A nitrogen-enriching phosphazene polymer adsorbent, its preparation method and application
By preparing a nitrogen-enriched phosphazene polymer adsorbent, the problem of low adsorption capacity of existing amino polymers was solved by utilizing strong coordination chelation, electrostatic attraction and spatial confinement effect, achieving efficient and renewable palladium ion recovery.
Patent Information
- Application Number
- CN202611621229.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing amino polymers have low adsorption capacity in the field of palladium ion recovery, making it difficult to develop efficient, renewable, and selective adsorption materials.
A nitrogen-enriched phosphazene polymer adsorbent is formed by polymerizing phosphazene compounds and heterocyclic diamine compounds in an organic alkaline solution using a preparation method. This adsorbent utilizes strong coordination chelation, electrostatic attraction, and spatial confinement effects to achieve efficient capture and selective adsorption of palladium ions.
The prepared nitrogen-enriched phosphazene polymer adsorbent exhibits high adsorption capacity and selectivity for palladium ions, with an adsorption rate of up to 100% and an adsorption capacity of up to 534.64 mg/g. Furthermore, the adsorbent can be reused through desorption and regeneration.
Smart Images

Figure CN123102318A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of adsorption materials technology, and in particular to a nitrogen-enriching phosphazene polymer adsorbent, its preparation method, and its application. Background Technology
[0002] Palladium, a scarce precious metal, has irreplaceable applications in electronics, catalysis, medicine, and jewelry. Improper discharge of palladium-containing wastewater not only wastes palladium resources but also causes heavy metal pollution, threatening ecological security and human health. For example, palladium ions readily form complexes in acidic wastewater, making efficient recovery difficult with traditional treatment methods (such as chemical precipitation and ion exchange), and potentially leading to secondary pollution. Therefore, developing adsorption materials that combine high selectivity, high adsorption capacity, and renewability is a key breakthrough for achieving palladium resource recycling and pollution control.
[0003] The key to achieving efficient palladium adsorption lies in the adsorbent having binding sites with a strong affinity for palladium. According to the hard-soft acid-base theory, palladium is a soft acid and tends to bind with soft base coordination atoms containing nitrogen, sulfur, and oxygen. Among these, nitrogen atoms have a larger atomic radius and lower electronegativity than oxygen, resulting in a stronger electron-donating ability and enabling the formation of a more stable coordination structure with palladium ions. Therefore, by introducing nitrogen-containing ligands into the adsorbent, their coordination with palladium and supramolecular interactions can be utilized to efficiently recover palladium ions from the leachate. Amino groups, with their unique electronic structure and coordination ability, play an irreplaceable role in the adsorption of noble metals. As a soft acid, palladium ions readily form stable complexes with nitrogen-containing soft base groups (such as 3,5-diaminopyridine). The pyridine nitrogen atom in 3,5-diaminopyridine provides a lone pair of electrons, which bind with Pd... 2+The empty d orbitals are coordinated, while the amino group can further stabilize the adsorption configuration through hydrogen bonding or electrostatic interactions. For example, Wang et al. (see existing literature: Wang J, Luo C, Wang W, et al. Enhanced separation of palladium from nuclear wastewater by the sulfur-rich functionalized covalent organic framework [J]. Nanomaterials, 2025, 15(10), 714.) synthesized amino covalent organic frameworks (COFs) using 1,3,5-tris(4-aminophenyl)benzene and 2,5-bis(methylthio)terephthalaldehyde as monomers. They utilized the nitrogen sites to chelate and coordinate tetrachloropalladium salts, and the resulting material had an adsorption capacity of 343.60 mg / g for palladium. Currently, a series of amino polymers with excellent adsorption properties have been reported in existing literature, such as aromatic covalent organic polymers (COPs) (see existing literature: Wang Y, Wu Y, Li J, et al. Ultra-selective and efficient static / dynamic palladium capture from highly acidic solution with robust macrocycle-based polymers [J]. Advanced Functional Materials, 2023, 33(50), 2304051.), covalent triazine frameworks (CTFs) (see existing literature: Wu P, Liu H, Sun M, et al. Covalent triazine frameworks for the selective sorption of palladium from highly acidic radioactive liquid wastes [J]. Journal of Materials Chemistry A, 2021, 9(48): 27320-27331.), and porous aromatic frameworks (PAFs) (see existing literature: Yuan Y, Han L, Wang N. Selective recovery of palladium from nuclearwaste by covalent organic framework [J]. Matter, 2022, 5(10): 3086-3111.).Amino polymers have great potential in palladium recovery, but they still face challenges, namely that the adsorption capacity of existing amino polymers is generally below 400 mg / g, while improving the adsorption capacity can significantly reduce investment costs.
[0004] Therefore, there is an urgent need to develop a nitrogen-enriched phosphazene polymer adsorbent with high adsorption capacity, high selectivity, and renewability, as well as its preparation method and application. Summary of the Invention
[0005] The present invention aims to provide a nitrogen-enriched phosphazene polymer adsorbent, its preparation method, and its application. The specific technical solution is as follows: In a first aspect, the present invention provides a method for preparing a nitrogen-enriched phosphazene polymer adsorbent, comprising: The prepared phosphazene compound solution and heterocyclic diamine compound solution were mixed and an organic alkali solution was added. After mixing, the mixture underwent polymerization and post-treatment to obtain a nitrogen-enriched phosphazene polymer adsorbent. The molar ratio of the phosphazene compound in the phosphazene compound solution to the heterocyclic diamine compound in the heterocyclic diamine compound solution is 1:1 to 1:3. The volume ratio of the phosphazene compound solution, the heterocyclic diamine compound solution, and the organic alkali solution is 5:5:6.5.
[0006] Optionally, the mass ratio of the phosphazene compound used in the phosphazene compound solution to the volume ratio of the first organic solution is 0.0695 g: 2 mL; The phosphazene compound includes hexachlorophosphazene; the organic alkaline solution includes triethylamine; The first organic solution includes at least one of tetrahydrofuran, N,N-dimethylformamide, and acetonitrile.
[0007] Optionally, the mass ratio of the heterocyclic diamine compound used in the heterocyclic diamine compound solution to the volume ratio of the second organic solution is 0.0649~0.0661g:3mL; The heterocyclic diamine compound includes at least one of m-phenylenediamine, 2,6-diaminopyridine, 3,5-diaminopyridine, 2,4-diaminopyridine, and 4,6-diaminopyrimidine; The second organic solution includes at least one of tetrahydrofuran, N,N-dimethylformamide, and acetonitrile.
[0008] Optionally, the polymerization reaction is carried out at a reaction temperature of 180°C for a reaction time of 3 hours.
[0009] Optionally, the post-processing includes centrifugation, washing, and freeze-drying in sequence; the centrifugation is performed at a speed of 5000 r / min for 5 min; the washing process includes washing the precipitate after centrifugation with ethanol and ultrapure water in sequence; and the freeze-drying process is performed at a temperature of -10℃ for 24 h.
[0010] In a second aspect, the present invention provides a nitrogen-enriched phosphazene polymer adsorbent, which is prepared by the aforementioned method for preparing nitrogen-enriched phosphazene polymer adsorbents.
[0011] In a third aspect, the present invention provides an application of the nitrogen-enriched phosphazene polymer adsorbent in the adsorption of palladium ions, wherein the nitrogen-enriched phosphazene polymer adsorbent is added to acidic wastewater containing palladium ions to carry out an adsorption reaction and recover palladium ions. The mass ratio of the nitrogen-enriched phosphazene polymer adsorbent to the volume of the palladium-containing acidic wastewater is 0.002~2g:3~3000mL; The concentration of palladium ions in the acidic wastewater containing palladium ions is not higher than 610 mg / L; The acidic substance used in the palladium-containing acidic wastewater includes hydrochloric acid solution; the concentration of the hydrochloric acid solution is 0.1~1 mol / L. The pH value of the acidic wastewater containing palladium ions is 1; The adsorption reaction was carried out at an adsorption temperature of 25°C for a time of 1 min to 72 h.
[0012] Optionally, the mass ratio of the nitrogen-enriched phosphazene polymer adsorbent to the volume ratio of the palladium-containing acidic wastewater is 0.005~1g:30~300mL; The concentration of palladium ions in the acidic wastewater containing palladium ions is 10~500 mg / L; The concentration of the hydrochloric acid solution is 0.1~0.5 mol / L.
[0013] Optionally, the nitrogen-enriched phosphazene polymer adsorbent can achieve an adsorption rate of up to 100% for palladium ions in the acidic wastewater containing palladium ions. The nitrogen-enriched phosphazene polymer adsorbent exhibits an adsorption capacity of up to 534.64 mg / g for palladium ions in the acidic wastewater containing palladium ions.
[0014] Optionally, after adsorbing the palladium ions, the process further includes solid-liquid separation and desorption regeneration to obtain a reusable nitrogen-enriched phosphazene polymer adsorbent. The desorbent used in the desorption and regeneration includes a desorption solution containing thiourea and / or nitric acid; in the desorption solution, the molar concentration of thiourea is 0.5 mol / L and the molar concentration of nitric acid is 1 mol / L. The desorption and regeneration process uses a desorption temperature of 25°C and a desorption time of 8 hours.
[0015] The application of the technical solution of the present invention has at least the following beneficial effects: (1) The present invention provides a method for preparing a nitrogen-enriched phosphazene polymer adsorbent, which can prepare a nitrogen-enriched phosphazene polymer adsorbent with high adsorption capacity, high selectivity and renewability. Specifically: Regarding high adsorption capacity and high selectivity, this invention utilizes an adsorbent prepared from a reaction system with a specific composition. Based on molecular-level directional design, a high density of nitrogen-containing functional groups is successfully introduced into the polymer framework of the adsorbent. This achieves efficient capture of palladium ions through a synergistic effect of multiple microscopic mechanisms, including strong coordination chelation, electrostatic attraction, and spatial confinement. Firstly, strong coordination chelation is the core driving force. Based on the hard and soft acid-base theory, Pd... 2+ It is a typical soft acid, while the abundant nitrogen atoms (including -NH2, pyridine nitrogen, and phosphazene nitrogen) on the polymer backbone and side chains of the adsorbent belong to a soft base. The lone pairs of electrons carried by these nitrogen atoms can be rapidly filled into Pd. 2+ Stable coordination bonds are formed in the empty d orbitals of the palladium ion. Crucially, two or more adjacent nitrogen atoms can form multidentate chelate rings (such as five- or six-membered ring chelates) with the same palladium ion. This multidentate effect greatly enhances the complexation stability and binding energy, giving the adsorbent extremely high selectivity for palladium. Secondly, electrostatic attraction plays an important auxiliary role in the initial stage of adsorption. Under the specific pH environment of acidic wastewater containing palladium ions, the side-chain amino groups undergo protonation and acquire a positive charge (-NH3). + This allows it to rapidly attract negatively charged palladium complex anions (such as [PdCl4]) from aqueous solutions via electrostatic attraction. 2- The adsorbent attracts palladium ions to the surface, significantly accelerating the adsorption kinetics. Furthermore, the spatial confinement effect further enhances the enrichment capacity. This adsorbent possesses a high specific surface area and abundant microporous and mesoporous structures, allowing palladium ions to not only firmly bind to surface functional groups but also diffuse into the pores, achieving a dual utilization of "surface anchoring" and "pore enrichment." Based on the synergistic effect of these multiple mechanisms, this nitrogen-enriched phosphazene polymer adsorbent exhibits excellent adsorption performance for palladium ions in wastewater, thus possessing both high adsorption capacity and high selectivity.
[0016] Regarding regenerability, after the adsorbent adsorbs palladium ions, a desorbent can be used to remove the palladium ions, thus regenerating the adsorbent.
[0017] (2) The nitrogen-enriched phosphazene polymer adsorbent prepared in this invention can achieve an adsorption rate of up to 100% for palladium ions in acidic wastewater containing palladium ions, and an adsorption capacity of up to 534.64 mg / g for palladium ions in acidic wastewater containing palladium ions.
[0018] In addition to the objectives, features, and advantages described above, the present invention has other objectives, features, and advantages. The invention will now be described in further detail with reference to the figures. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.
[0020] Figure 1 SEM image of HCCP-3,5-DAP prepared in Example 1.
[0021] Figure 2 This is a SEM image of C in HCCP-3,5-DAP in Example 1.
[0022] Figure 3 This is a SEM image of N in HCCP-3,5-DAP in Example 1.
[0023] Figure 4 This is a SEM image of P in HCCP-3,5-DAP in Example 1.
[0024] Figure 5 This is a SEM image of Cl in HCCP-3,5-DAP in Example 1.
[0025] Figure 6 This is an EDS elemental distribution diagram of HCCP-3,5-DAP in Example 1.
[0026] Figure 7 The image shows the SEM image of HCCP-3,5-DAP after adsorption of Pd(II) in Example 1.
[0027] Figure 8 The image shows the SEM image of C after adsorbing Pd(II) by HCCP-3,5-DAP in Example 1.
[0028] Figure 9 The image shows the SEM image of N after adsorbing Pd(II) by HCCP-3,5-DAP in Example 1.
[0029] Figure 10 The image shows the SEM image of P after adsorbing Pd(II) by HCCP-3,5-DAP in Example 1.
[0030] Figure 11 The image shows the SEM image of Cl after Pd(II) adsorption by HCCP-3,5-DAP in Example 1.
[0031] Figure 12 The image shows the SEM image of Pd after adsorbing Pd(II) by HCCP-3,5-DAP in Example 1.
[0032] Figure 13 The image shows the EDS elemental distribution of HCCP-3,5-DAP after adsorbing Pd(II) in Example 1.
[0033] Figure 14 The N2 adsorption-desorption isotherm and BET specific surface area diagram of HCCP-3,5-DAP in Example 1 are shown.
[0034] Figure 15 The infrared spectra of HCCP, 3,5-DAP, and HCCP-3,5-DAP in Example 1 are shown.
[0035] Figure 16 The XRD patterns of HCCP-3,5-DAP and Pd@HCCP-3,5-DAP in Example 1 are shown.
[0036] Figure 17 The graph shows the adsorption-desorption cycle regeneration performance of HCCP-3,5-DAP in Example 1.
[0037] exist Figure 6 and Figure 13 In the diagram, the horizontal axis represents energy; the vertical axis represents signal strength. exist Figure 14 In this diagram, the horizontal axis represents Relative Pressure (P / P0); the vertical axis represents Quantity Adsorbed; the horizontal axis represents Pore Diameter; the vertical axis represents Pore Volume; Adsorption represents adsorption; Desorption represents desorption; and DFT represents the pore size distribution calculation model. exist Figure 15 In the diagram, the horizontal axis represents wavenumber; the vertical axis represents transmittance. exist Figure 16 In the diagram, the horizontal axis 2θ represents the Bragg angle; the vertical axis Intensity represents the signal strength. exist Figure 17 In the graph, the horizontal axis represents the number of cycles; the vertical axis represents the adsorption ratio; and the vertical axis represents the desorption ratio. Detailed Implementation
[0038] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0039] Example 1: A method for preparing a nitrogen-enriched phosphazene polymer adsorbent, comprising: The prepared phosphazene compound solution and heterocyclic diamine compound solution were mixed and an organic alkali solution was added. After ultrasonic mixing, the mixture underwent polymerization and post-treatment to obtain a nitrogen-enriched phosphazene polymer adsorbent (denoted as HCCP-3,5-DAP). The molar ratio of the phosphazene compound in the phosphazene compound solution to the heterocyclic diamine compound in the heterocyclic diamine compound solution is 1:3; The volume ratio of the phosphazene compound solution, the heterocyclic diamine compound solution, and the organic alkali solution is 5:5:6.5.
[0040] The mass ratio of the phosphazene compound to the volume of the first organic solution used in the phosphazene compound solution is 0.0695 g: 2 mL; the phosphazene compound is ultrasonically mixed and dissolved in the first organic solution to obtain the phosphazene compound solution. The phosphazene compound is hexachlorophosphazene (HCCP); the organic alkaline solution is triethylamine; The first organic solution includes at least one of tetrahydrofuran, N,N-dimethylformamide and acetonitrile, specifically tetrahydrofuran.
[0041] The mass ratio of the heterocyclic diamine compound to the volume ratio of the second organic solution used in the heterocyclic diamine compound solution is 0.0655 g: 3 mL; the heterocyclic diamine compound is ultrasonically mixed and dissolved in the second organic solution to obtain the heterocyclic diamine compound solution. The heterocyclic diamine compound includes at least one of m-phenylenediamine, 2,6-diaminopyridine, 3,5-diaminopyridine, 2,4-diaminopyridine and 4,6-diaminopyrimidine, specifically 3,5-diaminopyridine (abbreviated as 3,5-DAP). The second organic solution includes at least one of tetrahydrofuran, N,N-dimethylformamide, and acetonitrile, specifically tetrahydrofuran.
[0042] The polymerization reaction was carried out at a temperature of 180°C for 3 hours.
[0043] The post-processing includes centrifugation, washing, and freeze-drying in sequence. The centrifugation is performed at a speed of 5000 r / min for 5 min, after which the supernatant is discarded and the lower solid precipitate is collected. The washing process involves washing the precipitate after centrifugation with ethanol and ultrapure water in sequence. The freeze-drying process is performed at a temperature of -10℃ for 24 h.
[0044] Example 2: Unlike Example 1, the heterocyclic diamine compound is 2,6-diaminopyridine.
[0045] Example 3: Unlike Example 1, the heterocyclic diamine compound is m-phenylenediamine; the mass ratio of the heterocyclic diamine compound used in the heterocyclic diamine compound solution to the volume ratio of the second organic solution is 0.0649 g: 3 mL.
[0046] Example 4: Unlike Example 1, the heterocyclic diamine compound is 2,4-diaminopyridine.
[0047] Example 5: Unlike Example 1, the heterocyclic diamine compound is 4,6-diaminopyrimidine; the mass ratio of the heterocyclic diamine compound used in the heterocyclic diamine compound solution to the volume ratio of the second organic solution is 0.0661 g: 3 mL.
[0048] Application Example 1: Prepare an 80.11 mg / L Pd(II) aqueous solution (i.e., an aqueous solution containing divalent palladium ions). Take 7 centrifuge tubes and add 20 mL of Pd(II) aqueous solution to each centrifuge tube. Then, use hydrochloric acid solution with a concentration of 0.1~1 mol / L (specifically 0.1 mol / L) to adjust the pH value of the Pd(II) aqueous solution in each centrifuge tube to be 1, 2, 3, 4, 5, 6 and 7 respectively.
[0049] Add 5 mg of the adsorbent prepared in Example 1 to each centrifuge tube and shake in a constant temperature water shaker at 25°C for 24 h. After adsorption is complete, take the upper palladium ion aqueous solution, dilute it by the appropriate factor, and use an atomic absorption spectrophotometer (AA-6680) to test the concentration of the remaining palladium ions. Calculate the corresponding adsorption rate and adsorption capacity using the following formulas: Equation (1); Equation (2); in, This indicates the adsorption capacity of the adsorbent at adsorption equilibrium. This indicates the adsorption rate of the adsorbent for palladium ions in Pd(II) aqueous solution at adsorption equilibrium. This represents the concentration of palladium ions in the Pd(II) aqueous solution at the initial time. This represents the concentration of palladium ions in an aqueous Pd(II) solution at adsorption equilibrium. This represents the volume of the Pd(II) aqueous solution; This indicates the mass of the adsorbent.
[0050] The effects of different pH values on the adsorption rate and adsorption capacity of adsorbent Pd(II) were calculated and are shown in Table 1.
[0051] The adsorption capacity and adsorption rate data in Application Examples 1 to 14 were calculated using Equations (1) and (2), respectively, and the calculations used... , , and All values are measured and may contain random measurement errors that may exist between the adsorption capacity and adsorption rate data and the actual values.
[0052] Table 1. Effects of adsorbent on adsorption rate and adsorption capacity of Pd(II) at different pH values.
[0053] As shown in Table 1, the adsorption rate of palladium ions by the adsorbent generally increases with decreasing pH value; at pH 1, the maximum adsorption capacity of the adsorbent for palladium ions reaches 308.35 mg / g, and the adsorption rate is 96.23%.
[0054] Application Example 2: Prepare a 10.81 mg / L Pd(II) aqueous solution, then adjust the pH to 1 with a 0.1 mol / L hydrochloric acid solution. Measure 20 mL of the solution and add it to a 50 mL centrifuge tube. Then add 5 mg of the adsorbent prepared in Example 1 to the centrifuge tube containing the Pd(II) aqueous solution. Place the tube in a constant temperature water shaker at 25°C and shake. Take the upper palladium ion aqueous solution at different time levels, dilute it by the corresponding factor, and test the concentration of the remaining palladium ions using an atomic absorption spectrophotometer (AA-6680). The adsorption equilibrium point is when the concentration of the remaining palladium ions is at its lowest value. Calculate the corresponding adsorption capacity using equation (1) and the corresponding adsorption rate using equation (2). The calculation results show that for the Pd(II) aqueous solution, the adsorption equilibrium is reached in 1 min, and the corresponding adsorption rate is 99.97%. The adsorption capacity of the adsorbent at adsorption equilibrium is 43.24 mg / g.
[0055] Application Example 3: A 44.11 mg / L Pd(II) aqueous solution was prepared, and the pH was adjusted to 1 using a 0.1 mol / L hydrochloric acid solution. 20 mL of the solution was added to a 50 mL centrifuge tube, and 5 mg of the adsorbent prepared in Example 1 was added to the centrifuge tube. The tube was then shaken in a constant temperature water shaker at 25°C. The upper palladium ion aqueous solution was taken at different time points, diluted by the corresponding factor, and the remaining palladium ion concentration was tested using an atomic absorption spectrophotometer (AA-6680). The adsorption equilibrium point was reached when the remaining palladium ion concentration was at its lowest value. The corresponding adsorption capacity was calculated using equation (1), and the corresponding adsorption rate was calculated using equation (2). The calculation results show that for the Pd(II) aqueous solution, adsorption equilibrium was reached in 10 min, with a corresponding adsorption rate of 99.92%. The adsorption capacity of the adsorbent at adsorption equilibrium was 176.43 mg / g.
[0056] Application Example 4: Pd(II) aqueous solutions with pH=1 were prepared at concentrations of 10.76 mg / L, 47.80 mg / L, 62.14 mg / L, 84.89 mg / L, 105.52 mg / L, 160.65 mg / L, 214.13 mg / L, 353.82 mg / L, 403.13 mg / L, 462.88 mg / L, 496.97 mg / L, 550.00 mg / L, and 601.00 mg / L. 20 mL of each Pd(II) aqueous solution was transferred to a separate centrifuge tube, for a total of 13 centrifuge tubes. 5 mg of the adsorbent prepared in Example 1 was added to each of the centrifuge tubes. After sealing, the tubes were placed in a constant-temperature water shaker at 25°C and shaken for 72 h. After adsorption was complete, the upper palladium ion aqueous solution was taken, diluted by the corresponding factor, and the concentration of the remaining palladium ions was measured using an atomic absorption spectrophotometer (AA-6680). The corresponding adsorption capacity was calculated using equation (1), and the corresponding adsorption rate was calculated using equation (2). The results are shown in Table 2.
[0057] Table 2. Effects of different Pd(II) aqueous solution concentrations on the adsorption rate and adsorption capacity of Pd(II).
[0058] As shown in Table 2, the adsorption rate decreases with increasing concentration of Pd(II) aqueous solution, and the highest adsorption capacity of the adsorbent for Pd(II) is 534.64 mg / g.
[0059] Application Example 5: Pd(II) aqueous solutions with pH=1 were prepared at concentrations of 10.76 mg / L, 47.80 mg / L, 62.14 mg / L, 84.89 mg / L, 105.52 mg / L, 160.65 mg / L, 214.13 mg / L, 353.82 mg / L, 403.13 mg / L, 462.88 mg / L, 496.97 mg / L, 550.00 mg / L, and 601.00 mg / L. 20 mL of each Pd(II) aqueous solution was transferred to a separate centrifuge tube, for a total of 13 centrifuge tubes. 5 mg of the adsorbent prepared in Example 2 was added to each of the centrifuge tubes. After sealing, the tubes were placed in a constant-temperature water shaker at 25°C and shaken for 72 h. After adsorption was complete, the upper palladium ion aqueous solution was taken, diluted by the corresponding factor, and the concentration of the remaining palladium ions was measured using an atomic absorption spectrophotometer (AA-6680). The corresponding adsorption capacity was calculated using equation (1), and the corresponding adsorption rate was calculated using equation (2). The results are shown in Table 3.
[0060] Table 3. Effects of different Pd(II) aqueous solution concentrations on the adsorption rate and adsorption capacity of Pd(II).
[0061] As shown in Table 3, the adsorption rate decreases with increasing concentration of Pd(II) aqueous solution, and the highest adsorption capacity of the adsorbent for Pd(II) is 369.84 mg / g.
[0062] Application Example 6: Pd(II) aqueous solutions with pH=1 were prepared at concentrations of 10.76 mg / L, 47.80 mg / L, 62.14 mg / L, 84.89 mg / L, 105.52 mg / L, 160.65 mg / L, 214.13 mg / L, 353.82 mg / L, 403.13 mg / L, 462.88 mg / L, 496.97 mg / L, 550.00 mg / L, and 601.00 mg / L. 20 mL of each Pd(II) aqueous solution was transferred to a separate centrifuge tube, for a total of 13 centrifuge tubes. 5 mg of the adsorbent prepared in Example 3 was added to each of the centrifuge tubes. After sealing, the tubes were placed in a constant-temperature water shaker at 25°C and shaken for 72 h. After adsorption was complete, the upper palladium ion aqueous solution was taken, diluted by the corresponding factor, and the concentration of the remaining palladium ions was measured using an atomic absorption spectrophotometer (AA-6680). The corresponding adsorption capacity was calculated using equation (1), and the corresponding adsorption rate was calculated using equation (2). The results are shown in Table 4.
[0063] Table 4. Effects of different Pd(II) aqueous solution concentrations on the adsorption rate and adsorption capacity of Pd(II).
[0064] As shown in Table 4, the adsorption rate decreases with increasing concentration of Pd(II) aqueous solution, and the highest adsorption capacity of the adsorbent for Pd(II) is 170.22 mg / g.
[0065] Application Example 7: Pd(II) aqueous solutions with pH=1 were prepared at concentrations of 10.76 mg / L, 47.80 mg / L, 62.14 mg / L, 84.89 mg / L, 105.52 mg / L, 160.65 mg / L, 214.13 mg / L, 353.82 mg / L, 403.13 mg / L, 462.88 mg / L, 496.97 mg / L, 550.00 mg / L, and 601.00 mg / L. 20 mL of each Pd(II) aqueous solution was transferred to a separate centrifuge tube, for a total of 13 centrifuge tubes. 5 mg of the adsorbent prepared in Example 4 was added to each of the centrifuge tubes. After sealing, the tubes were placed in a constant-temperature water shaker at 25°C and shaken for 72 h. After adsorption was complete, the upper palladium ion aqueous solution was taken, diluted by the corresponding factor, and the concentration of the remaining palladium ions was measured using an atomic absorption spectrophotometer (AA-6680). The corresponding adsorption capacity was calculated using equation (1), and the corresponding adsorption rate was calculated using equation (2). The results are shown in Table 5.
[0066] Table 5. Effects of different Pd(II) aqueous solution concentrations on the adsorption rate and adsorption capacity of Pd(II).
[0067] As shown in Table 5, the adsorption rate decreases with increasing concentration of Pd(II) aqueous solution, and the highest adsorption capacity of the adsorbent for Pd(II) is 497.00 mg / g.
[0068] Application Example 8: Pd(II) aqueous solutions with pH=1 were prepared at concentrations of 10.76 mg / L, 47.80 mg / L, 62.14 mg / L, 84.89 mg / L, 105.52 mg / L, 160.65 mg / L, 214.13 mg / L, 353.82 mg / L, 403.13 mg / L, 462.88 mg / L, 496.97 mg / L, 550.00 mg / L, and 601.00 mg / L. 20 mL of each Pd(II) aqueous solution was transferred to a separate centrifuge tube, for a total of 13 centrifuge tubes. 5 mg of the adsorbent prepared in Example 5 was added to each of the centrifuge tubes. After sealing, the tubes were placed in a constant-temperature water shaker at 25°C and shaken for 72 h. After adsorption was complete, the upper palladium ion aqueous solution was taken, diluted by the corresponding factor, and the concentration of the remaining palladium ions was measured using an atomic absorption spectrophotometer (AA-6680). The corresponding adsorption capacity was calculated using equation (1), and the corresponding adsorption rate was calculated using equation (2). The results are shown in Table 6.
[0069] Table 6. Effects of different Pd(II) aqueous solution concentrations on the adsorption rate and adsorption capacity of Pd(II).
[0070] As shown in Table 6, the adsorption rate decreases with increasing concentration of Pd(II) aqueous solution, and the highest adsorption capacity of the adsorbent for Pd(II) is 402.16 mg / g.
[0071] Application Example 9: A mixed solution was prepared with an ion concentration ratio of Pd(II):heterogeneous ions = 10 mg / L: 100 mg / L. The heterogeneous ions included five types: divalent Zn(II), divalent Ni(II), divalent Cu(II), trivalent Fe(III), and divalent Cd(II), provided in the form of nitrates, with a molar ratio of 1:1:1:1:1. 20 mL of the mixed solution was transferred to a 50 mL centrifuge tube, and 5 mg of the adsorbent prepared in Example 1 was added. After sealing, the tube was placed in a constant-temperature water shaker at 25°C and shaken for 3 hours. After adsorption, the upper palladium ion aqueous solution was taken, diluted by the appropriate factor, and the remaining palladium ion concentration was measured using an atomic absorption spectrophotometer (AA-6680). The corresponding adsorption capacity was calculated using equation (1), and the corresponding adsorption rate was calculated using equation (2). The results showed that Pd(II) was completely adsorbed after 6 hours, while the adsorption rates for other impurity ions were as follows: Zn(II) 0%, Ni(II) 0%, Cu(II) 0%, and Fe(III) 2.22%. This demonstrates that the adsorbent prepared in Example 1 has excellent selectivity for palladium ions.
[0072] Application Example 10: Prepare an 80.11 mg / L Pd(II) aqueous solution. Take 7 centrifuge tubes and add 20 mL of Pd(II) aqueous solution to each centrifuge tube. Then, use 0.1 mol / L hydrochloric acid solution to adjust the pH value of the Pd(II) aqueous solution in each centrifuge tube to be 1, 2, 3, 4, 5, 6 and 7 respectively.
[0073] Add 5 mg of the adsorbent prepared in Example 2 to each centrifuge tube and shake in a constant temperature water shaker at 25°C for 24 h. After adsorption, take the upper palladium ion aqueous solution, dilute it by the corresponding factor, and test the concentration of the remaining palladium ions using an atomic absorption spectrophotometer (AA-6680). Calculate the corresponding adsorption capacity using equation (1) and the corresponding adsorption rate using equation (2). The results show that the adsorption rate of the adsorbent for palladium ions generally increases with decreasing pH value; at pH 1, the maximum adsorption capacity of the adsorbent for palladium ions reaches 181.78 mg / g, and the adsorption rate is 56.73%.
[0074] Application Example 11: Prepare an 80.11 mg / L Pd(II) aqueous solution. Take 7 centrifuge tubes and add 20 mL of Pd(II) aqueous solution to each centrifuge tube. Then, use 0.1 mol / L hydrochloric acid solution to adjust the pH value of the Pd(II) aqueous solution in each centrifuge tube to be 1, 2, 3, 4, 5, 6 and 7 respectively.
[0075] Add 5 mg of the adsorbent prepared in Example 3 to each centrifuge tube and shake in a constant temperature water shaker at 25°C for 24 h. After adsorption, take the upper palladium ion aqueous solution, dilute it by the corresponding factor, and test the concentration of the remaining palladium ions using an atomic absorption spectrophotometer (AA-6680). Calculate the corresponding adsorption capacity using equation (1) and the corresponding adsorption rate using equation (2). The results show that the adsorption rate of the adsorbent for palladium ions generally increases with decreasing pH value; at pH 1, the maximum adsorption capacity of the adsorbent for palladium ions reaches 96.00 mg / g, and the adsorption rate is 26.12%.
[0076] Application Example 12: Prepare an 80.11 mg / L Pd(II) aqueous solution. Take 7 centrifuge tubes and add 20 mL of Pd(II) aqueous solution to each centrifuge tube. Then, use 0.1 mol / L hydrochloric acid solution to adjust the pH value of the Pd(II) aqueous solution in each centrifuge tube to be 1, 2, 3, 4, 5, 6 and 7 respectively.
[0077] Add 5 mg of the adsorbent prepared in Example 4 to each centrifuge tube and shake in a constant temperature water shaker at 25°C for 24 h. After adsorption, take the upper palladium ion aqueous solution, dilute it by the corresponding factor, and test the concentration of the remaining palladium ions using an atomic absorption spectrophotometer (AA-6680). Calculate the corresponding adsorption capacity using equation (1) and the corresponding adsorption rate using equation (2). The results show that the adsorption rate of the adsorbent for palladium ions generally increases with decreasing pH value; at pH 1, the maximum adsorption capacity of the adsorbent for palladium ions reaches 166.06 mg / g, and the adsorption rate is 42.32%.
[0078] Application Example 13: Prepare an 80.11 mg / L Pd(II) aqueous solution. Take 7 centrifuge tubes and add 20 mL of Pd(II) aqueous solution to each centrifuge tube. Then, use 0.1 mol / L hydrochloric acid solution to adjust the pH value of the Pd(II) aqueous solution in each centrifuge tube to be 1, 2, 3, 4, 5, 6 and 7 respectively.
[0079] Add 5 mg of the adsorbent prepared in Example 5 to each centrifuge tube and shake in a constant temperature water shaker at 25°C for 24 h. After adsorption, take the upper palladium ion aqueous solution, dilute it by the corresponding factor, and test the concentration of the remaining palladium ions using an atomic absorption spectrophotometer (AA-6680). Calculate the corresponding adsorption capacity using equation (1) and the corresponding adsorption rate using equation (2). The results show that the adsorption rate of the adsorbent for palladium ions generally increases with decreasing pH value; at pH 1, the maximum adsorption capacity of the adsorbent for palladium ions reaches 166.32 mg / g, and the adsorption rate is 42.39%.
[0080] Application Example 14: 20 mL of a 202.83 mg / L Pd(II) aqueous solution was added to each of four centrifuge tubes. The pH of the Pd(II) aqueous solution in each centrifuge tube was adjusted to 1 using a 0.1 mol / L hydrochloric acid solution. 5 mg of the adsorbent prepared in Example 1 was added to each centrifuge tube. The four centrifuge tubes were then placed in a constant-temperature water shaker at 5℃, 15℃, 25℃, and 45℃ for 72 h. Another group was tested under the same conditions. After adsorption, the upper palladium ion aqueous solution was taken, diluted by the appropriate factor, and the concentration of the remaining palladium ions was measured using an atomic absorption spectrophotometer (AA-6680). The corresponding adsorption capacity was calculated using equation (1), and the corresponding adsorption rate was calculated using equation (2). The results are shown in Table 7.
[0081] Table 7 Results of the effect of temperature on adsorption rate and adsorption capacity
[0082] As shown in Table 7, the adsorption rate and adsorption capacity gradually increase with increasing adsorption temperature. When the temperature reaches 45℃, the adsorbent exhibits superior adsorption rate and adsorption capacity for palladium ions.
[0083] Analysis of the results from Application Examples 1 to 14 shows that, compared to the adsorbents prepared in Examples 2 to 5, the adsorbent prepared in Example 1 of this invention has a maximum adsorption capacity of 534.64 mg / g for Pd(II) and a maximum adsorption rate of 100% for Pd(II). Furthermore, the adsorbent prepared in Example 1 of this invention has a maximum adsorption rate of 100% for Pd(II), while its adsorption rates for Zn(II), Ni(II), and Cu(II) are 0%, and its adsorption rate for Fe(III) is 2.22%. This indicates that the adsorbent prepared in Example 1 of this invention exhibits high selectivity for Pd(II).
[0084] Furthermore, the adsorbent prepared in Example 1 of this invention exhibits relatively low adsorption capacity and adsorption rate for Pd(II). This is because HCCP-3,5-DAP is a cross-linked polyphosphazene adsorbent rich in nitrogen-rich active sites, including pyridine nitrogen, secondary amino groups, and primary amino groups. The adsorption of Pd(II) is primarily driven by coordination chelation, accompanied by electrostatic interactions and a weak reducing effect. Therefore, its adsorption capacity and adsorption rate are jointly regulated by four key factors: pH, adsorption temperature, adsorbent dosage, and the initial concentration of the Pd(II) aqueous solution. pH is the most crucial regulating factor; the peak adsorption performance for Pd(II) is reached at pH ≈ 1~2. Under moderately alkaline conditions, Pd(II) undergoes hydrolysis and precipitation, and OH... - Competition for active sites leads to a decrease in adsorption performance. Adsorption temperature mainly regulates performance through kinetic mass transfer and thermodynamic equilibrium. Within a reasonable range, increasing the temperature can accelerate the diffusion rate of Pd(II), promote the endothermic adsorption reaction to proceed in the forward direction, and expose more internal active sites, thereby simultaneously increasing adsorption capacity and adsorption rate. However, excessively high temperatures may cause a performance decline due to desorption or slight damage to the framework. Increasing the amount of adsorbent will increase the total number of active sites in the system, causing the adsorption rate to rise continuously and eventually plateau. However, the adsorption capacity per unit mass will continue to decrease due to the reduced saturation of active sites and the particle aggregation effect. Increasing the initial concentration of Pd(II) will increase the mass transfer driving force, driving the adsorption capacity to gradually increase until the active sites are completely saturated. However, the adsorption rate will gradually decrease due to the gradual filling of active sites and the enhanced interionic repulsion.
[0085] See Figures 1-6 The nitrogen-enriched phosphazene polymer adsorbent HCCP-3,5-DAP has a spherical structure with uniform distribution of C, N, P and Cl elements.
[0086] See Figures 7-13 After adsorbing Pd(II), HCCP-3,5-DAP still maintains its original spherical morphology, with C, N, P and Cl elements uniformly distributed, and Pd uniformly loaded on the surface of HCCP-3,5-DAP.
[0087] Depend on Figure 14 This indicates that HCCP-3,5-DAP has a low specific surface area of 1.13 m². 2 / g, with an average pore size of approximately 44.92nm.
[0088] Depend on Figure 15 Infrared spectroscopy showed that after HCCP reacted with 3,5-DAP, it was located at 3324 cm⁻¹. -1 and 3182cm -1 The primary amine NH stretching vibration peak disappears at 1010 cm⁻¹. -1The appearance of a new CNP stretching vibration peak confirms the successful crosslinking of HCCP-3,5-DAP.
[0089] exist Figure 16 In the XRD pattern, HCCP-3,5-DAP showed broad and diffuse diffraction peaks, indicating that it is an amorphous structure; no obvious crystal diffraction peaks were found in the pattern of Pd@HCCP-3,5-DAP (i.e., HCCP-3,5-DAP after adsorption of Pd(II)), indicating that the adsorbed Pd(II) did not form a crystalline phase, but existed in a highly dispersed state on the support.
[0090] The adsorption-desorption cycle performance of HCCP-3,5-DAP for Pd(II) was investigated using an atomic absorption spectrometer (AA-6680, Shimadzu Corporation, Japan). Specifically, 60 mg of HCCP-3,5-DAP was weighed and uniformly dispersed in 100 mL of a 20.39 mg / L Pd(II) aqueous solution. Adsorption was carried out by shaking at 25 °C and 230 rpm for 12 h. After filtration, the supernatant was used to determine the residual Pd(II) concentration using AAS. Subsequently, the adsorbed HCCP-3,5-DAP was immersed in an equal volume of a desorption solution of 0.5 mol / L thiourea and 1 mol / L nitric acid for 8 h. After washing with deionized water and freeze-drying (at -10 °C for 24 h), the regenerated adsorbent was reintroduced into the same Pd(II) aqueous solution for the next adsorption cycle. This process was repeated multiple times. The results are shown below. Figure 17 As shown, HCCP-3,5-DAP exhibits good cyclic stability.
[0091] The above description is only a preferred embodiment of the present invention and does not limit the scope of the present invention. All equivalent structural transformations made under the inventive concept of the present invention using the contents of the present invention specification and drawings, or direct / indirect applications in other related technical fields, are included within the protection scope of the present invention.
Claims
1. A method for preparing a nitrogen-enriched phosphazene polymer adsorbent, characterized in that, include: The prepared phosphazene compound solution and heterocyclic diamine compound solution were mixed and an organic alkali solution was added. After mixing, the mixture underwent polymerization and post-treatment to obtain a nitrogen-enriched phosphazene polymer adsorbent. The molar ratio of the phosphazene compound in the phosphazene compound solution to the heterocyclic diamine compound in the heterocyclic diamine compound solution is 1:1 to 1:
3. The volume ratio of the phosphazene compound solution, the heterocyclic diamine compound solution, and the organic alkali solution is 5:5:6.
5.
2. The preparation method of the nitrogen-enriched phosphazene polymer adsorbent as described in claim 1, characterized in that, The mass ratio of the phosphazene compound used in the phosphazene compound solution to the volume ratio of the first organic solution is 0.0695 g: 2 mL; The phosphazene compound includes hexachlorophosphazene; the organic alkaline solution includes triethylamine; The first organic solution includes at least one of tetrahydrofuran, N,N-dimethylformamide, and acetonitrile.
3. The preparation method of the nitrogen-enriched phosphazene polymer adsorbent as described in claim 1, characterized in that, The mass ratio of the heterocyclic diamine compound used in the heterocyclic diamine compound solution to the volume ratio of the second organic solution is 0.0649~0.0661g:3mL; The heterocyclic diamine compound includes at least one of m-phenylenediamine, 2,6-diaminopyridine, 3,5-diaminopyridine, 2,4-diaminopyridine, and 4,6-diaminopyrimidine; The second organic solution includes at least one of tetrahydrofuran, N,N-dimethylformamide, and acetonitrile.
4. The method for preparing the nitrogen-enriched phosphazene polymer adsorbent as described in claim 1, characterized in that, The polymerization reaction was carried out at a temperature of 180°C for 3 hours.
5. The method for preparing the nitrogen-enriched phosphazene polymer adsorbent as described in claim 1, characterized in that, The post-processing includes centrifugation, washing, and freeze-drying in sequence; the centrifugation is performed at a speed of 5000 r / min for 5 min; the washing process involves washing the precipitate after centrifugation with ethanol and ultrapure water in sequence; the freeze-drying process is performed at a temperature of -10℃ for 24 h.
6. A nitrogen-enriching phosphazene polymer adsorbent, characterized in that, It is prepared by the method described in any one of claims 1 to 5 for preparing nitrogen-enriched phosphazene polymer adsorbents.
7. An application of the nitrogen-enriched phosphazene polymer adsorbent as described in claim 6 in the adsorption of palladium ions, characterized in that, The nitrogen-enriched phosphazene polymer adsorbent is added to acidic wastewater containing palladium ions to carry out an adsorption reaction and recover palladium ions. The mass ratio of the nitrogen-enriched phosphazene polymer adsorbent to the volume of the palladium-containing acidic wastewater is 0.002~2g:3~3000mL; The concentration of palladium ions in the acidic wastewater containing palladium ions is not higher than 610 mg / L; The acidic substance used in the palladium-containing acidic wastewater includes hydrochloric acid solution; the concentration of the hydrochloric acid solution is 0.1~1 mol / L. The pH value of the acidic wastewater containing palladium ions is 1; The adsorption reaction was carried out at an adsorption temperature of 25°C for a time of 1 min to 72 h.
8. The application of the nitrogen-enriched phosphazene polymer adsorbent as described in claim 7 in the adsorption of palladium ions, characterized in that, The mass ratio of the nitrogen-enriched phosphazene polymer adsorbent to the volume of the palladium-containing acidic wastewater is 0.005~1g:30~300mL. The concentration of palladium ions in the acidic wastewater containing palladium ions is 10~500 mg / L; The concentration of the hydrochloric acid solution is 0.1~0.5 mol / L.
9. The application of the nitrogen-enriched phosphazene polymer adsorbent as described in claim 7 in the adsorption of palladium ions, characterized in that, The nitrogen-enriched phosphazene polymer adsorbent achieves an adsorption rate of up to 100% for palladium ions in the acidic wastewater containing palladium ions. The nitrogen-enriched phosphazene polymer adsorbent exhibits an adsorption capacity of up to 534.64 mg / g for palladium ions in the acidic wastewater containing palladium ions.
10. The application of the nitrogen-enriched phosphazene polymer adsorbent as described in claim 8 in the adsorption of palladium ions, characterized in that, After adsorbing the palladium ions, the process further includes solid-liquid separation and desorption regeneration to obtain a reusable nitrogen-enriched phosphazene polymer adsorbent. The desorbent used in the desorption and regeneration includes a desorption solution containing thiourea and / or nitric acid; in the desorption solution, the molar concentration of thiourea is 0.5 mol / L and the molar concentration of nitric acid is 1 mol / L. The desorption and regeneration process uses a desorption temperature of 25°C and a desorption time of 8 hours.