A low-shedding, highly weather-resistant, integrally molded porous moisture absorbent and its preparation method

The one-piece molded porous absorbent body solves the problems of powder clogging, low absorbency, and chlorine corrosion in absorbent components, achieving a highly efficient and safe porous absorbent effect, and is suitable for various closed cavity structures.

CN123102297APending Publication Date: 2026-11-17深圳市兴威格科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611324765.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing moisture-absorbing components suffer from problems such as high risk of powder clogging, low moisture absorption efficiency, chlorine corrosion risk, and poor shape adaptability, making it difficult to meet the high-efficiency dehumidification requirements of sealed cavities.

Method used

A continuous porous framework is formed by integral molding and curing of 4A molecular sieve and o-cresol modified bisphenol F epoxy resin. Combined with chlorine-free potassium carbonate pore-forming agent and silane coupling agent, an integrally molded porous hygroscopic body is prepared, achieving no powder shedding at the end face, multi-level pore structure and high-strength framework.

Benefits of technology

It significantly reduces powder shedding, improves moisture absorption efficiency, avoids chlorine corrosion, enhances structural strength and morphological adaptability, is suitable for different cavity structures, reduces manufacturing costs, and increases air permeability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102297A_ABST
    Figure CN123102297A_ABST
Patent Text Reader

Abstract

This application relates to a low-shedding, high-weather-resistant, integrally molded porous absorbent and its preparation method. The porous absorbent is formed by integrally molding and curing molecular sieve functional powder with epoxy resin to form a continuous porous framework. Pure potassium carbonate is used as a soluble pore-forming agent to construct macroporous channels, which are then washed and eluted with water to form through-channels. The porous absorbent is an integrally molded, seal-free structure, with its two opposite end faces being exposed porous end faces. The molecular sieve powder is firmly locked in place by an epoxy resin cross-linking network, achieving no powder shedding from the end faces. This invention also discloses the preparation method of this porous absorbent, including five major steps: ingredient mixing, warm pressing, stepped temperature curing, elution and pore-forming, gradient drying, and finished product testing. This invention, by coating molecular sieve powder with an epoxy cross-linking network, combined with a pure potassium carbonate chlorine-free pore-forming system and a seal-free integral molding process, can achieve zero powder shedding, low flow resistance, and chlorine-free dehumidification performance, with high structural strength and good weather resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of porous adsorption materials and closed cavity dehumidification technology, and in particular to a low-shedding, high-weather-resistant integrally molded porous absorbent and its preparation method. Background Technology

[0002] With the rapid development of new energy vehicles, energy storage power stations, and outdoor communication equipment, the operating environment of various enclosed electrical cavities is becoming increasingly complex. Under long-term operation, the risk of condensation caused by temperature changes and fluctuations in external humidity poses a direct threat to the electrical insulation performance and lifespan of core components. As a key component of the enclosed cavity protection system, moisture-proofing and dehumidification, the structural stability, moisture absorption efficiency, and environmental adaptability of its moisture-absorbing components directly affect the operational safety and service life of the equipment.

[0003] In existing technologies, sealed cavities such as battery pack explosion-proof valves and energy storage cabinets typically use bagged molecular sieve particles, absorbent cotton, or non-woven fabric wrapped with desiccant for dehumidification. The absorbent material is filled in the breathing channel in the form of loose particles or fibers, relying on the gaps between particles or the pores of fibers to achieve gas flow and moisture adsorption. Some solutions directly fill the absorbent material in bulk inside the valve cavity without an independent rigid support structure, relying on the cavity wall to limit the particles.

[0004] Existing technical solutions still have several shortcomings in practical applications: First, there is a high risk of dust clogging the membrane. Bagged granules are prone to generating dust under vehicle vibration or airflow, which can clog the breathable membrane or contaminate internal precision components. Furthermore, the lack of sealing at the granule ends allows some airflow to short-circuit through the gaps between granules, resulting in low dehumidification efficiency. Second, the moisture absorption efficiency is low. Uneven flow resistance in the gaps formed by granule accumulation makes it easy for airflow to short-circuit, preventing a large number of molecular sieve particles from effectively contacting water vapor, leading to low utilization of the effective adsorption area. Third, there is a risk of chlorine corrosion. Some pore-forming processes use chlorine-containing pore-forming agents such as sodium chloride, which can corrode the battery cell tabs and metal connectors after chloride ion precipitation, failing to meet low-chlorine environmental protection requirements. Fourth, the adaptability to different shapes is poor. Existing moisture-absorbing components are mostly fixed in shape, making it difficult to adapt to different cavity structures, resulting in low installation space utilization and numerous separate parts with poor assembly consistency. Therefore, developing an integrated moisture-absorbing component that is dust-free, has low flow resistance, is free of chlorine corrosion, and can be flexibly customized in shape has become an urgent technical problem to be solved in this field. Summary of the Invention

[0005] This application provides a low-shedding, high-weather-resistant, integrally molded porous moisture absorbent and its preparation method, in order to solve the existing technical problems of high risk of powder shedding and film blockage in moisture absorbent components, low moisture absorption efficiency, chlorine corrosion hazards, and poor morphological adaptability.

[0006] In the first aspect, this application provides a low-shedding, high-weather-resistant, integrally molded porous moisture absorbent, characterized in that the moisture absorbent is a rigid porous integral structure, which is formed by integral molding and curing of 4A molecular sieve functional powder and o-cresol formaldehyde modified bisphenol F type epoxy resin binder to form a continuous porous skeleton, and the interior forms uniform and interconnected multi-level micron-level breathable pores. The porous absorbent is a one-piece, unsealed structure with two exposed porous end faces. Molecular sieve powder is encapsulated and fixed by an epoxy resin cross-linking network, preventing powder shedding from the end faces. Experimental results show that even without end face coating, the amount of powder shedding from the skeleton under high-pressure air blowing is still less than 0.01 mg.

[0007] Furthermore, the raw material composition of the porous framework is as follows: 70 to 80 parts of low-chlorine ultrafine 4A molecular sieve, 18 to 25 parts of o-cresol formaldehyde modified bisphenol F epoxy resin, 20 to 35 parts of potassium carbonate pore-forming agent, and 1 to 2 parts of silane coupling agent; the residual chloride ion content of the system is <10ppm.

[0008] Furthermore, the porous absorbent has a hollow tubular structure with an outer diameter of 6 to 10 mm, an inner diameter of 3 to 5 mm, an axial height of 7 to 20 mm, and a concentricity of inner and outer circles ≤ 0.05 mm.

[0009] Furthermore, the potassium carbonate pore-forming agent adopts a two-stage particle size distribution of 50μm and 150μm, with a mass ratio of 4:6; after washing and elution with water, it forms a continuous and interconnected macroporous channel; the pore-forming agent system is free of PVA polyvinyl alcohol microspheres.

[0010] Furthermore, the o-cresol-modified bisphenol F epoxy resin is combined with a latent curing agent; the silane coupling agent is KH560 type, used to improve the interfacial bonding force between the molecular sieve and the epoxy group.

[0011] Secondly, this application provides a method for preparing a porous hygroscopic body, comprising the following steps: Step 1: Ingredient Mixing: Weigh the low-chlorine ultrafine 4A molecular sieve powder, o-cresol formaldehyde modified bisphenol F epoxy resin, potassium carbonate pore-forming agent, and silane coupling agent according to the mass ratio; first activate the molecular sieve at a high temperature of 350 to 400℃ to remove the water of crystallization, cool it to room temperature under nitrogen protection, premix it evenly with potassium carbonate, then add epoxy resin, curing agent, and silane coupling agent, put it into a vacuum mixer, shear and mix at high speed, and then degas under vacuum to make a paste-like premix without bubbles and agglomeration; Step 2: Warm pressing: The premixed material is quantitatively filled into a precision mold with a guide mandrel. The mold is preheated to 60 to 80°C. A segmented pressurization and degassing process is adopted. First, the pre-pressurization is carried out twice at 5MPa, and then the pressure is increased to 8 to 10MPa and held for 30 to 60 seconds to form a green body with uniform wall thickness. Step 3: Stepped temperature curing: Place the green body in a programmed temperature oven and use a three-stage stepped curing process: first, heat to 80℃ at 1℃ / min and hold for 1.5 to 2.5 hours to complete the initial setting; then heat to 120℃ and hold for 2.5 to 3.5 hours to complete the deep cross-linking; finally, heat to 140℃ and hold for 0.5 to 1 hour for post-curing. After slow cooling in the oven, a rigid skeleton is formed. Step 4: Elution and Gradient Drying: The cured green body is placed in deionized water at 60 to 80°C, and the soluble pore-forming agent is removed using a negative pressure immersion circulation elution process. The vacuum degree is -0.08 to -0.09 MPa, and the water is changed every 30 minutes. The conductivity of the immersion solution is monitored in real time until the conductivity is <5 μS / cm, forming a continuous and interconnected multi-level porous structure. After elution, gradient heating drying is used to remove residual moisture from the interior. Step 5: Finished product inspection and post-processing: The finished product is inspected for appearance, size, porosity, air resistance, high-pressure air blowing dust amount, and chloride ion residue. After high-pressure pulse dust removal, it is vacuum-packed for moisture protection and stored in the warehouse.

[0012] Furthermore, in step 1, the molecular sieve activation conditions are: oven heating at 380℃ for 2 hours, with nitrogen protection throughout the cooling process; the double planetary vacuum stirring mixing time is 10 to 15 minutes, followed by vacuum degassing for more than 20 minutes; the material temperature is controlled to ≤40℃ by cooling water during the mixing process; and the potassium carbonate pore-forming agent needs to be ground through a 200-mesh sieve before mixing.

[0013] Furthermore, in step 2, a Teflon non-stick coating is applied to the inner wall of the mold, and the surface of the mandrel is mirror-polished; the segmented pressurization process effectively eliminates air holes inside the green blank and improves the uniformity of the skeleton density.

[0014] Furthermore, the gradient drying process in step 4 is as follows: first, dry at 60℃ for 2 hours, then raise the temperature to 100℃ for 2 hours, and finally raise the temperature to 120℃ for 1 hour to slowly remove moisture and avoid stress cracking of the pores; in high-requirement scenarios, TOC detection is added to assist in determining the elution endpoint, requiring TOC≤5mg / L.

[0015] The technical solutions provided in this application have the following advantages compared with the prior art: 1. Low powder shedding and inherent safety: The epoxy resin cross-linking network completely encapsulates and fixes the 4A molecular sieve powder. Combined with the optimized epoxy ratio and molding pressure, the epoxy resin cross-linking network fully encapsulates the molecular sieve powder, achieving an extremely low powder shedding rate even without end-face sealing. Random vibration tests show that the amount of powder shedding is less than 0.01mg, significantly reducing the risk of clogging of the breathable membrane and contamination of precision components.

[0016] 2. Chlorine-free system, eliminating corrosion: Pure potassium carbonate chlorine-free pore-forming agent is used, and no chlorine element is introduced throughout the process. The final chloride ion residue in the system is <10ppm, which meets the low-chlorine environmental protection requirements of power batteries, energy storage systems and industrial equipment.

[0017] 3. No-sealing process, low cost and no risk of clogging: This application innovatively eliminates the end-face adhesive sealing process, saving multiple processes such as plasma activation, screen printing, and high-temperature curing, significantly simplifying the production process, reducing manufacturing costs, and completely avoiding the risk of adhesive overflow clogging the central hole caused by the adhesive coating process; at the same time, eliminating the sealing adhesive layer makes the airflow channel smoother, and the air permeability is increased by about 10% to 15% compared with the sample with the sealing layer.

[0018] 4. Multi-level channels, high moisture absorption efficiency: The hierarchical mass transfer network of macropores and mesopores allows gas to diffuse rapidly while water vapor comes into full contact with the molecular sieve, significantly improving the utilization rate of the effective moisture absorption area and the volumetric moisture absorption density is significantly higher than that of bagged 4A molecular sieve particles of the same volume; the channel distribution is uniform and controllable, the flow resistance is stable, and it does not affect the normal exhaust and throughput requirements of the equipment.

[0019] 5. High structural strength and full-cycle reliability: The integrated rigid frame is highly resistant to vibration, pressure impact, and high and low temperature cycles. It will not deform or break after long-term use, and its structural life is significantly better than that of traditional bagged structures. It is suitable for automotive-grade and harsh outdoor working conditions.

[0020] 6. Wide range of applications and strong modular adaptability: This moisture absorber can be adapted to various specifications of power battery packs, energy storage battery boxes, communication base station outdoor cabinets, special power supplies and moisture protection for precision electronic equipment, etc. It can be assembled as a standardized module without major modifications to the system. Attached Figure Description

[0021] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.

[0022] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0023] One or more embodiments are illustrated by way of example with reference numerals in the accompanying drawings. These illustrations do not constitute a limitation on the embodiments. Elements with the same reference numerals in the drawings are denoted as similar elements. Unless otherwise stated, the figures in the drawings are not to be limited by scale.

[0024] Figure 1This is a schematic diagram of a porous absorbent material with low shedding and high weather resistance, provided in an embodiment of this application.

[0025] Figure 2 This is a top view of a low-shedding, highly weather-resistant, integrally molded porous absorbent provided in an embodiment of this application.

[0026] Figure 3 This is a cross-sectional schematic diagram of a low-shedding, highly weather-resistant, integrally molded porous absorbent body provided in an embodiment of this application.

[0027] Figure 4 This is a schematic flowchart of a method for preparing a porous absorbent provided in an embodiment of this application.

[0028] Explanation of reference numerals in the attached figures: 1. Hygroscopic body. Detailed Implementation

[0029] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0030] The following disclosure provides numerous different embodiments or examples for implementing various structures of this application. To simplify the disclosure, specific examples of components and arrangements are described below. These are merely examples and are not intended to limit the scope of this application. Furthermore, reference numerals and / or letters may be repeated in different examples. Such repetition is for simplification and clarity and does not in itself indicate a relationship between the various embodiments and / or arrangements discussed.

[0031] For ease of description, spatial relative terms may be used in the text to describe the relative position or movement of one element or feature relative to another element or feature, as shown in the figure. These relative terms include, for example, "inside," "outside," "middle," "outer," "below," "below," "above," "front," "back," etc. Such spatial relative terms are intended to include different orientations of the device in use or operation, other than those depicted in the figure. For example, if the device in the figure undergoes a positional flip, orientation change, or change of motion, these directional indications will change accordingly. For instance, an element described as "below other elements or features" or "below other elements or features" will subsequently be oriented "above other elements or features" or "above other elements or features." Therefore, the example term "below" can include both upper and lower orientations. The device may be otherwise oriented (rotated 90 degrees or in other directions), and the spatial relative descriptors used in the text will be interpreted accordingly.

[0032] To address the existing technical problems of high risk of powder clogging, low moisture absorption efficiency, chlorine corrosion hazards, and poor morphological adaptability in existing moisture-absorbing components, this application provides a low-shedding, high-weather-resistant, integrally molded porous moisture absorber and its preparation method. This method achieves synergistic improvements through an integrally molded rigid porous framework structure, a chlorine-free composite pore-forming system, an epoxy-sealed end face structure, and the entire manufacturing process. It achieves the technical effects of low powder shedding, no chlorine residue in the system, low flow resistance and efficient dehumidification through multi-level pores, high structural strength and good weather resistance, and flexible morphological customization. This provides a low-shedding, high-weather-resistant, integrally molded porous moisture absorber and its preparation method.

[0033] Please see Figures 1 to 4 In the first aspect, this application provides a low-shedding, high-weather-resistant, integrally molded porous absorbent 1, which is a rigid porous integral structure. It is formed by integral molding and curing of 4A molecular sieve functional powder and o-cresol formaldehyde modified bisphenol F type epoxy resin binder to form a continuous porous skeleton, and the interior forms a uniform and interconnected multi-level micron-level breathable pores. The porous absorbent 1 is an integrally molded, unsealed structure with two exposed porous end faces. The molecular sieve powder is wrapped and fixed by an epoxy resin cross-linking network, so that no powder falls off the end faces.

[0034] In the embodiments provided in this application, the absorbent 1 includes a continuous porous framework and an integrally formed exposed porous end face. During operation, it is embedded as an independent functional component within the breathing channel of a sealed cavity. Gas flows axially through the central channel of the end face, fully contacting the internal multi-level pores to complete water vapor adsorption. The continuous porous framework is integrally molded and cured from 4A molecular sieve functional powder and o-cresyl formaldehyde modified bisphenol F type epoxy resin binder, forming a rigid porous integral structure. The epoxy cross-linking network encapsulates and fixes each molecular sieve powder particle, preventing the powder from detaching from the framework and eliminating moisture at the material matrix level. In some optional embodiments, the porous framework is composed of: 70 to 80 parts of low-chlorine ultrafine 4A molecular sieve, 18 to 25 parts of o-cresphenol-modified bisphenol F epoxy resin, 20 to 35 parts of potassium carbonate pore-forming agent, and 1 to 2 parts of silane coupling agent; the residual chloride ion content of the system is <10 ppm. The low-chlorine ultrafine 4A molecular sieve provides the main body for moisture absorption; if the molecular sieve content is too low, the moisture absorption capacity is insufficient; if it is too high, the resin binder phase is insufficient and the framework strength decreases. The o-cresphenol-modified bisphenol F epoxy resin provides the binding framework and weather-resistant matrix, firmly encapsulating the molecular sieve powder and forming a continuous rigid network. In some optional embodiments, the porous absorbent 1 is a hollow tubular structure with an outer diameter of 6 to 10 mm, an inner diameter of 3 to 5 mm, an axial height of 7 to 20 mm, and a concentricity of inner and outer circles ≤ 0.05 mm. The inner diameter of 3 to 5 mm ensures sufficient cross-sectional area for the central airflow channel, while the axial height of 7 to 20 mm can be flexibly selected according to the absorbency capacity requirements of different scenarios. The concentricity of inner and outer circles ≤ 0.05 mm ensures uniform wall thickness, avoiding insufficient strength due to excessively thin walls or uneven flow resistance due to excessively thick walls. The hollow tubular structure allows gas to pass through the central inner hole, with the inner wall of the channel fully contacting the airflow, resulting in a large effective absorbency area. Simultaneously, the outer wall fits snugly against the mounting cavity, ensuring stable positioning.

[0035] In some optional embodiments, the potassium carbonate pore-forming agent employs a two-stage particle size distribution of 50 μm and 150 μm in a mass ratio of 4:6; after washing and elution with water, it forms continuous and interconnected macroporous channels; the pore-forming agent system is free of PVA polyvinyl alcohol microspheres. During operation, the potassium carbonate pore-forming agent leaves macroporous channels within the framework after washing and elution with water. In some optional embodiments, the o-crestyral modified bisphenol F epoxy resin is combined with a latent curing agent; the silane coupling agent is KH560, used to improve the interfacial bonding force between the molecular sieve and the epoxy matrix. The o-crestyral modified bisphenol F epoxy resin combined with the latent curing agent forms a rigid framework with high crosslinking density and good temperature and moisture resistance after curing. The o-crestyral structure improves the resin's heat resistance and mechanical strength, while the bisphenol F structure provides good flowability and wettability, allowing the resin to fully encapsulate the molecular sieve powder. The latent curing agent does not react at room temperature, ensuring sufficient pot life for the premix. It cures gradually upon heating, achieving uniform crosslinking through a stepped heating process. One end of the KH560 silane coupling agent reacts with the hydroxyl groups on the surface of the molecular sieve powder, and the other end reacts with the epoxy resin matrix, forming a chemical bond between the inorganic powder and the organic resin. This significantly improves the interfacial bonding force, preventing interfacial delamination that can cause microcracks and powder detachment channels, and enhancing the overall strength and weather resistance of the framework.

[0036] Please see Figure 4 Secondly, this application provides a method for preparing a porous absorbent 1, comprising the following steps: Step 1: Ingredient Mixing: Weigh the low-chlorine ultrafine 4A molecular sieve powder, o-cresol formaldehyde modified bisphenol F epoxy resin, potassium carbonate pore-forming agent, and silane coupling agent according to the mass ratio; first activate the molecular sieve at a high temperature of 350 to 400℃ to remove the water of crystallization, cool it to room temperature under nitrogen protection, premix it evenly with potassium carbonate, then add epoxy resin, curing agent, and silane coupling agent, put it into a vacuum mixer, shear and mix at high speed, and then degas under vacuum to make a paste-like premix without bubbles and agglomeration; Step 2: Warm pressing: The premixed material is quantitatively filled into a precision mold with a guide mandrel. The mold is preheated to 60 to 80°C. A segmented pressurization and degassing process is adopted. First, the pre-pressurization is carried out twice at 5MPa, and then the pressure is increased to 8 to 10MPa and held for 30 to 60 seconds to form a green body with uniform wall thickness. Step 3: Stepped temperature curing: Place the green body in a programmed temperature oven and use a three-stage stepped curing process: first, heat to 80℃ at 1℃ / min and hold for 1.5 to 2.5 hours to complete the initial setting; then heat to 120℃ and hold for 2.5 to 3.5 hours to complete the deep cross-linking; finally, heat to 140℃ and hold for 0.5 to 1 hour for post-curing. After slow cooling in the oven, a rigid skeleton is formed. Step 4: Elution and Gradient Drying: The cured green body is placed in deionized water at 60 to 80°C, and the soluble pore-forming agent is removed using a negative pressure immersion circulation elution process. The vacuum degree is -0.08 to -0.09 MPa, and the water is changed every 30 minutes. The conductivity of the immersion solution is monitored in real time until the conductivity is <5 μS / cm, forming a continuous and interconnected multi-level porous structure. After elution, gradient heating drying is used to remove residual moisture from the interior. Step 5: Finished product inspection and post-processing: The finished product is inspected for appearance, size, porosity, air resistance, high-pressure air blowing dust amount, and chloride ion residue. After high-pressure pulse dust removal, it is vacuum-packed for moisture protection and stored in the warehouse.

[0037] According to the embodiments provided in this application, in step 1, during the mixing of ingredients, the molecular sieve is first activated at a high temperature of 350 to 400°C to remove crystal water and adsorbed water, ensuring the hygroscopic capacity of the molecular sieve; nitrogen protection cooling prevents the activated molecular sieve from re-adsorbing moisture from the air; potassium carbonate is premixed with the molecular sieve to ensure uniform dispersion of the pore-forming agent, and the potassium carbonate pore-forming agent is ground through a 200-mesh sieve before mixing to ensure uniform particle size; double planetary vacuum stirring combined with vacuum degassing produces a paste-like premix without bubbles or agglomerations, ensuring the uniformity of the subsequent molded skeleton. In step 2, during warm pressing, the mold is preheated to 60 to 80°C to reduce the temperature of the premix. In some optional embodiments, the molecular sieve activation conditions in step 1 are: oven heating at 380°C for 2 hours, with nitrogen protection throughout the cooling process; the mixing time of the double planetary vacuum stirring is 10 to 15 minutes, followed by vacuum degassing for more than 20 minutes after mixing; the material temperature is controlled to ≤40°C by cooling water during the mixing process; and the potassium carbonate pore-forming agent needs to be ground through a 200-mesh sieve before mixing.

[0038] In some optional embodiments, in step 2, a Teflon non-stick coating is applied to the inner wall of the mold, and the mandrel surface is mirror-polished. The segmented pressurization process effectively eliminates air pores inside the green blank, improving the uniformity of the skeleton density. The Teflon non-stick coating on the inner wall of the mold ensures smooth demolding of the green blank, preventing end face or outer wall defects due to adhesion; the mirror polishing of the mandrel surface ensures a smooth inner wall of the central hole, reducing airflow resistance; the segmented pressurization process first uses low-pressure pre-pressurization to expel air entrained in the premix, and then high-pressure holding to ensure uniform green blank density, avoiding uneven skeleton strength caused by local porosity.

[0039] In some optional embodiments, the gradient drying process in step 4 is as follows: first, drying at 60°C for 2 hours, then heating to 100°C for 2 hours, and finally heating to 120°C for 1 hour, slowly removing moisture to avoid stress cracking of the pores; in high-requirement scenarios, TOC detection is added to assist in determining the elution endpoint, requiring TOC ≤ 5 mg / L. Gradient drying first removes free water from the surface and macropores by drying at 60°C for 2 hours, then heats to 100°C for 2 hours to remove adsorbed water from the mesopores, and finally heats to 120°C for 1 hour to deeply remove bound water. The three-stage slow heating avoids the rapid vaporization of moisture in the pores, which can generate stress and cause pore wall cracking; in high-requirement scenarios, TOC detection is added, and when the TOC of the soaking solution is ≤ 5 mg / L, it confirms that the residual organic pore-forming agent is extremely low, ensuring high purity and low precipitation risk of the product.

[0040] The present application will be described below with reference to specific embodiments: Example 1: Standard porous moisture absorbent 1 This embodiment is a standard porous moisture absorber 1 adapted to explosion-proof valves and small and medium-sized energy storage dehumidification modules.

[0041] Structure and Formulation Parameters: The porous absorbent 1 has a hollow tubular structure with an outer diameter of 8 mm, an inner diameter of 4 mm, an axial height of 7.2 mm, and a concentricity of inner and outer circles ≤0.05 mm. The overall porosity is 45%. Raw materials, by weight: 78 parts D50 3μm low-chlorine 4A molecular sieve, 20 parts o-cresphenol-modified bisphenol F epoxy resin (including latent curing agent), 28 parts potassium carbonate pore-forming agent (all potassium carbonate, no PVA), and 2 parts KH560 silane coupling agent. The potassium carbonate uses a two-stage particle size distribution of 50 μm and 150 μm at a mass ratio of 4:6, and is ground through a 200-mesh sieve before mixing. Both ends of the absorbent are exposed porous surfaces without an epoxy sealing layer, and the residual chloride ion content in the finished product is <10 ppm.

[0042] Preparation process flow: Step 1: Ingredient mixing. Weigh each raw material according to the mass ratio; first, place the low-chlorine 4A molecular sieve in a 380℃ oven for 2 hours to fully remove crystal water and adsorbed water, and cool to room temperature under nitrogen protection; then, premix the molecular sieve and potassium carbonate at low speed for 5 minutes, then add o-cresol formaldehyde modified bisphenol F epoxy resin, latent curing agent, and silane coupling agent, and put them into a vacuum mixer, premix at low speed for 5 minutes, shear mix at high speed for 10 minutes, and finally degas under vacuum for 20 minutes to prepare a uniform, bubble-free paste premix; cooling water is circulated throughout the mixing process to control the temperature. Example 2: High-capacity porous absorbent 1 This embodiment is a high-capacity porous moisture absorber 1 designed for high-humidity energy storage scenarios.

[0043] Structure and Formulation Parameters: The porous absorbent 1 has a hollow tubular structure with an outer diameter of 8 mm, an inner diameter of 4 mm, an axial height of 20 mm, and a concentricity of inner and outer circles ≤0.05 mm. The overall porosity is approximately 50%. Raw materials, by weight: 78 parts D50 3μm low-chlorine 4A molecular sieve, 20 parts o-cresphenol-modified bisphenol F epoxy resin (including latent curing agent), 32 parts potassium carbonate pore-forming agent (all potassium carbonate, no PVA), and 2 parts KH560 silane coupling agent. The potassium carbonate uses a two-stage particle size distribution of 50 μm and 150 μm at a mass ratio of 4:6, and is ground through a 200-mesh sieve before mixing. Both ends of the absorbent are exposed porous surfaces without an epoxy sealing layer.

[0044] Preparation Process: Step 1: Ingredient Mixing. Weigh each raw material according to the mass ratio; first, activate the low-chlorine 4A molecular sieve in a 380℃ oven for 2 hours, then cool it to room temperature under nitrogen protection; then premix the molecular sieve and potassium carbonate at low speed for 5 minutes, then add o-cresolaldehyde modified bisphenol F epoxy resin, latent curing agent, and silane coupling agent, and put them into a vacuum mixer, premix at low speed for 5 minutes, shear mix at high speed for 10 minutes, and finally degas under vacuum for 20 minutes to make a uniform, bubble-free paste-like premix; cooling water is circulated throughout the mixing process to control the material temperature ≤40℃. Step 2: Warm Press Molding. Use a precision quantitative injection device to fill the premix into a hard alloy mold with a double guide mandrel. The mandrel diameter is 4mm, the outer diameter of the mold cavity is 8mm, and the mold cavity height corresponds to a finished product height of 20mm; preheat the mold to 70℃, and use a segmented pressurization and degassing process: first, pre-pressurize and degas twice at 5MPa, then increase the pressure... In this embodiment, the axial height is increased to 20mm, the total amount of composite pore-forming agent is adjusted to 32 parts, corresponding to a porosity of about 50%, and the overall moisture absorption capacity is increased by about 1.8 times compared with the standard version. It can maintain the anti-condensation effect for a longer period of time in high humidity environment, and is more suitable for large energy storage battery boxes and other scenarios in high humidity areas.

[0045] Example 3: High-porosity porous moisture absorbent 1 This embodiment is a high-porosity porous absorbent 1 designed for high-flow-rate, low-flow-resistance scenarios.

[0046] Structure and Formulation Parameters: The porous absorbent 1 has a hollow tubular structure with an outer diameter of 8 mm, an inner diameter of 4 mm, an axial height of 7.2 mm, and a concentricity of inner and outer circles ≤0.05 mm. The overall pore connectivity is approximately 78%. Raw materials, by weight: 78 parts D50 3μm low-chlorine 4A molecular sieve, 20 parts o-cresphenol-modified bisphenol F epoxy resin (including latent curing agent), 30 parts potassium carbonate pore-forming agent, and 2 parts KH560 silane coupling agent. The potassium carbonate uses a two-stage particle size distribution of 50 μm and 150 μm at a weight ratio of 4:6. Both ends of the absorbent are exposed porous surfaces without an epoxy sealing layer, resulting in a chloride ion residue of <10 ppm in the finished product.

[0047] Preparation Process: Step 1: Ingredient Mixing. Weigh each raw material according to the mass ratio; first, activate the low-chlorine 4A molecular sieve in a 380℃ oven for 2 hours, then cool it to room temperature under nitrogen protection; subsequently, premix the molecular sieve and potassium carbonate at low speed for 5 minutes, then add o-cresolaldehyde modified bisphenol F epoxy resin, latent curing agent, and silane coupling agent, and put them into a vacuum mixer, premix at low speed for 5 minutes, shear mix at high speed for 10 minutes, and finally degas under vacuum for 20 minutes to prepare a uniform, bubble-free paste-like premix; cooling water is circulated throughout the mixing process to control the material temperature ≤40℃. Step 2: Warm Press Molding. Use a precision quantitative injection device to fill the premix into a hard alloy mold with a double guide mandrel. The mandrel diameter is 4mm, and the outer diameter of the mold cavity is 8mm; preheat the mold to 70℃, and use a segmented pressurization and degassing process: first, pre-press and degas twice at 5MPa, then increase to 8MPa and hold for 45 seconds; This embodiment uses a higher dosage (30 parts) of potassium carbonate for pore formation. The total dosage is 30 parts. The formula is extremely simple, with zero organic residue. The pore connectivity rate is about 78%. The moisture absorption efficiency is slightly lower than the standard model, but the manufacturing cost is lower. It is suitable for general scenarios that are cost-sensitive or require high flow rate and low flow resistance.

[0048] Performance test comparison Standardized tests were conducted on the samples from the three embodiments described above. Vibration tests were performed according to GB / T 2423.10-2019 standard, and the amount of dust falling off was determined by gravimetric analysis using a 0.45μm filter membrane. The test results showed that the amount of dust falling off in all three embodiments was less than 0.01mg (below the detection limit of a precision balance), and the residual chloride ion content was less than 10ppm. Example 1 showed balanced overall performance, Example 2 had the highest moisture absorption capacity, and Example 3 had the highest porosity and lowest flow resistance, allowing for flexible selection based on different application scenarios.

[0049] Supplementary Performance Verification (Sealing-Free Structure): To verify the reliability of the "sealing-free" structure of this application, the following tests were performed on the sample prepared according to Example 1 (without an epoxy sealing layer): 1. Vibration Powder Drop Test: Following GB / T 2423.10-2019 standard, a sweep vibration was performed within the frequency range of 10Hz to 500Hz for 100 hours. After the test, the dropped powder was collected using a 0.45μm filter membrane and weighed using a precision electronic balance. The measured amount of dropped powder was less than 0.01mg, which is below the lower limit of the precision balance's detection limit. This demonstrates that the epoxy resin skeleton has sufficient encapsulation force for the 4A powder, ensuring no free powder without sealing. 2. High-Pressure Air Blow Test: Using a 0.3MPa compressed air nozzle, the two exposed end faces of the absorbent were continuously blown for 3 seconds at a distance of 50mm. No white powder particles were observed on the downstream filter paper. 3. Airflow Resistance Test: Due to the elimination of the end-face sealing layer, the airflow channel is smoother, and the air permeability of the sample under a pressure difference of 2.5 kPa is increased by approximately 10% to 15% compared to the sample with the end-face sealing layer. The above measured data fully demonstrate that this application, by using pure potassium carbonate for pore formation and combining it with an optimized epoxy ratio, not only achieves the construction of multi-level channels, but also utilizes the cross-linked network structure of the epoxy resin itself to completely lock in the molecular sieve powder. Therefore, eliminating the end-face sealing layer not only does not bring the risk of powder shedding, but also helps to improve air permeability and reduce process costs.

[0050] In the above embodiments, the descriptions of each embodiment have different focuses. For parts that are not described in detail in a certain embodiment, please refer to the relevant descriptions in other embodiments.

[0051] In the description of this application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.

[0052] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this application, "multiple" means two or more, unless otherwise explicitly specified.

[0053] In this application, unless otherwise expressly specified and limited, the terms "installation," "connection," "joining," and "fixing," etc., should be interpreted broadly. For example, they can refer to a connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.

[0054] In this application, unless otherwise expressly specified and limited, "above" or "below" the second feature can include direct contact between the first and second features, or contact between the first and second features through another feature between them. Furthermore, "above," "over," and "on top" of the second feature includes the first feature being directly above or diagonally above the second feature, or simply indicates that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature includes the first feature being directly below or diagonally below the second feature, or simply indicates that the first feature is at a lower horizontal level than the second feature.

[0055] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of this application. The illustrative expressions of the above terms in this specification should not be construed as necessarily referring to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. In addition, those skilled in the art can combine and integrate the different embodiments or examples described in this specification.

[0056] Obviously, those skilled in the art can make various modifications and variations to this application without departing from the spirit and scope of this application. Since these modifications and variations fall within the scope of the claims and their equivalents, this application also intends to include these modifications and variations.

[0057] The above description describes specific embodiments of this application, but the scope of protection of this application is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in this application, and these modifications or substitutions should all be covered within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.

Claims

1. A low-shedding, highly weather-resistant, integrally molded porous absorbent, characterized in that, The absorbent is a rigid porous integral structure, which is formed by integral molding and curing of 4A molecular sieve functional powder and o-cresol formaldehyde modified bisphenol F type epoxy resin binder to form a continuous porous skeleton, with uniform and interconnected multi-level micron-level air-permeable channels inside. The porous absorbent is a one-piece molded, unsealed structure with two exposed porous end faces. The molecular sieve powder is wrapped and fixed by an epoxy resin cross-linking network, so that no powder falls off the end faces.

2. The low-shedding, high-weather-resistant, integrally molded porous absorbent body according to claim 1, characterized in that, The porous framework is composed of the following raw materials: 70 to 80 parts of low-chlorine ultrafine 4A molecular sieve, 18 to 25 parts of o-cresol formaldehyde modified bisphenol F epoxy resin, 20 to 35 parts of potassium carbonate pore-forming agent, and 1 to 2 parts of silane coupling agent; the residual chloride ion content of the system is <10 ppm.

3. The low-shedding, high-weather-resistant, integrally molded porous absorbent body according to claim 1, characterized in that, The porous absorbent has a hollow tubular structure with an outer diameter of 6 to 10 mm, an inner diameter of 3 to 5 mm, an axial height of 7 to 20 mm, and a concentricity of inner and outer circles ≤ 0.05 mm.

4. The low-shedding, high-weather-resistant, integrally molded porous absorbent body according to claim 1, characterized in that, The potassium carbonate pore-forming agent has a two-stage particle size distribution of 50μm and 150μm, with a mass ratio of 4:6; after washing and elution with water, it forms a continuous and interconnected macroporous channel; the pore-forming agent system is free of PVA polyvinyl alcohol microspheres.

5. The low-shedding, high-weather-resistant, integrally molded porous absorbent body according to claim 1, characterized in that, The o-cresol-modified bisphenol F epoxy resin is combined with a latent curing agent; the silane coupling agent is KH560 type, used to improve the interfacial bonding force between the molecular sieve and the epoxy group.

6. A method for preparing a porous moisture absorbent, characterized in that, Includes the following steps: Step 1: Ingredient Mixing: Weigh the low-chlorine ultrafine 4A molecular sieve powder, o-cresol formaldehyde modified bisphenol F epoxy resin, potassium carbonate pore-forming agent, and silane coupling agent according to the mass ratio; first activate the molecular sieve at a high temperature of 350 to 400℃ to remove the water of crystallization, cool it to room temperature under nitrogen protection, premix it evenly with potassium carbonate, then add epoxy resin, curing agent, and silane coupling agent, put it into a vacuum mixer, shear and mix at high speed, and then degas under vacuum to make a paste-like premix without bubbles and agglomeration; Step 2: Warm pressing: The premixed material is quantitatively filled into a precision mold with a guide mandrel. The mold is preheated to 60 to 80°C. A segmented pressurization and degassing process is adopted. First, the pre-pressurization is carried out twice at 5MPa, and then the pressure is increased to 8 to 10MPa and held for 30 to 60 seconds to form a green body with uniform wall thickness. Step 3: Stepped temperature curing: Place the green body in a programmed temperature oven and use a three-stage stepped curing process: first, heat to 80℃ at 1℃ / min and hold for 1.5 to 2.5 hours to complete the initial setting; then heat to 120℃ and hold for 2.5 to 3.5 hours to complete the deep cross-linking; finally, heat to 140℃ and hold for 0.5 to 1 hour for post-curing. After slow cooling in the oven, a rigid skeleton is formed. Step 4: Elution and Gradient Drying: The cured green body is placed in deionized water at 60 to 80°C, and the soluble pore-forming agent is removed using a negative pressure immersion circulation elution process. The vacuum degree is -0.08 to -0.09 MPa, and the water is changed every 30 minutes. The conductivity of the immersion solution is monitored in real time until the conductivity is <5 μS / cm, forming a continuous and interconnected multi-level porous structure. After elution, gradient heating drying is used to remove residual moisture from the interior. Step 5: Finished product inspection and post-processing: The finished product is inspected for appearance, size, porosity, air resistance, high-pressure air blowing dust amount, and chloride ion residue. After high-pressure pulse dust removal, it is vacuum-packed for moisture protection and stored in the warehouse.

7. The method for preparing a porous moisture absorbent according to claim 6, characterized in that, In step 1, the molecular sieve activation conditions are: oven heating at 380℃ for 2 hours, with nitrogen protection throughout the cooling process; the mixing time for the double planetary vacuum stirring is 10 to 15 minutes, followed by vacuum degassing for more than 20 minutes; during the mixing process, cooling water is used to control the material temperature to ≤40℃; the potassium carbonate pore-forming agent needs to be ground through a 200-mesh sieve before mixing.

8. The method for preparing a porous moisture absorbent according to claim 6, characterized in that, In step 2, a Teflon non-stick coating is applied to the inner wall of the mold, and the surface of the mandrel is mirror-polished; the segmented pressurization process effectively eliminates air holes inside the green blank and improves the uniformity of the skeleton density.

9. The method for preparing a porous moisture absorbent according to claim 6, characterized in that, The gradient drying process in step 4 is as follows: first, dry at 60℃ for 2 hours, then raise the temperature to 100℃ for 2 hours, and finally raise the temperature to 120℃ for 1 hour to slowly remove moisture and avoid stress cracking of the pores; in high-requirement scenarios, TOC detection is added to help determine the elution endpoint, requiring TOC≤5mg / L.