving numerous nearly circular, interconnected micropores in the polyurethane matrix framework, forming water- and air-permeable channels (i.e., the hydrophilic modifier also acts as a pore-forming agent). Simultaneously, the hydrophobic modified nano-inorganic filler acts as a physical crosslinking point, enhancing the membrane's skeletal strength, preventing excessive decrease in water pressure resistance under high porosity, and assisting in the formation of a more uniform microporous structure. The subsequent bidirectional synchronous stretching process elongates the micropores, transforming them from nearly circular to elliptical shapes, thereby significantly increasing the throughput of gas and water vapor without significantly enlarging the pore size (maintaining water pressure resistance). The principle behind this application's ability to balance high air permeability, high water pressure resistance, and high moisture permeability is as follows: By limiting the Shore A hardness of thermoplastic polyurethane to Within the -90HA range, a moderately hard polyurethane matrix framework ensures molecular chain rigidity to provide a high water pressure resistant framework while maintaining the soft feel and tensile elasticity required for sleep contact. During subsequent biaxial stretching, the stretching temperature is limited to 40℃-60℃, the stretching speed to 50% / min-100% / min, the longitudinal stretching multiple to 1.2-1.5 times, and the transverse stretching multiple to 1.5-2.0 times. This allows the microporous membrane to form water- and air-permeable channels of specific pore sizes, thereby utilizing molecular-scale "hydrophilic channels" to transfer water vapor while maintaining macroscopically dense membrane layers to block liquid water, thus improving the water pressure resistance of the microporous membrane.
[0022] In this application, by limiting the particle size of the hydrophobic modified nano-inorganic filler to the range of 20nm-50nm, the pores formed between the hydrophobic modified nano-inorganic fillers can form water-permeable and air-permeable channels with specific pore sizes, effectively ensuring the moisture permeability and air permeability of the microporous membrane.
[0023] In this application, by adding ethanol to the coagulation bath, the phase separation rate during the phase transformation process can be slowed down, the formation of macroporous defects can be suppressed, and the formation of a sponge-like porous structure can be facilitated, thereby improving the air permeability, moisture permeability and water pressure resistance of the microporous membrane.
[0024] In this application, surface corona treatment can introduce polar functional groups such as carboxyl and hydroxyl groups onto the surface of the microporous membrane, thereby improving the bonding strength between the microporous membrane and the fabric to be laminated, ensuring the overall durability of the composite fabric, and avoiding delamination failure. Detailed Implementation
[0025] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the embodiments of this application. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.
[0026] One embodiment of this application provides a method for preparing a polyurethane microporous membrane, comprising the following steps: S1. A casting solution is prepared by mixing thermoplastic polyurethane, hydrophilic modifier, surfactant, hydrophobic modified nano-inorganic filler and organic solvent; the Shore A hardness of thermoplastic polyurethane is 80HA-90HA; S2. The casting solution is coated onto the support carrier and then immersed in the coagulation bath to carry out phase transformation and molding, thereby obtaining the shaped primary wet film. S3. Peel the nascent wet film from the support carrier, and then stretch the nascent wet film in both directions synchronously at a temperature of 40℃-60℃ and a stretching speed of 50% / min-100% / min. The longitudinal stretching ratio is 1.2 times-1.5 times and the transverse stretching ratio is 1.5 times-2.0 times. Heat set the film to obtain a polyurethane microporous membrane.
[0027] In this application, thermoplastic polyurethane is used as the film-forming matrix, a hydrophilic modifier as a hydrophilic additive, and a hydrophobic modified nano-inorganic filler as a nucleating agent and mechanical reinforcing agent. Surfactants are used to reduce the interfacial interaction between the thermoplastic polyurethane and the hydrophobic modified nano-inorganic filler, thus reducing the probability of microscopic pinhole defects during film formation. During phase transformation, the highly hydrophilic modifier dissolves and precipitates in the coagulation bath, leaving numerous nearly circular, interconnected micropores in the polyurethane matrix framework, forming water- and air-permeable channels (i.e., the hydrophilic modifier also acts as a pore-forming agent). Simultaneously, the hydrophobic modified nano-inorganic filler acts as a physical crosslinking point, enhancing the membrane's skeletal strength, preventing excessive decrease in water pressure resistance under high porosity, and assisting in the formation of a more uniform microporous structure. The subsequent bidirectional synchronous stretching process elongates the micropores, transforming them from nearly circular to elliptical shapes, thereby significantly increasing the throughput of gas and water vapor without significantly enlarging the pore size (maintaining water pressure resistance). The principle behind this application's ability to balance high air permeability, high water pressure resistance, and high moisture permeability is as follows: By limiting the Shore A hardness of thermoplastic polyurethane to Within the -90HA range, a moderately hard polyurethane matrix framework ensures molecular chain rigidity to provide a framework that can withstand high water pressure, while also maintaining the soft feel and tensile elasticity required for sleep contact. During subsequent biaxial stretching, the stretching temperature is limited to 40℃-60℃, the stretching speed to 50% / min-100% / min, the longitudinal stretching multiple to 1.2-1.5 times, and the transverse stretching multiple to 1.5-2.0 times. This allows the microporous membrane to form water- and air-permeable channels of specific pore sizes, thereby utilizing molecular-scale "hydrophilic channels" to transfer water vapor while maintaining macroscopically dense membrane layers to block liquid water.
[0028] In one embodiment of this application, in step S1, the thermoplastic polyurethane can be a polyether-type polyurethane. The hydrophilic modifier has a molecular weight of 10,000-50,000, preferably 15,000-50,000. The mass ratio of the hydrophilic modifier to the thermoplastic polyurethane is 15-25:100, preferably 18-23:100. The hydrophilic modifier includes polyvinylpyrrolidone and / or polyethylene glycol. The mass ratio of the surfactant to the thermoplastic polyurethane is 0.5-2:100, preferably 0.8-2:100. The surfactant includes nonionic fluorinated surfactants. The mass ratio of the hydrophobic modified nano-inorganic filler to the thermoplastic polyurethane is 5-10:100, preferably 6-10:100. The hydrophobic modified nano-inorganic filler includes hydrophobic modified nano-silica and / or hydrophobic modified nano-titanium dioxide. The hydrophobically modified nano-inorganic filler has a particle size of 20nm-50nm, preferably 25nm-50nm. The organic solvent includes N,N-dimethylformamide and / or N,N-dimethylacetamide. The mass ratio of the organic solvent to the thermoplastic polyurethane is 300-500:100, preferably 350-450:100. The preparation of the casting solution includes the following steps: mixing thermoplastic polyurethane, hydrophilic modifier, surfactant, hydrophobically modified nano-inorganic filler, and organic solvent; stirring; allowing to stand for degassing; and stirring at 60℃-80℃ for 4-8 hours.
[0029] In this application, by limiting the particle size of the hydrophobic modified nano-inorganic filler to the range of 20nm-50nm, the pores formed between the hydrophobic modified nano-inorganic fillers can form water-permeable and air-permeable channels with specific pore sizes, effectively ensuring the moisture permeability and air permeability of the microporous membrane.
[0030] In one embodiment of this application, in step S2, the support carrier can be release paper or non-woven fabric, etc. Exemplarily, a slit-type coating head can be used to coat the casting liquid onto the support carrier. The thickness of the liquid film is 150μm-250μm, preferably 160μm-250μm. The temperature of the coagulation bath is 25℃-40℃, preferably 25℃-35℃. The coagulation bath includes a water-ethanol mixture. The mass percentage of ethanol in the water-ethanol mixture is 10%-30%, preferably 15%-30%. The coagulation bath time (i.e., the immersion time in the coagulation bath) is specified. The time is 3-8 minutes, preferably 4-8 minutes.
[0031] The phase transformation stage determines the initial pore structure and dense skin thickness of the microporous membrane. In this application, by adding ethanol to the coagulation bath, the phase separation rate during the phase transformation process can be slowed down, the formation of macropore defects can be suppressed, and the formation of a sponge-like porous structure can be facilitated, thereby improving the air permeability, moisture permeability and water pressure resistance of the microporous membrane.
[0032] In one embodiment of this application, in step S3, the nascent wet film is washed and then subjected to bidirectional synchronous stretching. Exemplarily, deionized water can be used for washing. The heat setting temperature is 80℃-100℃, preferably 85℃-95℃; the time is 2min-5min, preferably 3min-5min.
[0033] In one embodiment of this application, after heat setting in step S3, the method further includes the following step: subjecting the heat-set polyurethane microporous membrane to surface corona treatment. The power of the surface corona treatment is 1kW-3kW, preferably 1.2kW-3kW; the speed is 10m / min-20m / min, preferably 12m / min-20m / min.
[0034] In this application, surface corona treatment can introduce polar functional groups such as carboxyl and hydroxyl groups onto the surface of the microporous membrane, thereby improving the bonding strength between the microporous membrane and the fabric to be laminated, ensuring the overall durability of the composite fabric, and avoiding delamination failure.
[0035] Another embodiment of this application provides a polyurethane microporous membrane prepared according to the method described above, wherein the polyurethane microporous membrane has an average pore size of 0.1 μm-0.5 μm, a porosity of 60%-75%, and a thickness of 30 μm-50 μm.
[0036] Another embodiment of this application provides a bedding textile product comprising a fabric base and a polyurethane microporous membrane as described above, laminated together with the fabric base. This polyurethane microporous membrane has a soft feel and excellent elasticity. When laminated onto a fabric base such as knitted fabric, it effectively prevents mites and liquid penetration while ensuring timely wicking away of perspiration, significantly improving the comfort of the microenvironment. The bedding textile product can be a fitted sheet, bed sheet, or similar item. The fabric base can be knitted fabric, non-woven fabric, etc. Furthermore, the aforementioned polyurethane microporous membrane can also be used in fields such as baby products, hotel linens, and medical protective equipment.
[0037] Furthermore, the term "and / or" in this application is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. Additionally, the technical solutions of the various embodiments can be combined with each other, but this must be based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or impossible to implement, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection claimed in this application.
[0038] Example 1 S1. Mix 100 kg of polyether polyurethane M-1609 (Shore A hardness of 85HA, Shore A hardness was measured using a Shore A hardness tester), 20 kg of polyvinylpyrrolidone (weight molecular weight of 30000), 1 kg of nonionic fluorinated surfactant TF-11056, 8 kg of hydrophobic modified nano silica VK-SP30G (particle size of 30 nm) and 400 kg of N,N-dimethylacetamide, stir at 70℃ for 6 h, and allow to stand to remove bubbles to obtain the casting solution; S2. The casting solution is coated onto the nonwoven fabric using a slit coating head to form a liquid film with a thickness of 200 μm; The nonwoven fabric with the liquid film formed is immersed in a coagulation bath at 30°C for 5 minutes. The coagulation bath is a mixture of deionized water and ethanol with a mass percentage of 20% ethanol, in order to carry out phase inversion molding and obtain the formed primary wet film. S3. Remove the nascent wet film from the coagulation bath and wash it thoroughly with deionized water to remove residual solvent; The nascent wet film was peeled off from the nonwoven fabric. Then, the nascent wet film was subjected to bidirectional synchronous stretching at a temperature of 50℃ and a stretching speed of 80% / min. The longitudinal stretching ratio was 1.3 times and the transverse stretching ratio was 1.8 times. After stretching, heat set at 90℃ for 3 minutes; After heat setting, the polyurethane microporous membrane was subjected to surface corona treatment at a power of 2kW and a speed of 15m / min to obtain the polyurethane microporous membrane.
[0039] Comparative Example 1 The difference between this comparative example and Example 1 is that the temperature during the bidirectional synchronous stretching process is 35°C.
[0040] Comparative Example 2 The difference between this comparative example and Example 1 is that the temperature during the bidirectional synchronous stretching process is 65°C.
[0041] Comparative Example 3 The difference between this comparative example and Example 1 is that the stretching speed during the bidirectional synchronous stretching process is 45% / min.
[0042] Comparative Example 4 The difference between this comparative example and Example 1 is that the stretching speed during the bidirectional synchronous stretching process is 110% / min.
[0043] Comparative Example 5 The difference between this comparative example and Example 1 is that the longitudinal stretching factor is 1.1 times.
[0044] Comparative Example 6 The difference between this comparative example and Example 1 is that the longitudinal stretching factor is 1.6 times.
[0045] Comparative Example 7 The difference between this comparative example and Example 1 is that the lateral stretching factor is 1.4 times.
[0046] Comparative Example 8 The difference between this comparative example and Example 1 is that the lateral stretching factor is 2.1 times.
[0047] Comparative Example 9 The difference between this comparative example and Example 1 is that the coagulation bath is deionized water.
[0048] That is, no ethanol was added to the coagulation bath in this comparative example.
[0049] Comparative Example 10 The difference between this comparative example and Example 1 is that polyvinylpyrrolidone was not added to the casting solution.
[0050] Comparative Example 11 The difference between this comparative example and Example 1 is that bidirectional synchronous stretching was not performed.
[0051] test The polyurethane microporous membranes obtained in Example 1 and Comparative Examples 10-11 were peeled off from the nonwoven fabric. The thickness of the peeled polyurethane microporous membrane was tested using a mechanical contact thickness gauge, and the results are shown in Table 1. The porosity of the exfoliated polyurethane microporous membrane was tested according to GB / T 33052-2016 "Method for Determination of Porosity of Microporous Functional Thin Films - Cetane Absorption Method", and the results are shown in Table 1. The average pore size of the peeled polyurethane microporous membrane was tested according to GB / T 32361-2015 "Test Method for Pore Size of Separation Membranes - Bubble Point and Average Flow Rate Method", and the results are shown in Table 1. The moisture permeability of the peeled polyurethane microporous membrane was tested according to Method A in GB / T 12704.1-2009 Textiles - Test methods for moisture permeability of fabrics - Part 1: Moisture absorption method. The results are shown in Table 2. The air permeability of the peeled polyurethane microporous membrane was tested according to GB / T 5453-2025 Textiles - Determination of air permeability of fabrics, and the results are shown in Table 2. The polyurethane microporous membrane was peeled off and bonded to cotton fiber fabric using PUR hot melt adhesive. The hydrostatic pressure of the composite fabric was tested according to GB / T4744-2013 Textiles Water Repellency Test - Static Water Pressure Method. The results are shown in Table 2. After washing the composite fabric 20 times, the hydrostatic pressure was tested again using the method described above, and the results are shown in Table 2.
[0052] Table 1. Test results of thickness, average pore size, and porosity
[0053] Table 2 Results of moisture permeability, air permeability and hydrostatic pressure tests
[0054] As shown in Tables 1 and 2, compared with Comparative Examples 1-8, the air permeability and post-wash hydrostatic pressure of Example 1 are significantly improved, and the moisture permeability of Example 1 is greater than 4000 g / m²·24h. This result indicates that by limiting the stretching temperature to the range of 40℃-60℃, the stretching speed to the range of 50% / min-100% / min, the longitudinal stretching multiple to the range of 1.2-1.5 times, and the transverse stretching multiple to the range of 1.5-2.0 times, this application can effectively balance high moisture permeability, high air permeability, and water pressure resistance.
[0055] As shown in Tables 1 and 2, compared with Comparative Example 9, the moisture permeability, air permeability, and post-wash water pressure resistance of Example 1 were significantly improved. This result indicates that, in this application, adding ethanol to the coagulation bath can improve the air permeability, moisture permeability, and water pressure resistance of the microporous membrane.
[0056] As shown in Tables 1 and 2, compared with Comparative Example 10, the moisture permeability and air permeability of Example 1 were significantly improved. This result indicates that, in this application, adding a hydrophilic modifier to the coagulation bath can improve the air permeability and moisture permeability of the microporous membrane.
[0057] As shown in Tables 1 and 2, compared with Comparative Example 11, the moisture permeability and air permeability of Example 1 are significantly improved. This result indicates that, in this application, bidirectional synchronous stretching can improve the air permeability and moisture permeability of the microporous membrane.
[0058] The above embodiments are merely illustrative of the principles and effects of this application and are not intended to limit this application. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of this application. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in this application should still be covered by the claims of this application.
Claims
1. A method for preparing a polyurethane microporous membrane, characterized in that, Includes the following steps: S1. A casting solution is prepared by mixing thermoplastic polyurethane, a hydrophilic modifier, a surfactant, a hydrophobic modified nano-inorganic filler, and an organic solvent; the thermoplastic polyurethane has a Shore A hardness of 80HA-90HA. S2. The casting solution is coated onto a support to form a liquid film, which is then immersed in a coagulation bath for phase transformation to obtain a formed nascent wet film. S3. Peel the nascent wet film from the support carrier, and then stretch the nascent wet film in both directions synchronously at a temperature of 40℃-60℃ and a stretching speed of 50% / min-100% / min. The longitudinal stretching ratio is 1.2 times-1.5 times and the transverse stretching ratio is 1.5 times-2.0 times. Then, perform heat setting to obtain the polyurethane microporous membrane.
2. The method for preparing the polyurethane microporous membrane as described in claim 1, characterized in that, Step S1 satisfies at least one of the following requirements (1)-(3): (1) The hydrophilic modifier has a molecular weight of 10,000-50,000; (2) The mass ratio of the hydrophilic modifier to the thermoplastic polyurethane is 15-25:100; (3) The hydrophilic modifier includes polyvinylpyrrolidone and / or polyethylene glycol.
3. The method for preparing the polyurethane microporous membrane as described in claim 1, characterized in that, In step S1, the mass ratio of the surfactant to the thermoplastic polyurethane is 0.5-2:100; And / or, in step S1, the surfactant includes a nonionic fluorinated surfactant.
4. The method for preparing the polyurethane microporous membrane as described in claim 1 or 3, characterized in that, Step S1 satisfies at least one of the following requirements (4)-(6): (4) The mass ratio of the hydrophobic modified nano-inorganic filler to the thermoplastic polyurethane is 5-10:100; (5) The hydrophobically modified nano-inorganic filler includes hydrophobically modified nano-silica and / or hydrophobically modified nano-titanium dioxide; (6) The particle size of the hydrophobic modified nano-inorganic filler is 20nm-50nm.
5. The method for preparing the polyurethane microporous membrane as described in claim 1, characterized in that, In step S1, the organic solvent includes N,N-dimethylformamide and / or N,N-dimethylacetamide; And / or, in step S1, the mass ratio of the organic solvent to the thermoplastic polyurethane is 300-500:
100.
6. The method for preparing the polyurethane microporous membrane as described in claim 1 or 5, characterized in that, In step S2, the thickness of the liquid film is 150μm-250μm; And / or, in step S2, the temperature of the coagulation bath is 25℃-40℃.
7. The method for preparing the polyurethane microporous membrane as described in claim 6, characterized in that, In step S2, the coagulation bath solution includes a water-ethanol mixture. And / or, in step S2, the coagulation bath time is 3 min-8 min.
8. The method for preparing the polyurethane microporous membrane as described in claim 1, characterized in that, In step S3, the heat setting temperature is 80℃-100℃, and the time is 2min-5min; And / or, in step S3, after the heat setting, the following step is also included: performing surface corona treatment on the heat-set polyurethane microporous membrane.
9. A polyurethane microporous membrane prepared according to any one of claims 1-8, characterized in that, The polyurethane microporous membrane has an average pore size of 0.1μm-0.5μm, a porosity of 60%-75%, and a thickness of 30μm-50μm.
10. A type of bedding textile, characterized in that, The bedding textiles include a fabric base and a polyurethane microporous membrane as described in claim 9, which is laminated together with the fabric base.