A hydroxyl-containing polyimide gas separation membrane, its preparation method and application

By introducing hydroxyl structures into the polyimide gas separation membrane to form hydrogen bonds and improve thermal stability, the problem of insufficient thermal stability of existing polyimide gas separation membranes at high temperatures is solved, and a gas separation effect with high selectivity and permeability is achieved.

CN123102181APending Publication Date: 2026-11-17SHENYANG RES INST OF CHEM IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611528421.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polyimide gas separation membranes have insufficient thermal stability at high temperatures, leading to membrane structure relaxation and reduced gas selectivity, which limits their application in high-temperature gas separation scenarios.

Method used

A polyamic acid solution is formed by polymerizing hydroxyl diamine monomers and dianhydride monomers. After defoaming, drying and thermal imidization treatment, a hydroxyl-containing polyimide gas separation membrane is prepared. The thermal stability and selectivity of the membrane are improved by using hydrogen bonds formed between hydroxyl groups and amide bonds.

Benefits of technology

The prepared hydroxyl-containing polyimide gas separation membrane maintains good gas selectivity and permeability at high temperatures, making it suitable for gas separation under high-temperature conditions, especially H2/N2 and CO2/N2 separation, thus improving the membrane's service life and separation stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102181A_ABST
    Figure CN123102181A_ABST
Patent Text Reader

Abstract

This invention provides a hydroxyl-containing polyimide gas separation membrane, its preparation method, and its application, belonging to the field of polymer membrane separation technology. The hydroxyl-containing polyimide gas separation membrane of this invention is polymerized from a diamine monomer and a dianhydride monomer; the diamine monomer contains hydroxyl groups. The polyimide gas separation membrane provided by this invention possesses both high selectivity and heat resistance, making it more suitable for gas separation operations under high-temperature conditions. The polyimide film of this invention is prepared by polymerizing a hydroxyl-containing diamine and a dianhydride into polyamic acid, followed by thermal imidization, introducing hydroxyl groups into the polyimide molecular backbone; the introduced hydroxyl groups form numerous hydrogen bonds with the amide and imide bonds in the polyimide, greatly increasing selectivity and thermal stability without affecting the membrane permeability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer membrane separation technology, and in particular to a hydroxyl-containing polyimide gas separation membrane, its preparation method, and its application. Background Technology

[0002] Compared to traditional gas separation methods such as cryogenic distillation and pressure swing adsorption, membrane separation technology offers significant advantages, including low energy consumption, ease of operation, compact equipment, and environmental friendliness, leading to its increasing popularity in the gas separation field. Polyimide (PI), with its excellent thermal stability, chemical stability, mechanical properties, good film-forming ability, and structural designability, has become one of the most promising membrane materials for gas separation.

[0003] Among numerous gas separation applications, carbon dioxide / nitrogen (CO2 / N2) separation and hydrogen / nitrogen (H2 / N2) separation have significant industrial value and practical implications. CO2 / N2 separation primarily targets the capture and storage of CO2 in coal-fired flue gas, a key technology for addressing global climate change. H2 / N2 separation, on the other hand, is widely used in industrial processes such as hydrogen recovery from ammonia synthesis off-gas and hydrogen purification from refinery gas. Polyimide gas separation membranes, with their excellent gas selectivity and permeability, demonstrate broad application prospects in both of these separation systems. However, existing polyimide gas separation membrane products still face challenges such as insufficient thermal stability in practical industrial applications. Many industrial gas separation processes require operation at high temperatures; for example, coal-fired flue gas temperatures are typically high, and the exhaust temperature of ammonia synthesis off-gas can reach above 150°C. While molecular design can improve the selectivity of the separation membrane, it often reduces its thermal stability. For example, Ayala et al. obtained a polyimide gas separation membrane by polymerizing dianhydride containing large-volume side groups with 2,2-bis(4-aminophenyl)hexafluoropropane. T g Only 265℃ J. Membr. Sci. 2013, 434 (121-129). Lower performance under high-temperature conditions. T g The separation membrane is prone to intensified chain segment movement, leading to membrane structure relaxation and a significant decrease in gas selectivity; at the same time, its thermal decomposition temperature ( T d The membrane's temperature is not high enough, and long-term operation at high temperatures poses a risk of thermal degradation, which seriously affects the membrane's service life and separation stability, thus limiting its application in high-temperature gas separation scenarios.

[0004] Therefore, a hydroxyl-containing polyimide gas separation membrane is provided to improve separation efficiency and thermal stability, effectively overcoming the technical defects of insufficient thermal stability of existing polyimide gas separation membrane products in high-temperature applications, and has significant technological advancements and broad industrial application prospects. Summary of the Invention

[0005] The purpose of this invention is to provide a hydroxyl-containing polyimide gas separation membrane, its preparation method, and its application. The hydroxyl-containing polyimide gas separation membrane has good gas separation performance and high thermal stability.

[0006] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a hydroxyl-containing polyimide gas separation membrane, which is polymerized from a diamine monomer and a dianhydride monomer; wherein the diamine monomer contains hydroxyl groups. The diamine monomer is one or two of the following structural formulas: , , , , , , , , , , , , , , , ; The dianhydride monomer is one or two of the following structural formulas: , , , , , , , .

[0007] The present invention also provides a method for preparing the hydroxyl-containing polyimide gas separation membrane, comprising the following steps: 1) Mix diamine monomer, dianhydride monomer and organic solvent, and carry out polymerization reaction of the mixture to obtain polyamic acid solution; 2) The polyamic acid solution was sequentially defoamed and allowed to stand to obtain the treated polyamic acid solution; 3) The treated polyamic acid solution is scraped onto the substrate and dried to obtain a solid film. The solid film is then subjected to thermal imidization and hydrothermal peeling to obtain a hydroxyl-containing polyimide gas separation membrane.

[0008] Preferably, in step 1), the molar ratio of diamine in the diamine monomer to dianhydride in the dianhydride monomer is 0.9~1.1:0.9~1.1, and the organic solvent is one or more of N,N-dimethylacetamide, N-methylpyrrolidone, N,N-dimethylformamide, m-cresol and p-cresol; the solid content of the mixture is 10~40%.

[0009] Preferably, the polymerization reaction in step 1) is carried out at a temperature of -10 to 30°C for 7 to 18 hours.

[0010] Preferably, the vacuum degree of the defoaming treatment in step 2) is 0.09~0.1MPa, the defoaming treatment time is 30~90min, and the standing time is 12~24h.

[0011] Preferably, the drying temperature in step 3) is 55~65℃, the drying vacuum degree is 0.07~0.09MPa, and the drying time is 5~7h; the substrate is a glass plate or a stainless steel plate.

[0012] Preferably, the thermal imidization in step 3) is divided into four stages: the first stage of thermal imidization is performed at a temperature of 50~150℃, a heating rate of 5~10℃ / min, and a holding time of 30~80min; the second stage of thermal imidization is performed at a temperature of 150~250℃, a heating rate of 2~10℃ / min, and a holding time of 30~80min; the third stage of thermal imidization is performed at a temperature of 250~300℃, a heating rate of 1~5℃ / min, and a holding time of 30~80min; and the fourth stage of thermal imidization is performed at a temperature of 300~350℃, a heating rate of 1~5℃ / min, and a holding time of 30~80min.

[0013] The present invention also provides the application of the hydroxyl-containing polyimide gas separation membrane in gas enrichment, gas purification and gas separation, wherein the gas is hydrogen or carbon dioxide.

[0014] The beneficial effects of this invention are: The polyimide gas separation membrane provided by this invention possesses both high selectivity and heat resistance, making it more suitable for gas separation operations under high-temperature conditions. The polyimide film of this invention is prepared by polymerizing polyamic acid from hydroxyl-containing diamines and dianhydrides, followed by thermal imidization, introducing hydroxyl groups into the polyimide molecular backbone. The introduced hydroxyl groups form numerous hydrogen bonds with the amide and imide bonds in the polyimide, significantly increasing selectivity and thermal stability without affecting the membrane's permeability.

[0015] The polyimide film of the present invention, as a gas separation membrane, is not only resistant to high temperature, but also has high permeability and selectivity, with a selectivity coefficient of H2 / N2 as high as 190, and is expected to be used for efficient hydrogen enrichment and purification. Attached Figure Description

[0016] Figure 1 The infrared spectrum of the hydroxyl-containing polyimide gas separation membrane prepared in Example 1. Detailed Implementation

[0017] This invention provides a hydroxyl-containing polyimide gas separation membrane, which is polymerized from a diamine monomer and a dianhydride monomer; wherein the diamine monomer contains hydroxyl groups. The diamine monomer is one or two of the following structural formulas: , , , , , , , , , , , , , , , ; The dianhydride monomer is one or two of the following structural formulas: , , , , , , , .

[0018] The present invention also provides a method for preparing the hydroxyl-containing polyimide gas separation membrane, comprising the following steps: 1) Mix diamine monomer, dianhydride monomer and organic solvent, and carry out polymerization reaction of the mixture to obtain polyamic acid solution; 2) The polyamic acid solution was sequentially defoamed and allowed to stand to obtain the treated polyamic acid solution; 3) The treated polyamic acid solution is scraped onto the substrate and dried to obtain a solid film. The solid film is then subjected to thermal imidization and hydrothermal peeling to obtain a hydroxyl-containing polyimide gas separation membrane.

[0019] In this invention, the molar ratio of diamine in the diamine monomer to dianhydride in the dianhydride monomer in step 1) is preferably 0.9~1.1:0.9~1.1, more preferably 0.95~1.05:0.95~1.05, and even more preferably 1:1; the organic solvent is preferably one or more of N,N-dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), m-cresol, and p-cresol; the solid content of the mixture is preferably 10~40%, more preferably 15~35%, and even more preferably 20~30%.

[0020] In this invention, the temperature of the polymerization reaction in step 1) is preferably -10~30℃, more preferably 0~20℃, and even more preferably 5~10℃, and the time of the polymerization reaction is preferably 7~18h, more preferably 8~16h, and even more preferably 10~14h.

[0021] In this invention, the vacuum degree of the defoaming treatment in step 2) is preferably 0.09~0.1MPa, more preferably 0.092~0.097MPa, and even more preferably 0.095~0.096MPa. The defoaming treatment time is preferably 30~90min, more preferably 40~80min, and even more preferably 50~60min. The standing time is preferably 12~24h, more preferably 15~20h, and even more preferably 17~18h.

[0022] In this invention, the drying temperature in step 3) is preferably 55~65℃, more preferably 57~63℃, and even more preferably 60℃; the drying vacuum degree is preferably 0.07~0.09MPa, more preferably 0.075~0.085MPa, and even more preferably 0.08MPa; the drying time is preferably 5~7h, more preferably 5.5~6.5h, and even more preferably 6h; the substrate is preferably a glass plate or a stainless steel plate.

[0023] In this invention, the thickness of the treated polyamic acid solution coating is preferably 180~220μm, more preferably 190~210μm, and even more preferably 200μm.

[0024] In this invention, the temperature of thermal imidization in step 3) is preferably 50~350℃, and the thermal imidization is divided into four stages: the temperature of the first stage thermal imidization is preferably 50~150℃, more preferably 80~130℃, more preferably 100℃, the heating rate is preferably 5~10℃ / min, more preferably 6~9℃ / min, more preferably 7~8℃ / min, and the holding time is preferably 30~80min, more preferably 40~70min, more preferably 50~60min; the temperature of the second stage thermal imidization is preferably 150~250℃, more preferably 180~220℃, more preferably 200℃, the heating rate is preferably 2~10℃ / min, more preferably 4~8℃ / min, more preferably 5~6℃ / min, and the holding time is preferably 30~80min, more preferably 40~70min. The temperature of the third stage of thermal imidization is preferably 250-300℃, more preferably 260-290℃, more preferably 270-280℃, the heating rate is preferably 1-5℃ / min, more preferably 2-4℃ / min, more preferably 3℃ / min, and the holding time is preferably 30-80min, more preferably 40-70min, more preferably 50-60min; the temperature of the fourth stage of thermal imidization is preferably 300-350℃, more preferably 310-340℃, more preferably 320-330℃, the heating rate is preferably 1-5℃ / min, more preferably 2-4℃ / min, more preferably 3℃ / min, and the holding time is preferably 30-80min, more preferably 40-70min, more preferably 50-60min.

[0025] The present invention also provides the application of the hydroxyl-containing polyimide gas separation membrane in gas enrichment, gas purification and gas separation, wherein the gas is hydrogen or carbon dioxide.

[0026] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0027] Example 1

[0028] Under a nitrogen atmosphere, 10 mmol of N,N′-[(1-methylene)bis(6-hydroxy-3,1-phenyl)]bis[3-amino-]benzoyl (m-BAP) and 80 mL of DMAc were added to a 250 mL three-necked flask and stirred at 0 °C for 2 h until completely dissolved. Then, 10 mmol of 4,4'-(hexafluoroisopropene)phthalic anhydride (6FDA) was added to the solution, and the mixture was stirred at 0 °C at 400 rpm for 8 h to obtain a polyamic acid solution. The polyamic acid solution was defoamed under a vacuum of 0.08 MPa for 60 min and allowed to stand for 24 h. A film with a thickness of 200 μm was then scraped onto a clean glass plate using a doctor blade. The glass plate was then placed in a vacuum oven at 60 °C and dried at 0.08 MPa for 6 h to obtain a solid film.

[0029] The solid membrane was placed in a muffle furnace and heated to 120°C at a rate of 10°C / min, and held at 120°C for 60 min. Then, the temperature was increased to 250°C at a rate of 5°C / min and held at 250°C for 60 min. Next, the temperature was increased to 300°C at a rate of 5°C / min and held at 300°C for 60 min. Then, the temperature was increased to 350°C at a rate of 1°C / min and held at 350°C for 60 min. Finally, the membrane was naturally cooled and annealed to room temperature at a rate of 10°C / min. The membrane was then hydrothermally exfoliated in deionized water to obtain a hydroxyl-containing polyimide gas separation membrane.

[0030] The infrared spectrum of the hydroxyl-containing polyimide gas separation membrane prepared in Example 1 is shown below. Figure 1 As shown: Infrared spectroscopy was performed using a Fourier transform infrared spectroscopy (FTIR) instrument (Spectrum Two, Perkin-Elmer, USA). The functional groups of the polyimide separation membrane were characterized using FTIR, with a scanning range of 4000–400 cm⁻¹. -1 The number of scans was 64.

[0031] Example 2

[0032] Under a nitrogen atmosphere, 10 mmol of N,N'-[[2,2,2-trifluoro-1-(trifluoromethyl)ethylidene]bis(6-hydroxy-3,1-phenylene)]bis[3-aminobenzamide] (m-6FDAP) and 80 mL of DMAc were added to a 250 mL three-necked flask and stirred at 400 rpm for 2 h at 0 °C until completely dissolved. 10 mmol of 4,4'-(hexafluoroisopropene)phthalic anhydride (6FDA) was added to the above solution and stirred at 0 °C for 10 h to obtain a polyamic acid solution.

[0033] The process conditions for preparing the hydroxyl-containing polyimide gas separation membrane from the polyamic acid solution are the same as in Example 1.

[0034] Example 3

[0035] Under a nitrogen atmosphere, 10 mmol of 2,2-bis[3-(4-aminobenzamido)-4-hydroxyphenyl] (p-6FDAP) and 80 mL of DMAc were added to a 250 mL three-necked flask and stirred at 0 °C for 2 h until completely dissolved. Then, 10 mmol of 4,4'-(hexafluoroisopropene)phthalic anhydride (6FDA) was added to the solution and stirred at 0 °C at 400 rpm for 10 h to obtain a polyamic acid solution.

[0036] The process conditions for preparing the hydroxyl-containing polyimide gas separation membrane from the polyamic acid solution are the same as in Example 1.

[0037] Example 4

[0038] Under a nitrogen atmosphere, 10 mmol of N,N'-[[2,2,2-trifluoro-1-(trifluoromethyl)ethylidene]bis(6-hydroxy-3,1-phenylene)]bis[3-aminobenzamide] (m-6FDAP) and 80 mL of DMAc were added to a 250 mL three-necked flask and stirred at 500 rpm for 2 h at 0 °C until completely dissolved. 10 mmol of 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA) was added to the above solution and stirred at 20 °C for 16 h to obtain a polyamic acid solution.

[0039] The process conditions for preparing the hydroxyl-containing polyimide gas separation membrane from the polyamic acid solution are the same as in Example 1.

[0040] Example 5

[0041] Under a nitrogen atmosphere, 10 mmol of N,N'-[[2,2,2-trifluoro-1-(trifluoromethyl)ethylidene]bis(6-hydroxy-3,1-phenylene)]bis[3-aminobenzamide] (m-6FDAP) and 80 mL of DMAc were added to a 250 mL three-necked flask and stirred at 500 rpm for 2 h at 0 °C until completely dissolved. 10 mmol of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride (BPDA) was added to the above solution and stirred at 10 °C for 16 h to obtain a polyamic acid solution.

[0042] The process conditions for preparing the hydroxyl-containing polyimide gas separation membrane from the polyamic acid solution are the same as in Example 1.

[0043] Example 6

[0044] Under a nitrogen atmosphere, 10 mmol of 3,3'-bis[3-(3-aminobenzoylamino)-4-hydroxyphenyl]diphenyl sulfone (m-DBAHS) and 80 mL of DMAc were added to a 250 mL three-necked flask and stirred at 0 °C for 2 h until completely dissolved. Then, 10 mmol of 4,4'-(hexafluoroisopropene)phthalic anhydride (6FDA) was added to the solution and stirred at 30 °C at 400 rpm for 16 h to obtain a polyamic acid solution.

[0045] The process conditions for preparing the hydroxyl-containing polyimide gas separation membrane from the polyamic acid solution are the same as in Example 1.

[0046] The thermal and permeability properties of the polyimide gas separation membranes prepared in each embodiment were tested, and the results are shown in Table 1.

[0047] The gas permeation flux was tested at 25°C and 0.10 MPa, in Barrers, and the average of three test results was taken.

[0048] Thin film performance testing instruments, testing conditions and methods: Glass transition temperature (T) g Differential scanning calorimeter, Mettler Toledo, DSC822E, test temperature range 50~450℃, heating rate 20℃ / min; Thermogravimetric temperature (T) d Thermogravimetric analyzer (TGA), TGA7, Perkin-Elmer, USA. Test method: heating at a rate of 10 °C / min under N2 conditions. Thermal stability of polyimide films was characterized within the range of 30–800 °C. The initial weight of polyimide was used as a baseline, and the decomposition temperature at which 5% of the polyimide mass decomposed was used as the measure of polyimide thermal stability.

[0049] Table 1 Performance test results of hydroxyl-containing polyimide gas separation membranes in each embodiment

[0050] As shown in Table 1, the polyimide gas separation membrane prepared by this invention has a high glass transition temperature and thermogravimetric temperature, and also exhibits good H2 / N2 and CO2 / N2 permeation selectivity, which can be used for gas purification and gas separation at higher temperatures.

[0051] This invention provides a novel polyimide gas separation membrane material. The separation membrane of this invention is produced by polymerizing a polyamic acid solution containing hydroxyl diamine monomers and dianhydride monomers in an organic solvent. The polyamic acid solution is then defoamed and uniformly coated onto a clean glass or stainless steel plate. After programmed temperature heating and thermal imidization, the polyimide gas separation membrane is hydrothermally exfoliated. By introducing hydroxyl and amide structures into the polymer chain, the separation membrane of this invention, through numerous hydrogen bonds, not only ensures gas separation efficiency but also endows the polyimide membrane with extremely excellent thermal properties, effectively overcoming the technical defect of insufficient thermal stability in existing polyimide gas separation membrane products for high-temperature applications.

[0052] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A hydroxyl-containing polyimide gas separation membrane, characterized in that, The hydroxyl-containing polyimide gas separation membrane is polymerized from a diamine monomer and a dianhydride monomer; the diamine monomer contains hydroxyl groups. The diamine monomer is one or two of the following structural formulas: 、 、 、 、 、 、 、 、 、 、 、 、 、 、 、 ; The dianhydride monomer is one or two of the following structural formulas: 、 、 、 、 、 、 、 。 2. The method for preparing the hydroxyl-containing polyimide gas separation membrane according to claim 1, characterized in that, Includes the following steps: 1) Mix diamine monomer, dianhydride monomer and organic solvent, and carry out polymerization reaction of the mixture to obtain polyamic acid solution; 2) The polyamic acid solution was sequentially defoamed and allowed to stand to obtain the treated polyamic acid solution; 3) The treated polyamic acid solution is scraped onto the substrate and dried to obtain a solid film. The solid film is then subjected to thermal imidization and hydrothermal peeling to obtain a hydroxyl-containing polyimide gas separation membrane.

3. The preparation method according to claim 2, characterized in that, Step 1) The molar ratio of diamine in the diamine monomer to dianhydride in the dianhydride monomer is 0.9~1.1:0.9~1.1, and the organic solvent is one or more of N,N-dimethylacetamide, N-methylpyrrolidone, N,N-dimethylformamide, m-cresol and p-cresol; the solid content of the mixture is 10~40%.

4. The preparation method according to claim 2 or 3, characterized in that, Step 1) The polymerization reaction temperature is -10~30℃, and the polymerization reaction time is 7~18h.

5. The preparation method according to claim 4, characterized in that, Step 2) The vacuum degree of the defoaming treatment is 0.09~0.1MPa, the defoaming treatment time is 30~90min, and the standing time is 12~24h.

6. The preparation method according to claim 5, characterized in that, Step 3) The drying temperature is 55~65℃, the drying vacuum degree is 0.07~0.09MPa, and the drying time is 5~7h; the substrate is a glass plate or a stainless steel plate.

7. The preparation method according to claim 5 or 6, characterized in that, Step 3) The thermal imidization is divided into four stages: the first stage of thermal imidization is performed at a temperature of 50~150℃, a heating rate of 5~10℃ / min, and a holding time of 30~80min; the second stage of thermal imidization is performed at a temperature of 150~250℃, a heating rate of 2~10℃ / min, and a holding time of 30~80min; the third stage of thermal imidization is performed at a temperature of 250~300℃, a heating rate of 1~5℃ / min, and a holding time of 30~80min; the fourth stage of thermal imidization is performed at a temperature of 300~350℃, a heating rate of 1~5℃ / min, and a holding time of 30~80min.

8. The application of the hydroxyl-containing polyimide gas separation membrane according to claim 1 in gas enrichment, gas purification, and gas separation, characterized in that, The gas is either hydrogen or carbon dioxide.