Lithium-ion adsorbent materials, their preparation methods and applications
By grafting specific structures onto a polymer backbone and using a mixture of aldehyde initiators, a lithium-ion adsorbent material with high selectivity and high adsorption capacity was prepared, solving the problems of insufficient selectivity and adsorption capacity of existing materials, and making it suitable for lithium-ion extraction in liquid environments.
Patent Information
- Application Number
- CN202510638101.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing lithium-ion adsorption materials have low adsorption capacity and poor selectivity for sodium and potassium ions, making them unable to effectively separate lithium ions from monovalent salt ions in liquid environments.
A lithium-ion adsorbent material containing abundant ether bonds was prepared by using a polymer framework and a lithium-ion sieve dispersed on it, through a specific structure grafted onto the polyacrylonitrile molecular chain. The mixing method with aldehyde initiators ensured that the lithium-ion sieve was uniformly dispersed in the framework.
It significantly improves the adsorption capacity and selectivity of lithium-ion adsorbent materials for K+/Li+, making them suitable for lithium-ion extraction in liquid environments and enhancing the adsorption efficiency and selectivity of the materials.
Smart Images

Figure CN123102308A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of adsorption materials, specifically to a lithium-ion adsorption material, its preparation method, and its application. Background Technology
[0002] With the rapid development of the lithium battery industry, the demand for lithium resources from various industries is continuously increasing, and the importance of lithium production is also growing. Currently, lithium resources are mainly distributed in lithium ore and salt lake brine, but lithium ore resources are constantly decreasing and development costs are constantly increasing; in contrast, lithium water resources in salt lake brine are low-cost and abundant, but extracting lithium from lithium water resources is a challenging task.
[0003] Currently, the main methods for lithium extraction from salt lakes include adsorption, precipitation, extraction, electrodialysis, and calcination. Among these, adsorption offers advantages such as simple process, energy efficiency, and high selectivity, outperforming other methods in terms of both time and cost, and thus has broad application prospects. Since salt lake brine often suffers from low lithium content, the core of lithium extraction using adsorption is the preparation of highly selective adsorbents. Highly selective lithium adsorbents mainly include ion sieve adsorbents and amorphous hydroxide adsorbents. However, because these adsorbents are synthesized in powder form, they cannot be directly applied to conventional equipment such as fixed-bed adsorption-desorption systems for lithium extraction. Currently, lithium adsorbents are also granulated to obtain granular lithium adsorbent materials. Common granulation methods include: (1) using inorganic binders such as alumina and silica gel for granulation. This method is simple to prepare granular adsorbents, but the stability is poor, and it often needs to be used in conjunction with polymer granulation methods; (2) using natural polymer materials such as chitosan and sodium alginate for granulation. However, the products prepared by this method have poor long-term performance stability; (3) using organic polymer materials such as PU, PAM, and PVC as binders for granulation. However, the prepared granular adsorbents have poor hydrophilicity and are prone to encapsulation of powder adsorbents, resulting in a significant decrease in adsorption capacity. Based on the above background, it is proposed to develop a highly efficient hydrophilic lithium adsorbent material.
[0004] Furthermore, in the extraction of lithium from actual salt lakes or produced water from oil and gas fields, the concentration of monovalent salt ions is extremely high, posing a challenge to the adsorption process, as lithium ions and monovalent salt ions cannot be separated in the subsequent nanofiltration membrane separation stage. Therefore, developing adsorbent materials with high selectivity for lithium ions and monovalent salt ions is crucial. Summary of the Invention
[0005] The purpose of this invention is to overcome the problems of low adsorption capacity and poor selectivity of lithium-ion adsorbent materials in the prior art for monovalent ions such as sodium and potassium ions and lithium ions, and to provide a lithium-ion adsorbent material, its preparation method and application, which has high adsorption capacity and high potassium / lithium and sodium / lithium ion selectivity.
[0006] To achieve the above objectives, the first aspect of the present invention provides a lithium-ion adsorption material, the lithium-ion adsorption material comprising a polymer framework and a lithium-ion sieve dispersed on the polymer framework;
[0007] The polymer backbone comprises polyacrylonitrile molecular chains and is formed by... The structure shown in Formula I, grafted onto the polyacrylonitrile molecular chain.
[0008]
[0009] Where R is H, OH or NH2; m is 0, 1 or 2; n is an integer from 1 to 50;
[0010] Based on the total weight of the lithium-ion adsorbent material, the content of polyacrylonitrile molecular chains is 10-23 wt%, the content of the structure shown in Formula I is 0.2-8 wt%, and the content of the lithium-ion sieve is 70-88 wt%.
[0011] A second aspect of the present invention provides a method for preparing a lithium-ion adsorbent material, the method comprising the following steps:
[0012] (1) Polyacrylonitrile, monomer A shown in Formula 1 and a first solvent are mixed to obtain a first mixture;
[0013] (2) The initiator is mixed with the first mixture to obtain a second mixture;
[0014] (3) Add the lithium ion sieve to the second mixture for a third mixing to obtain the third mixture;
[0015] (4) The third mixture is added dropwise to the second solvent to obtain a lithium-ion adsorbent material;
[0016] The initiator is an aldehyde compound;
[0017]
[0018] Where R is H, OH or NH2; m is 0, 1 or 2; n is an integer from 1 to 50.
[0019] A third aspect of the present invention provides a lithium-ion adsorbent material prepared by the preparation method described in the second aspect above.
[0020] The fourth aspect of the present invention provides the application of the lithium-ion adsorbent materials described in the first and third aspects above in lithium extraction, preferably in the application of lithium extraction in a liquid environment.
[0021] Through the above technical solutions, the lithium-ion adsorption material, its preparation method, and its application provided by the present invention achieve the following beneficial effects:
[0022] The lithium-ion adsorbent material provided by this invention comprises a polymer framework and lithium-ion sieves dispersed on the polymer framework. This lithium-ion adsorbent material has abundant ether bonds, which significantly increases its adsorption capacity for lithium ions and further enhances its adsorption capacity for K+. + / Li + The selectivity. Attached Figure Description
[0023] Figure 1 The infrared spectrum is shown for the lithium-ion adsorbent material prepared in Example 5. Detailed Implementation
[0024] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0025] The first aspect of the present invention provides a lithium-ion adsorption material, the lithium-ion adsorption material comprising a polymer framework and a lithium-ion sieve dispersed on the polymer framework;
[0026] The polymer backbone comprises polyacrylonitrile molecular chains and is formed by... The structure shown in Formula I, grafted onto the polyacrylonitrile molecular chain.
[0027]
[0028] Where R is H, OH or NH2; m is 0, 1 or 2; n is an integer from 1 to 50;
[0029] Based on the total weight of the lithium-ion adsorbent material, the content of polyacrylonitrile molecular chains is 10-23 wt%, the content of the structure shown in Formula I is 0.2-8 wt%, and the content of the lithium-ion sieve is 70-88 wt%.
[0030] In this invention, the lithium-ion adsorbent material comprises a polymer framework and lithium-ion sieves dispersed on the polymer framework. This lithium-ion adsorbent material has abundant ether bonds, which significantly increases its adsorption capacity for lithium ions and further enhances its adsorption capacity for K+. + / Li + The selectivity.
[0031] More preferably, R is H or NH2; m is 1 or 2; n is an integer from 15 to 50.
[0032] In this invention, based on the total weight of the lithium-ion adsorbent material, the content of polyacrylonitrile molecular chains is 10-23 wt%, for example, it can be any two values forming a range or values within the range of 10 wt%, 11 wt%, 11.5 wt%, 12 wt%, 12.5 wt%, 12.8 wt%, 13 wt%, 13.5 wt%, 14 wt%, 15 wt%, 15.5 wt%, 16 wt%, 17 wt%, 17.5 wt%, 18 wt%, 18.5 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, and 23 wt%, or more.
[0033] In this invention, based on the total weight of the lithium-ion adsorbent material, the content of the structure shown in Formula I is 0.2-8 wt%, for example, it can be any two values forming a range or values within the range of 0.2 wt%, 0.5 wt%, 0.8 wt%, 1 wt%, 1.5 wt%, 1.8 wt%, 2 wt%, 2.5 wt%, 2.8 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, 5 wt%, 6 wt%, 6.5 wt%, 7 wt%, and 8 wt%.
[0034] In this invention, based on the total weight of the lithium-ion adsorbent material, the content of the lithium-ion sieve is 70-88 wt%, for example, it can be any two values forming a range or values within the range of 70 wt%, 70.5 wt%, 71 wt%, 72 wt%, 73 wt%, 74 wt%, 75 wt%, 76 wt%, 77 wt%, 78 wt%, 80 wt%, 81 wt%, 82 wt%, 83 wt%, 84 wt%, 85 wt%, 86 wt%, 87 wt%, and 88 wt%.
[0035] In this invention, when the content of polyacrylonitrile molecular chains, the structure shown in Formula I, and the lithium ion sieve in the lithium ion adsorption material meets the above-mentioned range, the lithium ion adsorption material can have high adsorption capacity and selectivity.
[0036] In this invention, the total content of the polyacrylonitrile molecular chain, the content of the structure shown in Formula I, and the content of the lithium ion sieve is 100 wt%.
[0037] In this invention, the contents of polyacrylonitrile molecular chains, the structure shown in Formula I, and lithium ion sieves in the lithium ion adsorption material are determined by the following method: Specifically, the contents of polyacrylonitrile structural units and lithium ion sieves in the lithium ion adsorption material are measured by X-ray photoelectron spectroscopy (XPS). The mass percentage of -C=N is obtained by peak separation of the fine spectrum. The content of polyacrylonitrile structural units is calculated by the content of -C=N (mass percentage of polyacrylonitrile structural units = mass percentage of -C=N / 26 × relative atomic mass of polyacrylonitrile). The content of lithium ion sieves is calculated by the content of metals Mn, Al, or Ti (taking manganese-based lithium ion sieves as an example, the mass percentage of lithium ion sieves = mass percentage of manganese / relative atomic mass of manganese × relative atomic mass of lithium ion sieves). The content of the structure shown in Formula I = 1 - mass percentage of polyacrylonitrile structural units - mass percentage of lithium ion sieves.
[0038] Furthermore, based on the total weight of the lithium-ion adsorbent material, the content of polyacrylonitrile molecular chains is 12-17 wt%, the content of the structure shown in Formula I is 1-6 wt%, and the content of the lithium-ion sieve is 78-84 wt%.
[0039] According to the present invention, preferably, the lithium ions are screened from LiMn2O4 and Li 1.6 Mn 1.6 O4, Li 1.33 Mn 1.67 O4, Li4Mn5O 12 LiMnO2, Li2TiO3, Li 1.33 Ti 1.66 O4, Li4Ti5O 12 At least one of LiCl·2Al(OH)3·nH2O.
[0040] In this invention, there is no particular limitation on the source of the lithium-ion sieve; it can be commercially available or prepared in-house using conventional methods in the art.
[0041] In one specific embodiment of the present invention, the manganese-based lithium ion sieve can be prepared by a solid-state method, specifically: a lithium source and a manganese source are mixed with an n(Li):n(Mn) ratio of 0.8-1:1, and calcined at 600-800°C for 4-10 hours to obtain the manganese-based lithium ion sieve.
[0042] In another specific embodiment of the present invention, the titanium-based lithium-ion sieve can be prepared by a solid-state method. Specifically, the lithium source and the titanium source are mixed with an n(Li):n(Ti) ratio of 2-2.5:1 and calcined at 600-900°C for 4-10 hours to obtain the titanium-based lithium-ion sieve.
[0043] In this invention, there is no particular limitation on the lithium source, and conventional lithium sources in the art can be used, such as lithium carbonate, lithium nitrate, lithium chloride, lithium sulfate, etc.
[0044] In this invention, there is no particular limitation on the titanium source, and conventional titanium sources in the art, such as titanium dioxide, can be used.
[0045] In this invention, there is no particular limitation on the source of manganese; conventional manganese sources in the art, such as manganese carbonate and manganese nitrate, can be used.
[0046] According to the present invention, preferably, the content of element O is 10-20 at.%, based on the total weight of the lithium-ion adsorbent material. For example, it can be 10 at.%, 10.5 at.%, 10.8 at.%, 11 at.%, 11.5 at.%, 12 at.%, 12.5 at.%, 13 at.%, 13.5 at.%, 14 at.%, 14.5 at.%, 14.8 at.%, 15 at.%, 15.3 at.%, 15.5 at.%, 15.8 at.%, 16 at.%, 16.5 at.%, 17 at.%, 17.5 at.%, 18 at.%, 19 at.%, 19.5 at.%, 19.8 at.%, 20 at.%, or any two of the above values within a range.
[0047] In this invention, when the O element content in the lithium-ion adsorbent material meets the above-mentioned range, the polymer backbone of the lithium-ion adsorbent material has abundant ether bonds, which is beneficial to the adsorption of lithium ions. This significantly increases the adsorption capacity of the lithium-ion adsorbent material for lithium ions and also improves the adsorption capacity of the lithium-ion adsorbent material for K+. + / Li + The selectivity.
[0048] Furthermore, based on the total weight of the lithium-ion adsorbent material, the O element content is 13.5-20 at.%.
[0049] In this invention, the content of O element in the lithium ion adsorbent material is determined by X-ray photoelectron spectroscopy (XPS).
[0050] According to the present invention, preferably, the average particle size of the lithium-ion adsorbent material is 1-5 mm.
[0051] In this invention, when the average particle size of the lithium-ion adsorbent material meets the above-mentioned range, it can ensure that the lithium-ion adsorbent material has a high packing density when extracting lithium in a liquid environment, thereby ultimately improving the adsorption capacity for lithium.
[0052] Furthermore, the average particle size of the lithium-ion adsorbent material is 3-4 mm.
[0053] In this invention, the average particle size of the lithium-ion adsorbent material is determined by micrometer.
[0054] In this invention, the average particle diameter of the lithium ion sieve in the lithium ion adsorption material profile measured by SEM electron microscopy is less than or equal to 2 μm.
[0055] In this invention, when the average particle diameter of the lithium ion sieve in the profile of the lithium ion adsorption material meets the above-mentioned range, the effective adsorption performance of the lithium ion sieve is maximized, resulting in a large adsorption capacity and high desorption efficiency of the lithium ion adsorption material.
[0056] In this invention, the average particle diameter of the lithium ion sieve in the lithium ion adsorption material is measured by SEM electron microscopy. When the lithium ion sieve does not agglomerate at all, the average particle diameter is the average particle size of a single lithium ion sieve. When the lithium ion sieve partially agglomerates, the average particle diameter is the average particle diameter of the largest aggregate.
[0057] Furthermore, the average particle diameter of the lithium ion sieve in the lithium adsorbent material profile measured by SEM electron microscopy is less than or equal to 1 μm.
[0058] According to the present invention, preferably, the specific surface area of the lithium-ion adsorbent material is 15-40 m². 2 / g.
[0059] In this invention, when the specific surface area of the lithium-ion adsorbent material meets the above-mentioned range, the lithium-ion adsorbent material can have a high saturated adsorption capacity when used for liquid lithium extraction.
[0060] Furthermore, the specific surface area of the lithium-ion adsorbent material is 17-24 m². 2 / g.
[0061] In this invention, the specific surface area of the lithium-ion adsorbent material is determined using the BET method.
[0062] A second aspect of the present invention provides a method for preparing a lithium-ion adsorbent material, the method comprising the following steps:
[0063] (1) Polyacrylonitrile, monomer A shown in Formula 1 and a first solvent are mixed to obtain a first mixture;
[0064] (2) The initiator is mixed with the first mixture to obtain a second mixture;
[0065] (3) Add the lithium ion sieve to the second mixture for a third mixing to obtain the third mixture;
[0066] (4) The third mixture is added dropwise to the second solvent to obtain a lithium-ion adsorbent material;
[0067] The initiator is an aldehyde compound;
[0068]
[0069] Where R is H, OH or NH2; m is 0, 1 or 2; n is an integer from 1 to 50.
[0070] In this invention, a mixed solution containing polyacrylonitrile and monomer A undergoes a phase inversion under the action of an initiator. An amine compound containing ether oxygen bonds bonds with polyacrylonitrile through a reaction, resulting in a polymer backbone rich in ether bonds. The inventors of this invention discovered that ether oxygen bonds have a stronger affinity for lithium ions, which is beneficial for lithium ion adsorption, thus significantly increasing the adsorption capacity of the lithium ion adsorbent material. Furthermore, the introduction of ether bonds further enhances the material's adsorption capacity for K+. + / Li + The selectivity.
[0071] In this invention, by adopting the specific mixing sequence described above, the lithium-ion adsorbent material can be well shaped, and the dispersion of lithium-ion sieves in the polymer framework can be more uniform, thereby giving the lithium-ion adsorbent material a high adsorption capacity.
[0072] According to the present invention, preferably, the weight-average molecular weight of the polyacrylonitrile is 5000-25000 g / mol, more preferably 7000-9000 g / mol.
[0073] In this invention, monomer A can be selected from polyoxyethylene diamine (Mw = 200-2000 g / mol), methoxy polyethylene glycolamine (Mw = 20-2000 g / mol), 1,8-diamino-3,6-dioxaoctane, 2-[2-(2-aminoethoxy)ethoxy]ethanol, 1-amino-3,6,9-triox-11-undecane, 3,6,9-trioxa-1-aminodecane, dimethoxyethylamine, 2,2'-oxobis(ethylamine), 3-(2-chloroquinoline-3-yl)-1- At least one of phenyl-2-propen-1-one, aminododecyl glycol monomethyl ether, 2,5,8,11,14,17,20,23,26-nonoxaoctacosane-28-amine, O,O'-bis(2-aminoethyl)heptadecaoctadecyl glycol, 1-(2-aminoethoxy)-2-methoxyethane, 3,6,9,12,15,18,21-heptaoxatricarane-1,23-diamine, and aminohexadecyl glycol monomethyl ether, more preferably polyoxyethylene diamine (Mw = 2000 g / mol).
[0074] In this invention, the lithium ions are screened from LiMn2O4 and Li 1.6 Mn 1.6 O4, Li 1.33 Mn1.67 O4, Li4Mn5O 12 LiMnO2, Li2TiO3, Li 1.33 Ti 1.66 O4, Li4Ti5O 12 At least one of LiCl·2Al(OH)3·nH2O.
[0075] According to the present invention, preferably, in the first mixture, the concentration of polyacrylonitrile is 5-12 wt%, and the concentration of monomer A is 0.02-5 wt%.
[0076] In this invention, when the concentrations of polyacrylonitrile and monomer A in the first mixture are controlled to meet the above-mentioned range, the resulting lithium-ion adsorbent material can have a high adsorption capacity.
[0077] Furthermore, in the first mixture, the concentration of polyacrylonitrile is 6-8 wt%, and the concentration of monomer A is 0.5-3 wt%.
[0078] In this invention, the first solvent is a conventional organic solvent in the art. Preferably, the first solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide.
[0079] In this invention, there is no particular limitation on the amount of the first solvent, as long as the concentrations of polyacrylonitrile and monomer A in the first mixture meet the requirements of this invention.
[0080] According to the present invention, preferably, the initiator is selected from at least one of formaldehyde, acetaldehyde and glutaraldehyde, more preferably formaldehyde.
[0081] According to the present invention, preferably, the weight ratio of the initiator to the monomer A is 0.5-5:1.
[0082] In this invention, when the weight ratio of the initiator to monomer A meets the above-mentioned range, the resulting lithium-ion adsorbent material framework possesses abundant ether bonds, which facilitates lithium-ion adsorption, increases lithium adsorption capacity, and further enhances the lithium-ion adsorption capacity due to the introduction of ether bonds. + / Li + The selectivity.
[0083] Furthermore, the weight ratio of the initiator to the monomer A is 0.6-2:1.
[0084] According to the present invention, preferably, the concentration of lithium ion sieve in the third mixture is 20-50 wt%.
[0085] In this invention, when the concentration of lithium ion sieve in the third mixture is controlled to meet the above-mentioned range, the prepared lithium ion adsorbent material can have high adsorption capacity, magnesium-lithium selectivity, and calcium-lithium selectivity.
[0086] Furthermore, the concentration of lithium-ion sieves in the third mixture is 40-50 wt%.
[0087] According to the present invention, preferably, the conditions for the first mixing include: a mixing temperature of 20-80°C and a mixing time of 12-24 hours.
[0088] According to the present invention, preferably, the conditions for the second mixing include: a mixing temperature of 30-90°C and a mixing time of 12-24h.
[0089] According to the present invention, preferably, the conditions for the third mixing include: a mixing temperature of 20-80°C and a mixing time of 12-24 hours.
[0090] In this invention, when the conditions for controlling the first mixing, the second mixing, or the third mixing meet the above-mentioned range, the lithium ion sieves in the prepared lithium ion adsorbent material are uniformly dispersed in the framework, thereby improving the adsorption capacity and selectivity of the lithium ion adsorbent material.
[0091] Furthermore, the conditions for the first mixing include: a mixing temperature of 60-80°C and a mixing time of 18-24 hours.
[0092] Furthermore, the conditions for the second mixing include: a mixing temperature of 75-85°C and a mixing time of 18-24 hours.
[0093] Furthermore, the conditions for the third mixing include: a mixing temperature of 50-60°C and a mixing time of 18-24 hours.
[0094] In this invention, the first mixing, the second mixing, and the third mixing are preferably carried out under stirring.
[0095] In this invention, there is no particular limitation on the type of the second solvent, as long as the lithium-ion adsorbent material can be formed. Preferably, the second solvent is deionized water.
[0096] In this invention, there is no particular limitation on the amount of the second solvent, as long as the resulting lithium-ion adsorbent material can be formed.
[0097] In this invention, in step (4), the drop-addition method enables the lithium-ion adsorbent material to be formed and have a certain strength, so that it can be recycled multiple times.
[0098] In a preferred embodiment of the present invention, the third mixture is dripped into deionized water at a dripping rate of 0.8-1.2 mL / min using an auto-injector, and then soaked at 30-40°C for 12-24 hours.
[0099] In this invention, step (4) further includes rinsing the soaked lithium-ion adsorbent material with deionized water.
[0100] According to the present invention, preferably, the method further includes the step of washing the lithium-ion adsorbent material with an acidic solution.
[0101] In this invention, the lithium-ion adsorbent material is a lithium adsorbent material precursor. The lithium-ion adsorbent material is washed with an acidic solution to remove the lithium ions from the precursor. + and H + Exchange is used to activate the precursor, resulting in an H-type lithium-ion sieve, such as Li. 1.33 Mn 1.67 O4 is converted to H 1.33 Mn 1.67 O4, the resulting H-type lithium ion sieve has a specific adsorption effect on lithium ions.
[0102] Furthermore, the lithium-ion adsorbent material is circulated and washed using an acidic solution under the action of a peristaltic pump.
[0103] Furthermore, the acidic solution is selected from at least one of hydrochloric acid, phosphoric acid, and sulfuric acid.
[0104] Furthermore, with H + The concentration of the acidic solution is estimated to be 0.1-0.5 mol / L.
[0105] Furthermore, the flow rate of the peristaltic pump is 1-25 mL / min, and the circulation time is 4-24 h.
[0106] A third aspect of the present invention provides a lithium-ion adsorbent material prepared by the preparation method described in the second aspect above.
[0107] The fourth aspect of the present invention provides the application of the lithium-ion adsorbent material described in the first or third aspect above in lithium extraction, preferably in the application of lithium extraction in a liquid environment.
[0108] In this invention, the lithium-ion adsorbent material has high adsorption capacity and monovalent ion selectivity when used for liquid lithium extraction.
[0109] The present invention will be described in detail below through embodiments.
[0110] The average particle size of the lithium-ion adsorbent material was determined by micrometer.
[0111] The average particle diameter of the lithium ion sieve in the lithium ion adsorption material was measured by SEM electron microscopy.
[0112] The specific surface area of the lithium-ion adsorbent material was determined by the BET method. Specifically, the adsorption-desorption isotherm of N2 by the lithium-ion adsorbent material was measured at 77 K, and the BET specific surface area was obtained by fitting the isotherm.
[0113] The content of oxygen (O) in the lithium-ion adsorbent material was determined by X-ray photoelectron spectroscopy (XPS).
[0114] Adsorption capacity: The obtained granulated particles (4g) were packed into a glass column and acid-washed (using H2O). + The adsorption-desorption cycle was performed for 24 hours using 0.5 mol / L hydrochloric acid at a flow rate of 2 mL / min. A mixture of lithium chloride, sodium chloride, and potassium chloride (lithium ion concentration 1000 mg / L, sodium ion concentration 1000 mg / L, potassium ion concentration 1000 mg / L, pH adjusted to 9.5 with ammonia-ammonium chloride buffer, V = 400 mL) was then pumped in at a flow rate of 2 mL / min using a peristaltic pump for 24 hours to desorb lithium ions from the particles. The particles were then washed with deionized water until neutral, constituting one cycle. During one adsorption process, the change in adsorption capacity over time was monitored, and the saturated adsorption capacity Q was calculated using the following formula:
[0115]
[0116] Where Q is the saturated adsorption capacity in mg / g, reflecting the amount of adsorption at equilibrium; C0 and C are the initial and saturated ion concentrations in the solution, respectively, in mg / L; V is the volume of the adsorption solution in L; and m is the mass of the particulate adsorbent in g. Ion concentrations were determined using ion chromatography (ICS-1100, DIONEX, America).
[0117] Distribution coefficient (K) d (Unit: mg / L) represents the affinity of the reactive adsorbent for ions. Selectivity coefficient. The partition coefficient (K) indicates the preference of an adsorbent material for ions A when adsorbing two types of ions, A and B. A higher value indicates better selectivity for ions A, reflecting the selectivity of the lithium-ion adsorbent material for different ions. d The ratio of ).
[0118]
[0119] In the above formula, C0 represents the concentration of each ion in the solution before adsorption, in mg / L; C eV represents the concentration of each ion at adsorption saturation, in mg / L; V is the solution volume, in mL; and m is the mass of the lithium-ion adsorbent material, in g.
[0120] The content of polyacrylonitrile structural units and lithium ion sieves in lithium ion adsorbent materials was measured using X-ray photoelectron spectroscopy (XPS). Specifically, the mass percentage of -C=N was obtained by peak segmentation of the fine spectrum, and the content of polyacrylonitrile structural units was calculated from the content of -C=N (mass percentage of polyacrylonitrile structural units = mass percentage of -C=N / 26 × relative atomic mass of polyacrylonitrile). The content of lithium ion sieves was calculated from the content of metals Mn, Al, or Ti (taking manganese-based lithium ion sieves as an example, the mass percentage of lithium ion sieves = mass percentage of manganese / relative atomic mass of manganese × relative atomic mass of lithium ion sieves). The content of the structure shown in Equation I = 1 - mass percentage of polyacrylonitrile structural units - mass percentage of lithium ion sieves.
[0121] Additionally, in the following examples and comparative examples: all reagents were purchased from Innovent Biologics Inc.
[0122] Example 1
[0123] (1) Polyacrylonitrile (Mw = 80,000 g / mol) powder and polyoxyethylene diamine (Mw = 2,000 g / mol, where R = NH2, m = 2, n = 49) were dissolved in DMF and stirred at 60°C for 24 h to obtain the first mixture. The concentration of polyacrylonitrile in the first mixture was 6 wt% and the concentration of polyoxyethylene diamine was 2 wt%.
[0124] (2) Add formaldehyde (the weight ratio of formaldehyde to polyoxyethylene diamine is 1:1) to the first mixture, stir at 85°C for 24 hours to obtain the second mixture, the concentration of formaldehyde in the second mixture is 2wt%.
[0125] (3) Lithium ion sieve Li2TiO3 (average particle size 0.2μm) was added to the second mixture and stirred at 60℃ for 24h to obtain the third mixture. The concentration of lithium ion sieve in the third mixture was 40wt%.
[0126] (4) The third mixture was added to the deionized water solution by an automatic syringe at a dropping rate of 1 mL / min. After soaking at 30°C for 12 h, it was rinsed with deionized water to obtain lithium ion adsorbent material M1.
[0127] Example 2
[0128] (1) Polyacrylonitrile (Mw = 80,000 g / mol) powder and polyoxyethylene diamine (Mw = 2,000 g / mol, where R = NH2, m = 2, n = 49) were dissolved in DMF and stirred at 60°C for 24 h to obtain the first mixture. The concentration of polyacrylonitrile in the first mixture was 8 wt% and the concentration of polyoxyethylene diamine was 3 wt%.
[0129] (2) Add formaldehyde (the weight ratio of formaldehyde to polyoxyethylene diamine is 0.67:1) to the first mixture, stir at 85°C for 24 hours to obtain the second mixture, the concentration of formaldehyde in the second mixture is 2wt%.
[0130] (3) Lithium ion sieve Li2TiO3 (average particle size 0.2μm) was added to the second mixture and stirred at 60℃ for 24h to obtain the third mixture. The concentration of lithium ion sieve in the third mixture was 40wt%.
[0131] (4) The third mixture was added to the deionized water solution by an automatic syringe at a dropping rate of 1 mL / min. After soaking at 30°C for 12 h, it was rinsed with deionized water to obtain lithium ion adsorbent material M2.
[0132] Example 3
[0133] (1) Polyacrylonitrile (Mw = 80,000 g / mol) powder and polyoxyethylene diamine (Mw = 2,000 g / mol, where R = NH2, m = 2, n = 49) were dissolved in DMF and stirred at 60°C for 24 h to obtain the first mixture. The concentration of polyacrylonitrile in the first mixture was 8 wt% and the concentration of polyoxyethylene diamine was 0.5 wt%.
[0134] (2) Add formaldehyde (the weight ratio of formaldehyde to polyoxyethylene diamine is 2:1) to the first mixture, stir at 85°C for 24 hours to obtain the second mixture, the concentration of formaldehyde in the second mixture is 2wt%.
[0135] (3) Lithium ion sieve Li2TiO3 (average particle size 0.2μm) was added to the second mixture and stirred at 60℃ for 24h to obtain the third mixture. The concentration of lithium ion sieve in the third mixture was 40wt%.
[0136] (4) The third mixture was added to the deionized water solution by an automatic syringe at a dropping rate of 1 mL / min. After soaking at 30°C for 12 h, it was rinsed with deionized water to obtain lithium ion adsorbent material M3.
[0137] Example 4
[0138] (1) Polyacrylonitrile (Mw = 80,000 g / mol) powder and polyoxyethylene diamine (Mw = 2,000 g / mol, where R = NH2, m = 2, n = 49) were dissolved in DMF and stirred at 60°C for 24 h to obtain the first mixture. The concentration of polyacrylonitrile in the first mixture was 12 wt% and the concentration of polyoxyethylene diamine was 0.1 wt%.
[0139] (2) Add formaldehyde (the weight ratio of formaldehyde to polyoxyethylene diamine is 10:1) to the first mixture, stir at 85°C for 24 hours to obtain the second mixture, the concentration of formaldehyde in the second mixture is 1 wt%.
[0140] (3) Lithium ion sieve Li2TiO3 (average particle size 0.2μm) was added to the second mixture and stirred at 60℃ for 24h to obtain the third mixture. The concentration of lithium ion sieve in the third mixture was 40wt%.
[0141] (4) The third mixture was added to the deionized water solution by an automatic syringe at a dropping rate of 1 mL / min. After soaking at 30°C for 12 h, it was rinsed with deionized water to obtain lithium ion adsorbent material M4.
[0142] Example 5
[0143] (1) Polyacrylonitrile (Mw = 80,000 g / mol) powder and polyoxyethylene diamine (Mw = 2,000 g / mol, where R = NH2, m = 2, n = 49) were dissolved in DMF and stirred at 60°C for 24 h to obtain the first mixture. The concentration of polyacrylonitrile in the first mixture was 6 wt% and the concentration of polyoxyethylene diamine was 2 wt%.
[0144] (2) Add formaldehyde (the weight ratio of formaldehyde to polyoxyethylene diamine is 0.25:1) to the first mixture, stir at 85°C for 24 hours to obtain the second mixture, the concentration of formaldehyde in the second mixture is 0.5 wt%.
[0145] (3) LiMn2O4 lithium ion sieve (average particle size 1 μm) was added to the second mixture and stirred at 60°C for 24 h to obtain the third mixture. The concentration of lithium ion sieve in the third mixture was 40 wt%.
[0146] (4) The third mixture was dripped into the deionized water solution at a rate of 1 mL / min using an automatic syringe. After soaking at 30°C for 12 h, it was rinsed with deionized water to obtain lithium ion adsorbent material M5.
[0147] Example 6
[0148] (1) Polyacrylonitrile (Mw = 80,000 g / mol) powder and polyoxyethylene diamine (Mw = 2,000 g / mol, where R = NH2, m = 2, n = 49) were dissolved in DMF and stirred at 30°C for 24 h to obtain the first mixture. The concentration of polyacrylonitrile in the first mixture was 6 wt% and the concentration of polyoxyethylene diamine was 2 wt%.
[0149] (2) Add formaldehyde (the weight ratio of formaldehyde to polyoxyethylene diamine is 1:1) to the first mixture, stir at 30°C for 24 hours to obtain the second mixture, the concentration of formaldehyde in the second mixture is 2wt%.
[0150] (3) Lithium ion sieve Li2TiO3 (average particle size 0.2μm) was added to the second mixture and stirred at 60℃ for 24h to obtain the third mixture. The concentration of lithium ion sieve in the third mixture was 40wt%.
[0151] (4) The third mixture was added to the deionized water solution by an automatic syringe at a dropping rate of 1 mL / min. After soaking at 30°C for 12 h, it was rinsed with deionized water to obtain lithium ion adsorbent material M6.
[0152] Example 7
[0153] (1) Polyacrylonitrile (Mw = 80,000 g / mol) powder and 1,8-diamino-3,6-dioxaneamine (where R = NH2, m = 2, n = 2) were dissolved in DMF and stirred at 60°C for 24 h to obtain the first mixture. The concentration of polyacrylonitrile in the first mixture was 6 wt% and the concentration of 1,8-diamino-3,6-dioxaneamine was 2 wt%.
[0154] (2) Add formaldehyde (the weight ratio of formaldehyde to polyoxyethylene diamine is 1:1) to the first mixture, stir at 85°C for 24 hours to obtain the second mixture, the concentration of formaldehyde in the second mixture is 2wt%.
[0155] (3) Lithium ion sieve Li2TiO3 (average particle size 0.2μm) was added to the second mixture and stirred at 60℃ for 24h to obtain the third mixture. The concentration of lithium ion sieve in the third mixture was 40wt%.
[0156] (4) The third mixture was added to the deionized water solution by an automatic syringe at a dropping rate of 1 mL / min. After soaking at 30°C for 12 h, it was rinsed with deionized water to obtain lithium ion adsorbent material M7.
[0157] Example 8
[0158] The preparation method of Example 2 was followed, except that the concentration of polyoxyethylene diamine in step (1) was 6 wt% and the weight ratio of formaldehyde to polyoxyethylene diamine in step (2) was 0.5:1. Lithium-ion adsorbent material M8 was obtained.
[0159] Example 9
[0160] (1) Polyacrylonitrile (Mw = 80,000 g / mol) powder and polyoxyethylene diamine (Mw = 2,000 g / mol, where R = NH2, m = 2, n = 49) were dissolved in DMF and stirred at 20°C for 24 h to obtain the first mixture. The concentration of polyacrylonitrile in the first mixture was 8 wt% and the concentration of polyoxyethylene diamine was 3 wt%.
[0161] (2) Add formaldehyde (the weight ratio of formaldehyde to polyoxyethylene diamine is 0.67:1) to the first mixture, stir at 20°C for 24 hours to obtain the second mixture, the concentration of formaldehyde in the second mixture is 2wt%.
[0162] (3) Add lithium ion sieve Li2TiO3 (average particle size 0.2μm) to the second mixture, stir at 20℃ for 24h to obtain the third mixture, the concentration of lithium ion sieve in the third mixture is 40wt%;
[0163] (4) The third mixture was added to the deionized water solution by an automatic syringe at a dropping rate of 1 mL / min. After soaking at 4°C for 12 h, it was rinsed with deionized water to obtain lithium ion adsorbent material M9.
[0164] Example 10
[0165] The preparation method of Example 2 was followed, except that the concentration of polyoxyethylene diamine in step (1) was 10 wt% and the weight ratio of formaldehyde to polyoxyethylene diamine in step (2) was 0.2:1. Lithium-ion adsorbent material M10 was obtained.
[0166] Example 11
[0167] The preparation method of Example 2 was followed, except that the weight-average molecular weight of polyoxyethylene diamine in step (1) was 400 g / mol (where R = NH2, m = 2, n = 9). Lithium-ion adsorbent material M11 was obtained.
[0168] Comparative Example 1
[0169] The lithium-ion adsorbent material was prepared according to the method of Example 1, except that polyoxyethylene diamine was not added in step (1) and step (2) was not performed. The lithium-ion adsorbent material N1 was obtained.
[0170] Comparative Example 2
[0171] The lithium-ion adsorbent material was prepared according to the method in Example 1, except that formaldehyde was not added in step (2). The resulting lithium-ion adsorbent material N2 was obtained.
[0172] Comparative Example 3
[0173] The lithium-ion adsorbent material was prepared according to the method of Example 1, except that the amine monomer in step (1) was amino polyethylene glycol (Mw = 2000 g / mol). The lithium-ion adsorbent material N3 was obtained.
[0174] The structure and physicochemical parameters of the lithium-ion adsorbent materials prepared in the examples and comparative examples were tested, and the results are shown in Table 1.
[0175] Table 1
[0176]
[0177]
[0178] Test case
[0179] The adsorption capacity, potassium-lithium selectivity coefficient, and sodium-lithium selectivity coefficient of the lithium-ion adsorbent materials prepared in the examples and comparative examples were tested, and the results are shown in Table 2.
[0180] Table 2
[0181] Adsorption capacity (mg / g) Potassium-lithium selectivity coefficient Sodium-lithium selectivity Example 1 17.4 13102 4906 Example 2 17.6 11034 3982 Example 3 16.8 12567 4104 Example 4 11.3 10169 2198 Example 5 16.6 11478 3141 Example 6 13.2 9987 1896 Example 7 14.1 1154 1353 Example 8 12.8 965 1156 Example 9 11.9 984 1241 Example 10 12.3 865 1268 Example 11 12.1 877 1201 Comparative Example 1 8.6 318 196 Comparative Example 2 8.4 289 150 Comparative Example 3 8.7 364 220
[0182] Figure 1 This is the infrared spectrum of the polymer and polyacrylonitrile after the reaction of polyacrylonitrile and polyoxyethylene diamine in Example 5. Figure 1 It can be seen that at approximately 3500cm -1 and 1670cm -1 Two absorption peaks appeared at the point, which correspond to the stretching vibration peaks of NH and C=NH, indicating that the grafting of polyacrylonitrile and polyoxyethylene diamine was successful.
[0183] As can be seen from Tables 1 and 2, compared with Comparative Example 1, the lithium-ion adsorbent material prepared in the embodiments of the present invention has abundant ether-oxygen bonds in its polymer framework, which is beneficial to the adsorption of lithium ions. This significantly increases the adsorption capacity of the lithium-ion adsorbent material for lithium ions. Furthermore, the introduction of ether bonds improves the material's adsorption capacity for K+. + / Li + The selectivity.
[0184] In Comparative Example 2, without formaldehyde to promote the reaction, the polymer skeleton could not effectively introduce ether oxygen bonds, resulting in low adsorption capacity of the lithium-ion adsorbent material and small potassium-lithium and sodium-lithium selectivity coefficients.
[0185] Compared with Comparative Example 3, the monomer A of Formula 1 can react effectively, providing ether oxygen bonds, which is more conducive to the adsorption of lithium ions. The resulting material has a larger adsorption capacity for lithium ions and stronger selectivity.
[0186] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A lithium-ion adsorbent material, characterized in that, The lithium-ion adsorption material includes a polymer framework and a lithium-ion sieve dispersed on the polymer framework; The polymer backbone comprises polyacrylonitrile molecular chains and is formed by... The structure shown in Formula I, grafted onto the polyacrylonitrile molecular chain. Where R is H, OH or NH2; m is 0, 1 or 2; n is an integer from 1 to 50; Based on the total weight of the lithium-ion adsorbent material, the content of polyacrylonitrile molecular chains is 10-23 wt%, the content of the structure shown in Formula I is 0.2-8 wt%, and the content of the lithium-ion sieve is 70-88 wt%.
2. The lithium-ion adsorbent material according to claim 1, wherein, R is H or NH2; m is 1 or 2; n is an integer from 15 to 50; Preferably, based on the total weight of the lithium-ion adsorbent material, the content of polyacrylonitrile molecular chains is 12-17 wt%, the content of the structure shown in Formula I is 1-6 wt%, and the content of the lithium-ion sieve is 78-84 wt%.
3. The lithium-ion adsorbent material according to claim 1 or 2, wherein, The lithium ions are selected from LiMn2O4 and Li 1.6 Mn 1.6 O4, Li 1.33 Mn 1.67 O4, Li4Mn5O 12 LiMnO2, Li2TiO3, Li 1.33 Ti 1.66 O4, Li4Ti5O 12 At least one of LiCl·2Al(OH)3·nH2O; Preferably, the content of oxygen element is 10-20 at.%, based on the total weight of the lithium-ion adsorbent material.
4. The lithium-ion adsorbent material according to any one of claims 1-3, wherein, The lithium-ion adsorbent material has an average particle size of 1-5 mm, preferably 3-4 mm; In this invention, the average particle diameter of the lithium ion sieve in the lithium ion adsorption material profile measured by SEM electron microscopy is less than or equal to 2 μm, preferably less than or equal to 1 μm. Preferably, the specific surface area of the lithium-ion adsorbent material is 15-40 m². 2 / g, preferably 17-24m 2 / g.
5. A method for preparing a lithium-ion adsorbent material, characterized in that, The method includes the following steps: (1) Polyacrylonitrile, monomer A shown in Formula 1 and a first solvent are mixed to obtain a first mixture; (2) The initiator is mixed with the first mixture to obtain a second mixture; (3) Add the lithium ion sieve to the second mixture for a third mixing to obtain the third mixture; (4) The third mixture is added dropwise to the second solvent to obtain a lithium-ion adsorbent material; The initiator is an aldehyde compound; Where R is H, OH or NH2; m is 0, 1 or 2; n is an integer from 1 to 50.
6. The preparation method according to claim 5, wherein, The weight-average molecular weight of the polyacrylonitrile is 5000-25000 g / mol; Preferably, in the first mixture, the concentration of polyacrylonitrile is 5-12 wt%, more preferably 6-8 wt%; and the concentration of monomer A is 0.02-5 wt%, more preferably 0.5-3 wt%. Preferably, the first solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide; Preferably, the lithium ions are selected from LiMn2O4 and Li 1.6 Mn 1.6 O4, Li 1.33 Mn 1.67 O4, Li4Mn5O 12 LiMnO2, Li2TiO3, Li 1.33 Ti 1.66 O4, Li4Ti5O 12 At least one of LiCl·2Al(OH)3·nH2O.
7. The preparation method according to claim 5 or 6, wherein, The initiator is selected from at least one of formaldehyde, acetaldehyde, and glutaraldehyde; Preferably, the weight ratio of the initiator to monomer A is 0.5-5:1; Preferably, the concentration of lithium ion sieve in the third mixture is 20-50 wt%, more preferably 40-50 wt%.
8. The preparation method according to any one of claims 5-7, wherein, The conditions for the first mixing include: a mixing temperature of 20-80℃ and a mixing time of 12-24h; Preferably, the conditions for the second mixing include: a mixing temperature of 30-90°C and a mixing time of 12-24 hours; Preferably, the conditions for the third mixing include: a mixing temperature of 20-80℃ and a mixing time of 12-24h.
9. The method according to any one of claims 5-8, wherein, The method further includes the step of washing the lithium-ion adsorbent material with an acidic solution; Preferably, the lithium-ion adsorbent material is circulated and washed using an acidic solution under the action of a peristaltic pump; Preferably, the acidic solution is selected from at least one of hydrochloric acid, phosphoric acid, and sulfuric acid; Preferably, H + The concentration of the acidic solution is calculated to be 0.1-1 mol / L; Preferably, the flow rate of the peristaltic pump is 1-25 mL / min, and the circulation time is 1-24 h.
10. A lithium-ion adsorbent material prepared by the preparation method according to any one of claims 5-9.
11. The application of the lithium-ion adsorbent material according to any one of claims 1-4 and 10 in lithium extraction, preferably in lithium extraction in a liquid environment.