Silica mortar for concrete and preparation method thereof

By preparing uniform and stable silica fume mortar, the problem of reduced reactivity of silica fume in concrete is solved, and the performance of silica fume concrete is improved, which is suitable for promotion and application.

CN118908618APending Publication Date: 2024-11-08CHINA CONSTR WEST CONSTR SOUTHWEST CO LTD +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410893421.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When used in concrete, the reactive activity of silica fume is reduced due to encryption treatment, which affects transportation efficiency and performance, and the properties of fine powder make it difficult to transport and store.

Method used

Using a concrete mortar, the preparation of fume, water, dispersant, stabilizer, thickener and defoaming agent, control the pH value between 2 and 4, and stir with a high-speed dispersion shearing machine to prepare uniform and stable Silicone fume mortar reduces the particle size of silicon fume and improves reaction activity.

Benefits of technology

It significantly improves the working performance, mechanical properties and durability of fume concrete, improves the utilization efficiency of fume particles, and is suitable for promotion and application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004928251930000071
    Figure BDA0004928251930000071
  • Figure BDA0004928251930000081
    Figure BDA0004928251930000081
Patent Text Reader

Abstract

The invention discloses silica mortar for concrete. The silica mortar comprises the following raw materials in parts by weight: 30-50 parts of silica fume, 50-70 parts of water, 0.6-5 parts of a dispersing agent, 0.6-2.5 parts of a stabilizer, 0.05-0.2 part of a thickening agent and 0.1-0.5 part of a defoaming agent, wherein the pH value of the silica mortar is adjusted to be 2-4 by a pH regulator. The silica fume is used as a main raw material, the composition of the dense silica fume is regulated and controlled, the composite dispersing agent, the stabilizer, the thickening agent and the defoaming agent are combined, and the pH value of the slurry is regulated by using the organic acid; the uniform and stable silica mortar is prepared through comprehensive action of various means, the utilization efficiency of silica fume particles can be greatly improved, the particle size of the silica fume particles is effectively reduced, the reaction activity of silica fume is improved, and the working performance, mechanical performance, durability and the like of silica fume concrete are improved; a new thought can be provided for efficient application of the silica fume.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to silicon mortar for concrete and a preparation method thereof. Background Art

[0002] Silica fume, also known as silicon powder, is a byproduct of the production of silicon metal or ferrosilicon alloy in an electric arc furnace. Its main component is amorphous silicon dioxide, with a content of 85-96%. Silica fume particles are very fine, with an average particle size of 0.1-1um, which is about 1 / 100 of ordinary cement particles. It is a highly active volcanic ash mineral admixture. Adding silica fume to cement concrete can improve the strength, impermeability, frost resistance and chemical corrosion resistance of concrete, and can also inhibit or reduce alkali aggregate reaction. However, the bulk density of silica fume is only 120-280kg / m 3 It is a fine powder that easily flies, making it difficult to transport, store and use.

[0003] In response to the above technical problems, the commonly used treatment method is to densify the silica fume to make it have a higher bulk density, thereby reducing transportation costs. However, after the silica fume is densified, it will cause problems such as particle agglomeration, which will greatly reduce the reactivity of the silica fume and is not conducive to the performance of its performance in concrete. How to improve the transportation efficiency of silica fume while effectively improving the reactivity of silica fume in concrete is a major problem in the concrete industry. Summary of the invention

[0004] The main purpose of the present invention is to provide a silica ash mortar for concrete in view of the problems and shortcomings of the prior art, prepare silica ash into a uniform and stable silica ash mortar, effectively reduce the particle size of silica ash particles, enhance the reaction activity of silica ash, and thereby effectively improve the working performance, mechanical properties and durability of silica ash concrete.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A silica ash mortar for concrete, the raw materials and their weight proportions include: 30-50 parts of silica ash, 50-70 parts of water, 0.6-5 parts of dispersant, 0.6-2.5 parts of stabilizer, 0.05-0.2 parts of thickener, 0.1-0.5 parts of defoamer, and pH regulator to adjust the pH value of the silica ash mortar to 2-4.

[0007] In the above scheme, the silica fume is densified silica fume with a bulk density of 650-700 kg / m 3 The SiO2 content in the silica ash is not less than 90wt%, and the total content of CaO, MgO and Fe2O3 is less than 2.5wt%.

[0008] In the above scheme, the dispersant is two or more selected from polyvinyl pyrrolidone (molecular weight 18000-20000), polysorbate 40, dodecyl glucoside, arachidonic glucoside and the like.

[0009] In the above scheme, the stabilizer is a polyethylene glycol polyvinyl alcohol graft copolymer; it is obtained by grafting low-polymerization degree polyvinyl alcohol (molecular weight 25000-28000) with polyethylene glycol (molecular weight 400-500); its molecular weight is 27000-28500.

[0010] In the above scheme, the thickener is one or more of guar gum (molecular weight 120000-150000), gelatin (molecular weight 14000-18000), etc.

[0011] In the above scheme, the defoaming agent is a silicone defoaming agent.

[0012] In the above scheme, the pH adjuster is one or more of formic acid, acetic acid, etc.

[0013] The above-mentioned method for preparing silica mortar for concrete comprises the following steps:

[0014] (1) Weigh silica fume, water, dispersant, stabilizer, thickener and defoamer according to the proportion and put them into the mixing equipment;

[0015] (2) stirring at room temperature;

[0016] (3) Then, a pH adjuster is slowly added into the obtained slurry to adjust the pH value of the obtained silica ash slurry to 2-4.

[0017] In the above scheme, a high-speed dispersing shearing machine is used in step (2), and the edge linear speed of the stirring blade is 60 to 80 m / s; and the stirring treatment time is 20 to 30 min.

[0018] In the above scheme, the room temperature condition in step (2) is 20-30°C.

[0019] The silica ash mortar for concrete prepared according to the above scheme has a D50 of 1.0-1.5 μm and a fluidity of 210-240 mm. It can remain uniform and stable without stratification for more than 14 days, and its activity index can be increased by 15% or more compared with the original densified silica ash.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The total content of CaO, MgO and Fe2O3 in the silica ash used in the present invention is less than 2.5wt%, which can effectively prevent the silica ash from reacting with water to form precipitates such as Ca(OH)2, Mg(OH)2, Fe(OH)3, etc., ensure the uniformity and stability of the resulting silica ash slurry, and is beneficial to controlling the particle size of the silica ash slurry particles. At the same time, it can avoid the problem that Ca(OH)2 reacts prematurely with the active SiO2 in the silica ash, thereby reducing the subsequent reaction activity of the silica ash.

[0022] (2) During the densification process, silica fume is affected by different densification methods, resulting in different charges on the surface of silica fume particles. The present invention further introduces a non-ionic dispersant with specific compounding conditions, which has better versatility and stability.

[0023] (3) There is a large amount of active SiO2 in the silica mortar. In the present invention, the pH value of the silica mortar is maintained at 2 to 4 by using pH regulators such as formic acid and acetic acid, and a small amount of Ca(OH)2, Mg(OH)2, Fe(OH)3 and the like in the silica mortar can be promoted to precipitate and react to generate soluble salts, which can effectively ensure the stability, uniformity and activity of the silica mortar and is conducive to refining the particle size in the silica mortar;

[0024] (4) The present invention controls the temperature of the silica ash slurry during stirring to 20-30°C, on the one hand to avoid the temperature being too low to weaken the dispersant effect; on the other hand, if the temperature is too high, the surface tension of the silica ash slurry will decrease during stirring, making it more likely to foam, resulting in the weakening of the shearing effect on the silica ash particles during stirring, which seriously reduces the dispersion efficiency.

[0025] (5) The present invention regulates the composition of densified silica fume, combines a composite dispersant and a preferred stabilizer, thickener, and defoamer, and uses an organic acid to adjust the pH value of the slurry; through the combined effect of various means, a silica fume slurry with good uniformity, good stability, and extremely high activity is prepared, which can greatly improve the utilization efficiency of silica fume particles and is suitable for promotion and application. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0027] In the following examples, the stabilizer used is a polyethylene glycol polyvinyl alcohol graft copolymer; it is obtained by grafting low-polymerization degree polyvinyl alcohol (molecular weight 26,000) with polyethylene glycol 400 in a molar ratio of 1:1; its molecular weight is 26,400.

[0028] The organic silicon defoamer used is THIX-278 defoamer produced by Hengxin Chemical Technology Co., Ltd.

[0029] In the following examples, a high-speed dispersing shearing machine is used in the stirring step, and the edge linear speed of the stirring blade is 60 to 80 m / s.

[0030] Example 1

[0031] A silica ash mortar for concrete, the raw materials used include, by weight: 40 parts of silica ash (silica ash A), 60 parts of water, 1.0 parts of dispersant, 0.8 parts of stabilizer, 0.15 parts of thickener, and 0.1 parts of defoamer; wherein the silica ash A used is densified silica ash, the SiO2 content in the silica ash is 90wt%, and the total content of CaO, MgO and Fe2O3 is 1.5wt%; the dispersant is prepared by mixing polysorbate 40 and dodecyl glucoside in a mass ratio of 4:6; the stabilizer is a polyethylene glycol polyvinyl alcohol copolymer; the thickener is guar gum (molecular weight 150000); the defoamer is an organosilicon defoamer; and the pH value regulator is formic acid;

[0032] The preparation method of the silica slurry is as follows:

[0033] (1) Weigh silica fume, water, dispersant, stabilizer, thickener and defoamer according to the proportion, and then put them into a stirring device;

[0034] (2) Turn on the stirring equipment and adjust the stirring speed to the specified speed (60m / s) for 30 minutes. During stirring, the temperature of the silica ash slurry should be controlled at 25°C;

[0035] (3) Then, the pH regulator is slowly added into the slurry to adjust the pH value of the silica ash slurry to 3, and the slurry is stirred evenly to obtain the silica ash slurry for concrete.

[0036] Example 2

[0037] A silica ash mortar for concrete, the raw materials used include, by weight: 50 parts of silica ash (silica ash B), 50 parts of water, 2.5 parts of dispersant, 1.5 parts of stabilizer, 0.15 parts of thickener, and 0.15 parts of defoamer; wherein the silica ash B used is densified silica ash, the SiO2 content in the silica ash is 92wt%, and the total content of CaO, MgO and Fe2O3 is 1.5wt%; the dispersant is a mixture of polysorbate 40, dodecyl glucoside and arachidonic glucoside in a mass ratio of 2:5:3; the stabilizer is a polyethylene glycol polyvinyl alcohol copolymer; the thickener is a mixture of guar gum (molecular weight of 150000) and gelatin (molecular weight of 15000) in a mass ratio of 6:4; the defoamer is an organosilicon defoamer; and the pH value regulator is a mixture of formic acid and acetic acid in a mass ratio of 3:7;

[0038] The preparation method of the silica slurry is as follows:

[0039] (1) Weigh silica fume, water, dispersant, stabilizer, thickener and defoamer according to the proportion, and then put them into a stirring device;

[0040] (2) Turn on the stirring equipment and adjust the stirring speed to the specified speed (80 m / s) for 30 min. During stirring, the temperature of the silica ash slurry is controlled to be 22° C.;

[0041] (3) Then, the pH regulator is slowly added into the slurry to adjust the pH value of the silica ash slurry to 3, and the slurry is stirred evenly to obtain the silica ash slurry for concrete.

[0042] Example 3

[0043] A silica ash mortar for concrete, the raw materials used include, by weight: 45 parts of silica ash (silica ash C), 55 parts of water, 2.0 parts of dispersant, 1.5 parts of stabilizer, 0.15 parts of thickener, and 0.15 parts of defoamer; wherein the silica ash C used is densified silica ash, the SiO2 content in the silica ash is 94wt%, and the total content of CaO, MgO and Fe2O3 is 2.0wt%; the dispersant is prepared by mixing polyvinyl pyrrolidone (molecular weight of 18000) and polysorbate 40 in a mass ratio of 5:5; the stabilizer is a polyethylene glycol polyvinyl alcohol copolymer; the thickener is prepared by mixing guar gum (molecular weight of 150000) and gelatin (molecular weight of 15000) in a mass ratio of 3:7; the defoamer is an organosilicon defoamer; and the pH value regulator is acetic acid;

[0044] The preparation method of the silica slurry is as follows:

[0045] (1) Weigh silica fume, water, dispersant, stabilizer, thickener and defoamer according to the proportion, and then put them into a stirring device;

[0046] (2) Turn on the stirring equipment and adjust the stirring speed to the specified speed (70 m / s) for 30 min. During stirring, the temperature of the silica ash slurry is controlled at 20°C;

[0047] (3) Then, the pH adjuster is slowly added into the slurry to adjust the pH value of the silica ash slurry to 3.5, and the mixture is stirred evenly to obtain the silica ash slurry for concrete.

[0048] Example 4

[0049] A silica ash mortar for concrete, the raw materials used include, by weight: 45 parts of silica ash (silica ash C), 55 parts of water, 2.0 parts of dispersant, 1.5 parts of stabilizer, 0.15 parts of thickener, and 0.15 parts of defoamer; wherein the silica ash C used is densified silica ash, the SiO2 content in the silica ash is 94wt%, and the total content of CaO, MgO and Fe2O3 is 2.0wt%; the dispersant is prepared by mixing polyvinyl pyrrolidone (molecular weight of 18000) and polysorbate 40 in a mass ratio of 5:5; the stabilizer is a polyethylene glycol polyvinyl alcohol copolymer; the thickener is prepared by mixing guar gum (molecular weight of 150000) and gelatin (molecular weight of 15000) in a mass ratio of 3:7; the defoamer is an organosilicon defoamer; and the pH value regulator is acetic acid;

[0050] The preparation method of the silicon ash slurry is as follows:

[0051] (1) Weigh silica fume, water, dispersant, stabilizer, thickener and defoamer according to the proportion, and then put them into a stirring device;

[0052] (2) Turn on the stirring equipment and adjust the stirring speed to the specified speed (70 m / s) for 30 min. During stirring, the temperature of the silica ash slurry is controlled at 20°C;

[0053] (3) Then, the pH adjuster is slowly added into the slurry to adjust the pH value of the silica ash slurry to 3.5, and the mixture is stirred evenly to obtain the silica ash slurry for concrete.

[0054] Comparative Example 1

[0055] A silica ash mortar for concrete, the raw materials used include, by weight: 40 parts of silica ash, 60 parts of water, 1.0 parts of dispersant, 0.8 parts of stabilizer, 0.15 parts of thickener, and 0.1 parts of defoamer; wherein the silica ash D used is densified silica ash, the SiO2 content in the silica ash is 90wt%, and the total content of CaO, MgO and Fe2O3 is 4.5wt%; the dispersant is prepared by mixing polysorbate 40 and dodecyl glucoside in a mass ratio of 4:6; the stabilizer is polyethylene glycol polyvinyl alcohol; the thickener is guar gum (molecular weight is 150000); the defoamer is an organosilicon defoamer;

[0056] The preparation method of the silica slurry is as follows:

[0057] (1) Weigh silica fume, water, dispersant, stabilizer, thickener and defoamer according to the proportion, and then put them into a stirring device;

[0058] (2) Turn on the mixing equipment and adjust the stirring speed to a specified speed (60 m / s) for 30 minutes. During stirring, the temperature of the silica ash slurry should be controlled at 25° C.; thus, the silica ash slurry for concrete is obtained.

[0059] Comparative Example 2

[0060] A silica ash mortar for concrete, the raw materials used include, by weight: 50 parts of silica ash, 50 parts of water, 2.5 parts of dispersant, 1.5 parts of stabilizer, 0.15 parts of thickener, and 0.15 parts of defoamer; wherein the silica ash B used is densified silica ash, the SiO2 content in the silica ash is 92wt%, and the total content of CaO, MgO and Fe2O3 is 1.5wt%; the dispersant is lauryl alcohol polyoxyethylene ether; the stabilizer is polyethylene glycol polyvinyl alcohol copolymer; the thickener is obtained by mixing guar gum (molecular weight of 150000) and gelatin (molecular weight of 15000) in a mass ratio of 6:4; the defoamer is an organosilicon defoamer; and the pH value regulator is obtained by mixing formic acid and acetic acid in a mass ratio of 3:7;

[0061] The preparation method of the silica slurry is as follows:

[0062] (1) Weigh silica fume, water, dispersant, stabilizer, thickener and defoamer according to the proportion, and then put them into a stirring device;

[0063] (2) Turn on the stirring equipment and adjust the stirring speed to the specified speed (80 m / s) for 30 min. During stirring, the temperature of the silica ash slurry is controlled to be 22° C.;

[0064] (3) Then, the pH regulator is slowly added into the slurry to adjust the pH value of the silica ash slurry to 3, and the slurry is stirred evenly to obtain the silica ash slurry for concrete.

[0065] Comparative Example 3

[0066] A silica ash mortar for concrete, the raw materials used include, by weight: 50 parts of silica ash, 50 parts of water, 2.5 parts of dispersant, 1.5 parts of stabilizer, 0.15 parts of thickener, and 0.15 parts of defoamer; wherein the silica ash B used is densified silica ash, the SiO2 content in the silica ash is 92wt%, and the total content of CaO, MgO and Fe2O3 is 1.5wt%; the dispersant is a mixture of sodium hexametaphosphate and dodecyl glucoside in a mass ratio of 4:6; the stabilizer is polyethylene glycol polyvinyl alcohol; the thickener is a mixture of guar gum and gelatin in a mass ratio of 6:4; the defoamer is an organosilicon defoamer; and the pH value regulator is a mixture of formic acid and acetic acid in a mass ratio of 3:7;

[0067] The preparation method of the silica slurry is as follows:

[0068] (1) Weigh silica fume, water, dispersant, stabilizer, thickener and defoamer according to the proportion, and then put them into a stirring device;

[0069] (2) Turn on the stirring equipment and adjust the stirring speed to the specified speed (80 m / s) for 30 min. During stirring, the temperature of the silica ash slurry is controlled to be 22° C.;

[0070] (3) Then, the pH regulator is slowly added into the slurry to adjust the pH value of the silica ash slurry to 3, and the slurry is stirred evenly to obtain the silica ash slurry for concrete.

[0071] Comparative Example 4

[0072] A silica ash mortar for concrete, the raw materials used include, by weight: 45 parts of silica ash, 55 parts of water, 2.0 parts of dispersant, 1.5 parts of stabilizer, 0.15 parts of thickener, and 0.15 parts of defoamer; wherein the silica ash C used is densified silica ash, the SiO2 content in the silica ash is 94wt%, and the total content of CaO, MgO and Fe2O3 is 2.0wt%; the dispersant is prepared by mixing polyvinyl pyrrolidone (molecular weight of 18000) and polysorbate 40 in a mass ratio of 5:5; the stabilizer is polyethylene glycol polyvinyl alcohol; the thickener is obtained by mixing guar gum (molecular weight of 150000) and gelatin (molecular weight of 15000) in a mass ratio of 3:7; the defoamer is an organic silicon defoamer;

[0073] The preparation method of the silica slurry is as follows:

[0074] (1) Weigh silica fume, water, dispersant, stabilizer, thickener and defoamer according to the mass ratio and put them into the mixing equipment;

[0075] (2) Turn on the stirring equipment and adjust the stirring speed to the specified speed and stir for 30 minutes to obtain the silica ash slurry. During stirring, the temperature of the silica ash slurry is controlled to be 20°C.

[0076] Comparative Example 5

[0077] A silica ash mortar for concrete, the raw materials used include, by weight: 45 parts of silica ash, 55 parts of water, 2.0 parts of dispersant, 1.5 parts of stabilizer, 0.15 parts of thickener, and 0.15 parts of defoamer; wherein the silica ash C used is densified silica ash, the SiO2 content in the silica ash is 94wt%, and the total content of CaO, MgO and Fe2O3 is 2.0wt%; the dispersant is a mixture of polyvinyl pyrrolidone (molecular weight of 18000) and polysorbate 40 in a mass ratio of 5:5; the stabilizer is a polyethylene glycol polyvinyl alcohol copolymer; the thickener is a mixture of guar gum (molecular weight of 150000) and gelatin (molecular weight of 15000) in a mass ratio of 3:7; the defoamer is an organosilicon defoamer; and the pH value regulator is acetic acid;

[0078] The preparation method of the silica slurry is as follows:

[0079] (1) Weigh silica fume, water, dispersant, stabilizer, thickener and defoamer according to the proportion, and then put them into a stirring device;

[0080] (2) Turn on the stirring equipment and adjust the stirring speed to the specified speed (70 m / s) for 30 min. During stirring, the temperature of the silica ash slurry is controlled at 40°C;

[0081] (3) Then, the pH adjuster is slowly added into the slurry to adjust the pH value of the silica ash slurry to 3.5, and the mixture is stirred evenly to obtain the silica ash slurry for concrete.

[0082] Comparative Example 6

[0083] A silica ash mortar for concrete, the raw materials used include, by weight: 45 parts of silica ash (silica ash C), 55 parts of water, 2.0 parts of dispersant, 1.5 parts of stabilizer, 0.15 parts of thickener, and 0.15 parts of defoamer; wherein the silica ash C used is densified silica ash, the SiO2 content in the silica ash is 94wt%, and the total content of CaO, MgO and Fe2O3 is 2.0wt%; the dispersant is prepared by mixing polyvinyl pyrrolidone (molecular weight of 18000) and polysorbate 40 in a mass ratio of 5:5; the stabilizer is a polyethylene glycol polyvinyl alcohol copolymer; the thickener is prepared by mixing guar gum (molecular weight of 150000) and gelatin (molecular weight of 15000) in a mass ratio of 3:7; the defoamer is an organosilicon defoamer; and the pH value regulator is sulfuric acid;

[0084] The preparation method of the silica slurry is as follows:

[0085] (1) Weigh silica fume, water, dispersant, stabilizer, thickener and defoamer according to the proportion, and then put them into a stirring device;

[0086] (2) Turn on the stirring equipment and adjust the stirring speed to the specified speed (70 m / s) for 30 min. During stirring, the temperature of the silica ash slurry is controlled at 20°C;

[0087] (3) Then, the pH adjuster is slowly added into the slurry to adjust the pH value of the silica ash slurry to 3.5, and the mixture is stirred evenly to obtain the silica ash slurry for concrete.

[0088] Comparative Example 7

[0089] A silica ash mortar for concrete, the raw materials used include, by weight: 45 parts of silica ash (silica ash C), 55 parts of water, 2.0 parts of dispersant, 1.5 parts of stabilizer, 0.15 parts of thickener, and 0.15 parts of defoamer; wherein the silica ash C used is densified silica ash, the SiO2 content in the silica ash is 94wt%, and the total content of CaO, MgO and Fe2O3 is 2.0wt%; the dispersant is prepared by mixing polyvinyl pyrrolidone (molecular weight of 18000) and polysorbate 40 in a mass ratio of 5:5; the thickener is prepared by mixing guar gum (molecular weight of 150000) and gelatin (molecular weight of 15000) in a mass ratio of 3:7; the defoamer is an organosilicon defoamer; and the pH value regulator is acetic acid;

[0090] The preparation method of the silica slurry is as follows:

[0091] (1) Weigh silica fume, water, dispersant, stabilizer, thickener and defoamer according to the proportion, and then put them into a stirring device;

[0092] (2) Turn on the stirring equipment and adjust the stirring speed to the specified speed (70 m / s) for 30 min. During stirring, the temperature of the silica ash slurry is controlled at 20°C;

[0093] (3) Then, the pH adjuster is slowly added into the slurry to adjust the pH value of the silica ash slurry to 3.5, and the mixture is stirred evenly to obtain the silica ash slurry for concrete.

[0094] The performance of the silica ash slurry prepared in the above embodiments and comparative examples was tested, mainly including particle fineness, fluidity, uniform stability, pH value and activity index, etc. The particle fineness was tested by a laser particle size analyzer and expressed by D50; the fluidity was tested by a truncated cone mold in the cement slurry test method, the silica ash slurry was poured into the mold and then the mold was lifted to test the maximum diameter of the silica ash slurry flowing freely on the glass plane; the uniform stability was tested by measuring the silica ash slurry with a 50ml measuring cylinder and then letting it stand for 14 days to observe the height of the supernatant; the activity index was tested by referring to the activity index method in GB / T 27690 "Silica Ash for Mortar and Concrete", and the cement replacement comparison test was carried out by converting the solid content of the silica ash slurry; the performance test results of each group of silica ash slurry are shown in Table 1.

[0095] Table 1 Silica mortar performance test results

[0096]

[0097]

[0098] It can be seen from the above test results that the particle size of the silica ash particles in the silica ash slurries prepared in Examples 1 to 4 is approximately 1 / 22 of the particle size of the dense silica ash, which significantly reduces the particle size of the silica ash. At the same time, the silica ash slurry prepared by this method has good fluidity, and there is no stratification phenomenon for 14 days (the supernatant height is 0), and it has excellent uniform stability. In addition, by comparing the activity index of Examples 1 to 4 with that of silica ash A, silica ash B, and silica ash C, it can be seen that the activity index of the silica ash slurry described in the present invention can be increased by more than 15% compared with the original dense silica ash.

[0099] Comparative Example 1 uses silica ash D, whose total content of CaO, MgO and Fe2O3 is 4.5wt%, and the pH value of the slurry is not adjusted after the slurry preparation is completed, resulting in the silica ash slurry particles being coarser than those in the embodiment, and its fluidity and stability are also worse. The activity index of the prepared silica ash slurry is even lower than that of the original dense silica ash.

[0100] Comparative Example 2 uses non-ionic dispersant lauryl alcohol polyoxyethylene ether as a dispersant. The silica ash slurry particles prepared are coarser than those in Example 2, and the fluidity and stability are insufficient. In addition, the silica ash slurry also has serious stratification during long-term storage.

[0101] Comparative Example 3 uses sodium hexametaphosphate and dodecyl glucoside in a mass ratio of 4:6 as dispersants, but the fluidity and stability are insufficient.

[0102] In Comparative Example 4, the pH value was not adjusted after the pulping was completed, resulting in the coarsening of the particles in the slurry, affecting the stability and reducing the activity index to a certain extent. The reasons are similar to those in Comparative Example 1. The precipitates such as Ca(OH)2, Mg(OH)2, and Fe(OH)3 have larger particles and reduce the stability of the slurry. In addition, the active SiO2 in the silica ash further reacts and consumes with Ca(OH)2, Mg(OH)2, and Fe(OH)3, thereby reducing the activity index of the silica ash.

[0103] In Comparative Example 5, the temperature during slurry preparation is 40°C (high-speed shearing during stirring easily generates heat and causes temperature rise), the slurry surface energy is reduced, and foaming is easier, which weakens the shearing effect on the silica ash particles during stirring. Therefore, compared with Example 4, the silica ash slurry particles prepared in the same time are coarser, and the uniformity stability and activity index are reduced.

[0104] In Comparative Example 6, sulfuric acid was used as the pH regulator, and the prepared slurry particles were larger than those of the present invention, and the fluidity, stability and activity were all deteriorated.

[0105] In Comparative Example 7, polyethylene glycol polyvinyl alcohol copolymer was not added as a stabilizer, and the prepared slurry was very easy to precipitate and had very poor stability, which was not conducive to quality control during storage and use of silica ash slurry.

[0106] The above embodiments are only examples for clear explanation, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, so the obvious changes or modifications derived are still within the protection scope of the invention.

Claims

1. A silicon mortar for concrete, It is characterized in that The raw materials and their weight proportions include: 30-50 parts of silica ash, 50-70 parts of water, 0.6-5 parts of dispersant, 0.6-2.5 parts of stabilizer, 0.05-0.2 of thickener, 0.1-0.5 parts of defoamer, and pH regulator to adjust the pH value of silica ash slurry to 2-4.

2. The silica mortar for concrete according to claim 1, It is characterized in that The silica fume is densified silica fume with a bulk density of 650-700 kg / m 3 , SiO in silica ash 2 The content is not less than 90wt%, CaO, MgO and Fe 2 O 3 The total content is 2.5 wt% or less.

3. The silica mortar for concrete according to claim 1, It is characterized in that The dispersant is two or more of polyvinyl pyrrolidone, polysorbate 40, dodecyl glucoside and arachidonic glucoside.

4. The silica mortar for concrete according to claim 1, It is characterized in that The stabilizer is a polyethylene glycol polyvinyl alcohol graft copolymer with a molecular weight of 27,000 to 28,500.

5. The silica mortar for concrete according to claim 1, It is characterized in that The thickener is one or more of guar gum and gelatin.

6. The silica mortar for concrete according to claim 1, It is characterized in that The defoamer is an organosilicon defoamer.

7. The silica mortar for concrete according to claim 1, It is characterized in that The pH adjuster is one or more of formic acid and acetic acid.

8. The method for preparing the silica mortar for concrete according to any one of claims 1 to 7, It is characterized in that The steps include: (1) Weigh silica fume, water, dispersant, stabilizer, thickener and defoamer according to the proportion and put them into the mixing equipment; (2) stirring at room temperature; (3) Add a pH adjuster to the obtained slurry to adjust the pH value of the obtained silica ash slurry to 2-4.

9. The silica mortar for concrete according to claim 1, It is characterized in that The stirring treatment time is 20 to 30 minutes.

10. The silica mortar for concrete according to claim 1, It is characterized in that The room temperature condition in step (2) is 20-30°C.

Citation Information

Cited By

  • Composite viscosity-reducing early-strength slurry for UHPC as well as preparation method and application of composite viscosity-reducing early-strength slurry

    CN121609530A

  • Anti-coagulation high-activity silicon mortar and preparation method thereof

    CN122520390A

  • Anti-agglomerating high-activity silica mortar and method for its preparation

    CN122520390B