A method for preparing yttrium-type cationic silica sol
By using yttrium element modification to prepare yttrium-type cationic silica sol, the gelation or precipitation problem when silica sol is compounded with cationic systems is solved, enabling the widespread application of silica sol in mid-to-high-end fields, and exhibiting excellent thermal and chemical stability.
Patent Information
- Application Number
- CN202611426345.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional silica sols are prone to gelation or precipitation when combined with cationic systems, which limits their application in mid-to-high-end fields. Furthermore, zirconium-modified silica sols have environmental pollution and stability issues.
Yttrium was used as a modifier. The pH was adjusted by organic acid and then slowly added to alkaline silica sol to form YO-Si chemical bonds, thereby achieving charge reversal on the silica sol surface and preparing yttrium-type cationic silica sol.
Stable yttrium-type cationic silica sol was prepared, which is suitable for food contact materials, medical device coatings and other fields. It has excellent thermal and chemical stability, which expands its application in mid-to-high-end fields.
Smart Images

Figure CN123102250A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of silica sol preparation technology, specifically a method for preparing yttrium-type cationic silica sol. Background Technology
[0002] Silica sol is a colloidal liquid formed by the uniform and stable dispersion of nano-sized silica particles in water, and it belongs to important inorganic polymer nanomaterials. Due to the abundance of silanol groups (-Si-OH) on the surface of silica particles, they possess excellent reactivity and modifiability, and are widely used in precision casting, coatings, textiles, papermaking, electronic polishing, catalyst supports, and other fields.
[0003] Based on pH range, silica sols can be classified into basic silica sols and acidic silica sols. Industrially, basic silica sols are mainly prepared via ion exchange or elemental silica hydrolysis, exhibiting high stability. Acidic silica sols, on the other hand, are typically obtained by treating basic silica sols with cation exchange resins, a process that removes sodium from the system. + Other metal ions are exchanged for H+ in the resin. + However, the change in the double-layer structure leads to a sharp decrease in the stability of acidic silica sol. More importantly, the silica particles in conventional silica sol usually carry a negative charge on their surface. When mixed and used with cationic emulsions, cationic aqueous resins, and other cationic systems, gelation or precipitation easily occurs due to charge neutralization, severely limiting the application of silica sol in cationic systems.
[0004] To address the aforementioned issues, existing technologies have reported the use of metal ions to modify the surface of silica sol. For example, Chinese patent document CN113135573 discloses a zirconium-modified cationic silica sol and its preparation method. This method involves reacting an aqueous zirconium salt solution with an alkaline silica sol, causing the zirconium ion hydrolysis products to condense with silanol groups to form Zr-O-Si bonds, successfully achieving charge reversal (charge modification). However, zirconium is a heavy metal, posing potential environmental pollution and health risks in certain applications with stringent environmental requirements (such as food contact materials, medical device coatings, and high-end electronic materials). Furthermore, there is still room for improvement in the temperature resistance and long-term stability of zirconium-modified silica sol.
[0005] Yttrium (Y), as a rare earth element, possesses a unique electronic structure and chemical properties. Yttrium ions (Y2) 3+ With its high valence state and moderate ionic radius, yttrium's hydrolysis product, Y(OH)3, possesses abundant surface hydroxyl groups, which can undergo condensation reactions with -Si-OH on the surface of silica sol. Compared to zirconium, yttrium exhibits relatively lower toxicity and better biocompatibility, while the unique 4f electron structure of rare earth elements endows it with excellent thermal and chemical stability.
[0006] Yttrium-type cationic silica sols possess both cationic surface properties and the physicochemical properties of rare-earth yttrium, giving them unique applications that distinguish them from conventional silica sols and zirconium-modified silica sols in the following areas: 1) Precision optics and optoelectronics: Y 3+ 4D 0 The electronic configuration exhibits no dd transition absorption in the ultraviolet-visible-near-infrared region, and the YO-Si bonds do not introduce chromophore centers. In antireflection coatings or anti-reflection films, the transmittance at 400–800 nm is ≥85%, far superior to zirconium-modified silica sol (zirconium has strong absorption in the ultraviolet region), making it suitable for camera lenses, solar cell cover plates, and display panels. In optical fiber preform cladding materials, the high-purity Y₂O₃-SiO₂ system has an adjustable refractive index, and the cationic surface facilitates uniform recombination with organosilane precursors, reducing fiber loss. 2) High-temperature structural ceramics and refractory materials: The YO-Si bond has high bond energy, and the melting point of Y2O3 is approximately 2430℃. 3+ Yttrium can stabilize the amorphous structure of SiO2 at high temperatures. In ceramic matrix composite binders, it is used for impregnation and bonding of C / C composites and silicon carbide fiber-reinforced ceramics. After high-temperature sintering, it forms a Y-Si-O glassy phase, improving interfacial bonding strength and oxidation resistance. In high-temperature sealing coatings, it is used in hot-end components of aero-engines; Y2O3 exhibits better resistance to hot corrosion (such as Na2SO4 molten salt) than ZrO2. In nuclear-grade ceramic insulating materials, yttrium has a low neutron absorption cross section, and the Y-Si-O system demonstrates excellent radiation stability in nuclear reactor environments. 3) Catalysis and Adsorption Materials: Y 3+ With moderate Lewis acidity and unique coordination unsaturated sites, the cationic silica sol surface is suitable for loading anionic active species. In automotive exhaust purification catalyst supports, when loading noble metals such as Pd / Pt / Rh, Y... 3+ The Lewis acidity can regulate the metal dispersion, and the YO-Si interface provides unique oxygen vacancies to promote CO / HC oxidation; 4) Electronic Packaging and Dielectric Materials: Y₂O₃ is a high-k dielectric material (k≈15), and the cationic surface of yttrium-type silica sol can form strong electrostatic adsorption with negatively charged substrates (such as alumina and silicon wafers). In semiconductor CMP polishing slurries, cationic SiO₂ abrasives selectively adsorb negatively charged copper / tantalum barrier layers, improving the removal rate; Y can also inhibit copper surface oxidation. As an underfill adhesive for chip packaging, Y₂O₃ acts as an inorganic filler surface treatment agent, enhancing the interfacial bonding between cationic surface-enhancing agents and epoxy resins, thereby improving the material's thermal conductivity and dielectric properties. In thin-film capacitor dielectric layers, spin-coated Y-Si-O films possess both high dielectric constant and low leakage current, making them suitable for flexible electronic devices. 5) Specialty Coatings and Functional Coatings: Can be stably blended with cationic emulsions / resins, offering both optical transparency and weather resistance. Cationic waterborne wood coatings, when blended with cationic polyurethane / acrylic emulsions, do not gel; high transparency preserves the natural texture of wood. Antistatic / static coatings, with their positive surface charge neutralizing static electricity buildup, are used in precision instrument packaging and electronic workshop flooring. In paper surface sizing agents, the cationic properties enable retention with negatively charged pulp fibers, reducing loss; Y2O3 enhances the flame retardancy rating of paper.
[0007] Therefore, developing a method for preparing cationic silica sol using yttrium as a modifier is of great significance for expanding the application of silica sol in mid-to-high-end fields. Summary of the Invention
[0008] This invention proposes a method for preparing yttrium-type cationic silica sol, which solves the problem of gelation or precipitation that easily occurs when traditional silica sol is compounded with cationic systems, and expands the application of silica sol in mid-to-high-end fields.
[0009] The technical solution of this invention is implemented as follows: The first aspect of this invention is to provide a method for preparing yttrium-type cationic silica sol, the steps of which include: S1. Obtain or prepare an aqueous solution of trivalent yttrium salt; S2. Add organic acid to adjust the pH of the yttrium salt aqueous solution to 1.5~2.5; S3. Under stirring conditions, slowly add alkaline silica sol to the yttrium salt aqueous solution obtained in step S2, and then heat to 60~90℃ and react for 0.5~3 h to obtain yttrium-type cationic silica sol.
[0010] Furthermore, the trivalent yttrium salt is selected from one or more of yttrium chloride hexahydrate, yttrium nitrate hexahydrate, yttrium acetate, yttrium sulfate octahydrate, or yttrium bromide nonahydrate.
[0011] Furthermore, the organic acid is selected from one or more of citric acid, tartaric acid, malic acid, mandelic acid, or lactic acid.
[0012] Furthermore, the mass fraction of SiO2 in the alkaline silica sol is 5-40%; And / or, the mass fraction of the yttrium salt aqueous solution is 3-35%; And / or, the mass ratio of the yttrium salt aqueous solution to the alkaline silica sol is 1:(1.5~15).
[0013] Furthermore, the alkaline silica sol contains 0.1-0.6% Na2O by mass and has a pH value of 8.5-11.5. And / or, the particle size of SiO2 particles in the alkaline silica sol is 5~200 nm.
[0014] Furthermore, in step S3, the stirring speed is not less than 500 rpm; and / or, the feeding rate of the alkaline silica sol is 5~35 mL / min, and the feeding process is carried out under normal temperature conditions.
[0015] Furthermore, in step S3, the reaction conditions are 70~90℃ for 1~2 h.
[0016] A second aspect of the present invention is to provide a yttrium-type cationic silica sol, which is prepared by the preparation method described in the first aspect.
[0017] Furthermore, the yttrium-type cationic silica sol satisfies at least one of the following properties: a) The mass fraction of SiO2 is 5%~35%. b) pH value is 1.5~5.0; c) Viscosity of 1~10 mm 2 / s; d) Electrical conductivity is 5~50 mS / cm; e) The Zeta potential is +15 to +65 mV.
[0018] A third aspect of the present invention is to provide the application of the yttrium-type cationic silica sol described in the second aspect in precision casting, coatings, textile auxiliaries, papermaking auxiliaries, electronic polishing fluids, or catalyst carriers.
[0019] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. This invention uses yttrium as a modifier. By first adding an organic acid to adjust the pH and then complexing it, a cationic silica sol with a positively charged surface is successfully prepared through a slow alkaline silica sol method. This effectively solves the problem that gelation or precipitation easily occurs when traditional silica sol is compounded with cationic systems.
[0020] 2. Compared with existing zirconium-type charge-modified cationic silica sols, this invention uses the rare earth element yttrium to replace the heavy metal zirconium, which has relatively lower toxicity, better biocompatibility, and is more in line with green chemistry and environmental protection requirements. It is also more suitable for fields with high safety requirements, such as food contact materials and medical device coatings.
[0021] 3. The yttrium-type cationic silica sol prepared by this invention contains rare earth yttrium and has excellent thermal stability. The obtained yttrium-type cationic silica sol can be stably stored at 60°C for more than 4 months and at room temperature for more than 12 months.
[0022] 4. The yttrium element in the obtained yttrium-type cationic silica sol is uniformly distributed on the particle surface, which endows the product with excellent high-temperature resistance and chemical stability, and has broad application prospects in precision casting, high-end coatings, electronic polishing and other fields.
[0023] 5. The preparation process of this invention is simple, requires no complex equipment, and the reaction conditions are relatively mild, making it easy to achieve large-scale industrial production. Attached Figure Description
[0024] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0025] Figure 1 This is a scanning electron microscope characterization image of the alkaline silica sol in Example 1 of the present invention; Figure 2 This is a Zeta potential distribution diagram of the alkaline silica sol used in Example 1 of the present invention; Figure 3 This is a scanning electron microscope image of the yttrium-type cationic silica sol obtained in Example 1 of the present invention; Figure 4 This is a Zeta potential distribution diagram of the yttrium-type cationic silica sol obtained in Example 1 of the present invention; Figure 5 This is a Zeta potential distribution diagram of the acidic silica sol obtained in Comparative Example 1 of the present invention. Detailed Implementation
[0026] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0027] This invention provides a method for preparing yttrium-type cationic silica sol, the steps of which include: S1. Obtain or prepare an aqueous solution of trivalent yttrium salt; S2. Add organic acid to adjust the pH of the yttrium salt aqueous solution to 1.0~3.0; S3. Under stirring conditions, alkaline silica sol is slowly added to the yttrium salt aqueous solution obtained in step S2, and then the temperature is raised to 60~90℃ and reacted for 0.5~3h to obtain yttrium-type cationic silica sol.
[0028] The reaction principle for preparing yttrium-type cationic silica sol in this invention is as follows: When trivalent yttrium salts dissolve in water, Y 3+A hydrolysis reaction occurs, which is accelerated by heating, forming a hydroxyyttrium polymer mainly composed of Y(OH)3. The surface of this hydrolysis product is rich in active hydroxyl groups (=Y-OH). When alkaline silica sol is added to an aqueous solution of yttrium salt, the pH of the system gradually decreases. The hydrolysis products of yttrium undergo a dehydration condensation reaction with the silanol groups (≡Si-OH) on the surface of the silica sol particles, forming stable YO-Si- chemical bonds. Since yttrium ions are positively charged, and the formation of YO-Si- bonds alters the electric double layer structure on the particle surface, the originally negatively charged surface charge of the silica sol particles is reversed to positive, ultimately yielding a stable yttrium-type acidic cationic silica sol.
[0029] The main reactions are illustrated below: Y 3+ + 3H₂O → Y(OH)₃ + 3H + ≡Si-OH + HO-Y= → ≡Si-OY= + H2O It is worth noting that the preparation process of the yttrium-type cationic silica sol described in this invention has the following technical bottlenecks: 1) Precise control of hydrolysis-condensation kinetics, Y 3+ The hydrolysis behavior is better than that of other metal ions (such as Zr). 4+ (etc.) are more complex and difficult to predict.
[0030] a. Multi-step hydrolysis equilibrium: Y 3+ Hydrolysis in water is not a simple one-step process, but involves multiple equilibria: Y 3+ [Y(OH)] 2+ [Y(OH)2] + Y(OH)3. The dominant products are completely different at different pH values, and during the dropwise addition of silica sol, the pH of the yttrium salt system gradually increases from strongly acidic. 3+ The hydrolysis state of the silanol group changes continuously, resulting in uncontrollable active sites that react with the silanol group.
[0031] b. Hydroxyl-bridged polymerization tendency: rare earth ions (including Y) 3+ It readily forms polynuclear clusters or chains, such as [Y2(OH)2], through hydroxyl bridging (μ2-OH). 4+ [Y4(OH)8] 8+ If these multinucleated species cannot be anchored on the silica surface in time, they will nucleate and grow independently into Y2O3 or Y(OH)3 nanoparticles, causing the system to become turbid, reduce light transmittance, and even induce gelation.
[0032] c. with Zr 4+ Comparison: Zr 4+Although it has a higher charge density, its hydrolysis products (such as [Zr4(OH)8(H2O)) 16 ] 8+ The structure is relatively well-defined and clear, and its condensation reaction with silanol groups is highly reactive, exhibiting a clear "switch" characteristic. Meanwhile, Y... 3+ The reactivity is moderate and the window is narrow; "insufficient reactivity leads to incomplete modification, while excessive reactivity results in independent phase formation."
[0033] The inventors of this invention discovered that it is necessary to use a suitable complexing agent (such as citric acid) with Y. 3+ Forming stable precursor complexes to achieve Y 3+ The "slow release" method maintains the concentration of effective hydrolysis products within a narrow range.
[0034] 2) Critical stoichiometric control of surface charge reversal: There is a narrow stoichiometric window for achieving charge reversal from negative to positive.
[0035] a. Charge reversal threshold: The surface of silica sol particles is initially negatively charged (Zeta potential approximately -20 to -40 mV). Sufficient Yg is required to achieve cationization. 3+ The hydrolysis products neutralize the surface negative charge and provide excess positive charge. However, Y... 3+ As a trivalent ion, its "charge contribution efficiency" is theoretically lower than that of tetravalent Zr. 4+ Therefore, more Y is needed. 3+ Only then can the same effect be achieved.
[0036] b. Risk of gelation: Excessive Y 3+ (Especially in the free state) it will act as a crosslinking agent, bridging different silica sol particles through YO-Si-OY, leading to an increase in the viscosity of the system and gelation.
[0037] c. Critical mass ratio: The mass ratio of yttrium salt aqueous solution to alkaline silica sol needs to be strictly controlled. Exceeding this ratio will lead to incomplete charge reversal or direct gel formation.
[0038] This invention employs a reverse addition method (adding silica sol dropwise to the yttrium salt solution, rather than adding the yttrium salt to the silica sol) to ensure that the reaction is always carried out at high γ levels. 3+ The process is carried out within the concentration zone to promote surface saturation adsorption; at the same time, the feeding rate is controlled to avoid localized Y... 3+ Too low a concentration leads to uneven modification.
[0039] 3) The contradiction between double layer reconstruction and colloidal stability: The double layer of cationic silica sol needs to be reconstructed on the basis of anionic silica sol. The reconstruction process needs to go through the equilibrium fragility point of anionic silica sol. Anionic silica sol itself needs a cationic double layer with positive charge on the surface to balance it, while the balance ions of the double layer after becoming cationic silica sol are exactly the opposite.
[0040] a. Counterion compression effect: The modified system is acidic (pH 1.5~4.0), at which point the solution contains a high concentration of H+. + Cl - / NO3 - Counterions compress the electric double layer. 3+ Although the modified particles are positively charged, their double-layer thickness may not be sufficient to provide long-term stability.
[0041] b. Electrostatic repulsion and van der Waals attraction: Y 3+ The absolute value of the Zeta potential on the surface of the modified particles is usually lower than that of the original anionic silica sol (+12~+55 mV vs -20~-40 mV). The electrostatic repulsion barrier between particles is reduced, making them more likely to aggregate due to Brownian motion collisions.
[0042] c. Temperature sensitivity: The YO-Si bonds may hydrolyze and break during high temperatures or long-term storage, leading to surface Y... 3+ Shedding and charge reversal cause failure.
[0043] The inventors of this invention have discovered that it is necessary to use complexing agents and optimize the reaction temperature (70~90℃) to ensure the full formation and dense coverage of YO-Si bonds, while controlling the pH of the product to be no less than 1.5 to avoid excessive acidification leading to excessive compression of the electric double layer.
[0044] 4) Balance between optical transparency and degree of modification (this applies to cationic silica sols with small particle size or high light transmittance requirements): There is an inherent contradiction between the requirement for high light transmittance and sufficient modification.
[0045] a. Scattering loss of independent phases: Any Y2O3 or Y(OH)3 nanoparticles that are not anchored to the surface of silica sol have a large difference in refractive index from SiO2 and will become optical scattering centers, resulting in a decrease in light transmittance.
[0046] b. Increased surface roughness: Y 3+ The uneven deposition of hydrolysis products on the SiO2 surface increases the surface roughness of the particles and enhances Rayleigh scattering.
[0047] Comparison with zirconium modification: Zr 4+ Even with slight agglomeration, the modified silica sol exhibits a significant difference in refractive index between ZrO2 (~2.1) and SiO2 (~1.46). 4+ It exhibits high reactivity and high anchoring efficiency; while Y₂O₃ also has a relatively high refractive index (~1.9). 3 + Independent phase formation causes more severe damage to light transmittance.
[0048] If a transmittance of ≥85% in the 400–800 nm visible light region is required, this necessitates precise control of the complexing agent Y.3+ Release to avoid local oversaturation; control reaction time (0.5~2.5h) to ensure sufficient reaction while avoiding excessive condensation; and prefer small-particle-size silica sol (5~30 nm) to reduce intrinsic scattering.
[0049] 5) Screening and adaptation of complexing agent systems: Not all complexing agents are suitable for Y. 3+ - Silica sol system.
[0050] a. Complexation strength matching: complexing agent to Y 3+ The complexation constant (log K) must be moderate; too strong a constant (such as EDTA, log K≈18) will cause Y to... 3+ Under the reaction conditions, it is difficult to release the substance, and the modification is incomplete; if it is too weak (such as acetate), it will not have a sustained-release effect. Citric acid (log K≈8~10) is in the better range.
[0051] b. Steric hindrance effect: Macromolecular complexing agents (such as EDTA) may be present in the Y... 3+ The steric hindrance between the silanol group and the silanol group hinders the formation of YO-Si bonds.
[0052] c. Side reaction risk: Some complexing agents (such as sulfur-containing ligands) may react with silica sol or introduce colored groups.
[0053] In this invention, the trivalent yttrium salt is selected from one or more common soluble yttrium salts selected from yttrium chloride hexahydrate, yttrium nitrate hexahydrate, yttrium acetate, yttrium sulfate octahydrate, or yttrium bromide nonahydrate.
[0054] In this invention, the organic acid is an α-hydroxycarboxylic acid, selected from one or more of citric acid, tartaric acid, malic acid, mandelic acid, or lactic acid; the pH of the yttrium salt aqueous solution is adjusted using the above organic acid, preferably to a pH of 1.5 to 2.5.
[0055] In this invention, the mass fraction of SiO2 in the alkaline silica sol is 5-40%, and the mass fraction of the yttrium salt aqueous solution is 3-35%, more preferably 15-30%; the mass ratio of the yttrium salt aqueous solution to the alkaline silica sol is 1:(1.5-15), preferably 1:(2-10), to ensure a suitable ratio for the yttrium salt and alkaline silica sol to fully react and generate YO-Si bonds, promoting saturated adsorption on the silica sol surface while avoiding the formation of YO-Si bonds. 3+ Excessive bridging of different silica sol particles leads to increased viscosity and gelation of the system.
[0056] In a preferred embodiment, the alkaline silica sol contains 0.1-0.6% Na2O by mass and has a pH value of 8.5-11.5.
[0057] In a preferred embodiment, the SiO2 particles in the alkaline silica sol have a particle size of 5~200 nm. After modification with yttrium salt, a cationic silica sol is generated with a stable zeta potential and good silica sol stability. Moreover, this particle size is suitable for a wide range of applications.
[0058] In a preferred embodiment, in step S3, the stirring speed is not less than 500 rpm. A higher stirring speed generates stronger shear force, enhancing the hydrolysis effect and preventing gel formation. The alkaline silica sol is added at a rate of 5~35 mL / min to prevent localized Y-phase formation in the reaction system. 3+ Too low a concentration leads to uneven modification, so the feeding process is carried out at room temperature without the need for heating.
[0059] In a preferred embodiment, in step S3, the reaction conditions are 70~90℃ for 1~2h. Under these reaction conditions, hydrolysis is promoted to form a surface rich in active hydroxyl groups, which undergo dehydration condensation reaction with the silanol groups (≡Si-OH) on the surface of the silica sol particles to form stable YO-Si- chemical bonds.
[0060] The yttrium-type cationic silica sol prepared by the above-described preparation method of the present invention satisfies the following properties: a) The mass fraction of SiO2 is 5%~35%. b) pH value is 1.5~5.0; c) Viscosity of 1~10 mm 2 / s; d) Electrical conductivity is 5~50 mS / cm; e) The Zeta potential is +15 to +65 mV.
[0061] The yttrium-type cationic silica sol described above possesses long-term stability and excellent positive charge properties, and can be well compounded with cationic systems. Combining the advantages of yttrium itself, it can be used in mid-to-high-end fields such as precision casting, coatings, textile auxiliaries, papermaking auxiliaries, electronic polishing fluids, or catalyst carriers.
[0062] The following are preferred embodiments of the present invention. Unless otherwise specified, the reagents used are commercially available standards in the art, and the experimental methods used are those well-known in the art.
[0063] The alkaline silica sol used in the examples was prepared by ion exchange, and the stabilizer was NaOH. The specific preparation method is based on existing technology.
[0064] Example 1
[0065] Yttrium chloride hexahydrate (YCl3·6H2O) was dissolved in deionized water to prepare a 25% (w / w) YCl3 aqueous solution, and the pH was adjusted to 2.0 with 2% citric acid. Then, under vigorous stirring at 500 rpm, alkaline silica sol (pH=9.82, SiO2 particle size approximately 14 nm, mass fraction 35%, Na2O mass fraction 0.3%) was slowly added to the prepared YCl3 aqueous solution at a rate of 25 mL / min, with a mass ratio of YCl3 aqueous solution to alkaline silica sol of 1:3.5. After the addition was complete, the temperature was raised to 80℃ and the reaction was continued for 2 h. After the reaction was completed, the solution was cooled to room temperature to obtain small-particle-size yttrium-type cationic silica sol.
[0066] Example 2
[0067] Yttrium chloride hexahydrate (YCl3·6H2O) was dissolved in deionized water to prepare a 25% (w / w) YCl3 aqueous solution, and the pH was adjusted to 1.8 with 2% citric acid. Then, under vigorous stirring at 500 rpm, alkaline silica sol (pH=10.20, SiO2 particle size approximately 50 nm, mass fraction 35%, Na2O mass fraction 0.26%) was slowly added to the prepared YCl3 aqueous solution at a rate of 25 mL / min, with a mass ratio of YCl3 aqueous solution to alkaline silica sol of 1:5.0. After the addition was complete, the temperature was raised to 80℃ and the reaction was continued for 2 h. After the reaction was completed, the solution was cooled to room temperature to obtain a medium-particle-size yttrium-type cationic silica sol.
[0068] Example 3
[0069] Yttrium chloride hexahydrate (YCl3·6H2O) was dissolved in deionized water to prepare a 25% (w / w) YCl3 aqueous solution, and the pH was adjusted to 2.2 with 2% citric acid. Then, under vigorous stirring at 500 rpm, alkaline silica sol (pH=10.81, SiO2 particle size approximately 100 nm, 35% (w / w), Na2O 0.25% (w / w)) was slowly added to the prepared YCl3 aqueous solution at a rate of 25 mL / min. The mass ratio of YCl3 aqueous solution to alkaline silica sol was 1:7.8. After the addition was complete, the temperature was raised to 75℃ and the reaction was continued for 2 h. After the reaction was completed, the solution was cooled to room temperature to obtain large-particle-size yttrium-type cationic silica sol.
[0070] Example 4
[0071] Yttrium nitrate hexahydrate (Y(NO3)3·6H2O) was dissolved in deionized water to prepare a 25% (w / w) Y(NO3)3 aqueous solution, and the pH was adjusted to 2.0 with 2% citric acid. Then, under vigorous stirring at 500 rpm, alkaline silica sol (pH=9.82, SiO2 particle size approximately 14 nm, mass fraction 35%, Na2O mass fraction 0.3%) was slowly added to the prepared Y(NO3)3 aqueous solution at a rate of 25 mL / min, with a mass ratio of Y(NO3)3 aqueous solution to alkaline silica sol of 1:3.8. After the addition was complete, the temperature was raised to 85℃ and the reaction was continued for 2 h. After the reaction was completed, the solution was cooled to room temperature to obtain small-particle-size yttrium-type cationic silica sol.
[0072] Example 5
[0073] Yttrium chloride hexahydrate (YCl3·6H2O) was dissolved in deionized water to prepare a 25% (w / w) YCl3 aqueous solution, and the pH was adjusted to 2.0 with 2% tartaric acid. Then, under vigorous stirring at 500 rpm, alkaline silica sol (pH=9.82, particle size approximately 14 nm, SiO2 mass fraction 35%, Na2O mass fraction 0.3%) was slowly added to the prepared YCl3 aqueous solution at a rate of 25 mL / min, with a YCl3 aqueous solution to alkaline silica sol mass ratio of 1:2.8. After the addition was complete, the temperature was raised to 80℃ and the reaction was continued for 2 h. After the reaction was completed, the solution was cooled to room temperature to obtain small-particle-size yttrium-type cationic silica sol.
[0074] Comparative Example 1
[0075] Take the same alkaline silica sol as in Example 1, first perform ion exchange treatment through the regenerated cation exchange resin, and then dilute it with distilled water to the same concentration as in Example 1 to obtain acidic silica sol.
[0076] Comparative Example 2
[0077] The method was the same as in Example 1, except that the addition method was changed to adding an aqueous solution of YCl3 to the alkaline silica sol. During the addition process, it was found that the silica sol particles agglomerated and eventually formed a gel.
[0078] Comparative Example 3
[0079] The method was followed in Example 1, except that the mass ratio of YCl3 aqueous solution to alkaline silica sol was adjusted to 1:18. During the addition process, the reaction system became turbid, and after continued stirring, it gelled, making it impossible to obtain a stable yttrium-type cationic silica sol.
[0080] Comparative Example 4
[0081] The method is the same as in Example 1, except that the mass ratio of YCl3 aqueous solution to alkaline silica sol is adjusted to 1:1.
[0082] Comparative Example 5
[0083] The method was followed as in Example 1, except that the pH was adjusted to 1.0 with 2% citric acid. Turbidity occurred during heating.
[0084] Comparative Example 6
[0085] The method was followed as in Example 1, except that the pH was adjusted to 4.0 with 2% citric acid. During the addition process, turbidity and gelation occurred.
[0086] Comparative Example 7
[0087] The method was followed in Example 1, except that the heating temperature was increased to 95°C. During the heating process, turbidity occurred.
[0088] Comparative Example 8
[0089] The method was followed as in Example 1, except that the heating temperature was adjusted to 50°C. The solution remained clear and stable.
[0090] Comparative Example 9
[0091] The method was followed as in Example 1, except that citric acid was replaced with ethylenediaminetetraacetic acid (EDTA). The solution remained clear and stable throughout.
[0092] Comparative Example 10
[0093] The method is the same as in Example 1, except that citric acid is replaced with acetic acid. During the addition process, the solution becomes cloudy, forming a precipitate or gel.
[0094] Test case
[0095] 1. Characterization and detection
[0096] In Example 1 above, the SEM images and Zeta potential diagrams of the small-particle-size alkaline anionic silica sol are shown below. Figure 1 , Figure 2 As shown; the SEM images and Zeta potential diagrams of the yttrium-type cationic silica sol prepared with small particle size are shown below. Figure 3 , Figure 4 As shown; in Comparative Example 1, the Zeta potential diagram of the small-particle-size acidic anionic silica sol prepared is shown. Figure 5 As shown.
[0097] 2. Performance Comparison and Analysis
[0098] The above Examples 1-5 were compared with the original alkaline anionic silica sol, and the silica sols obtained from Comparative Examples 1-10 were tested for relevant performance. The results are shown in Table 1 and Table 2, respectively.
[0099] Table 1: Comparison of various indicators between the examples and the original alkaline anionic silica sol
[0100] As can be seen from the data in Table 1, the zeta potential of the cationic silica sols prepared in Examples 1-5 changed significantly from negative to positive compared with the original alkaline anionic silica sols, thus achieving charge modification. Its significant feature is that the yttrium-type cationic silica sols are acidic silica sols with increased conductivity.
[0101] Table 2: Comparison of various indicators between the examples and the comparative examples
[0102] Based on the data in Table 2, it can be seen that the cationic silica sols prepared in Examples 1 to 5 can change the surface charge of silica sol particles from negative to positive, and the absolute value of the charge is significantly increased. This can enhance the charge repulsion between sol particles and significantly improve the storage stability of acidic silica sols compared with Comparative Example 1.
[0103] In the preparation of yttrium-type cationic silica sol, alkaline silica sol can only be added dropwise to the yttrium salt aqueous solution, and cannot be added in reverse. If added in reverse, the surface charge of the silica sol particles will rapidly reverse due to excessive local acidity, but uniform coating will not be achieved, resulting in agglomeration between particles and eventually forming a gel (Comparative Example 2).
[0104] In the preparation of yttrium-type cationic silica sol, the amount of alkaline silica sol used should not be excessive; otherwise, the yttrium salt content in the system will be too low, and the positive charge will be insufficient to cover the surface of the original anionic silica sol particles, thus failing to achieve surface charge reversal and system stabilization. Conversely, the amount of alkaline silica sol used should not be too small; otherwise, excessive anion collisions in the system will prevent the new cationic silica sol from maintaining long-term stability (Comparative Examples 3 and 4).
[0105] In the preparation of yttrium-type cationic silica sol, the pH of the system must be properly adjusted using citric acid. If the acidity is too strong, the yttrium salt will exist as a large number of hydrated yttrium ions, which will rapidly compress the electric double layer of the anionic silica sol and cause gelation. If the acidity is too weak, the hydrolysis of yttrium ions will lead to the transformation into uncharged precipitation, which will make the system turbid (Comparative Examples 5 and 6).
[0106] In the preparation of yttrium-type cationic silica sol, the reaction temperature must be kept appropriate. If the temperature is too high, Brownian motion will be accelerated, causing collisions in the gel. If the temperature is too low, effective dehydration condensation cannot be achieved to form dense encapsulations (Comparative Examples 7 and 8).
[0107] In the preparation of yttrium-type cationic silica sol, the binding ability of the complexing agent must be appropriate. If it is too strong, the yttrium ions cannot be effectively released to achieve charge reversal. If it is too weak, the release is rapid, which is disadvantageous in subsequent reactions (Comparative Examples 9 and 10).
[0108] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing yttrium-type cationic silica sol, characterized in that the steps include... include: S1. Obtain or prepare an aqueous solution of trivalent yttrium salt; S2. Add organic acid to adjust the pH of the yttrium salt aqueous solution to 1.5~2.5; S3. Under stirring conditions, slowly add alkaline silica sol to the yttrium salt aqueous solution obtained in step S2, and then heat to 60~90℃ and react for 0.5~3 h to obtain yttrium-type cationic silica sol.
2. The preparation method according to claim 1, characterized in that, The trivalent yttrium salt is selected from one or more of yttrium chloride hexahydrate, yttrium nitrate hexahydrate, yttrium acetate, yttrium sulfate octahydrate, or yttrium bromide nonahydrate.
3. The preparation method according to claim 1, characterized in that, The organic acid is selected from one or more of citric acid, tartaric acid, malic acid, mandelic acid, or lactic acid.
4. The preparation method according to claim 1, characterized in that, The mass fraction of SiO2 in the alkaline silica sol is 5-40%. And / or, the mass fraction of the yttrium salt aqueous solution is 3-35%; And / or, the mass ratio of the yttrium salt aqueous solution to the alkaline silica sol is 1:(1.5~15).
5. The preparation method according to claim 1, characterized in that, The alkaline silica sol contains 0.1-0.6% Na2O by mass and has a pH value of 8.5-11.
5. And / or, the particle size of SiO2 particles in the alkaline silica sol is 5~200 nm.
6. The preparation method according to claim 1, characterized in that, In step S3, the stirring speed is not less than 500 rpm; and / or the feeding rate of the alkaline silica sol is 5~35 mL / min, and the feeding process is carried out under normal temperature conditions.
7. The preparation method according to claim 1, characterized in that, In step S3, the reaction conditions are 70~90℃ for 1~2 h.
8. A yttrium-type cationic silica sol, characterized in that, It is prepared by the preparation method according to any one of claims 1-8.
9. The yttrium-type cationic silica sol as described in claim 8, characterized in that, The yttrium-type cationic silica sol satisfies at least one of the following properties: a) The mass fraction of SiO2 is 5-35%. b) pH value is 1.5~5.0; c) Viscosity of 1~10 mm 2 / s; d) Electrical conductivity is 5~50 mS / cm; e) The Zeta potential is +15 to +65 mV.
10. The application of the yttrium-type cationic silica sol of claim 8 in precision casting, coatings, textile auxiliaries, papermaking auxiliaries, electronic polishing fluids, or catalyst carriers.