A catalytic system for the depolymerization of a polymer containing diol structural units to prepare ethylene and its application.
By using an iodine-containing compound and hydrogen catalytic system under metal-free conditions, highly selective depolymerization of polyester plastics into ethylene was achieved, solving the problems of low conversion efficiency and lengthy process in existing technologies, and realizing efficient and economical ethylene production.
Patent Information
- Application Number
- CN202611264018.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to convert polyester plastics into ethylene with high selectivity under mild conditions, and existing catalytic systems rely on metal catalysts, resulting in lengthy processes and low atom economy.
A catalytic system composed of iodine-containing compounds and hydrogen is used to depolymerize polyester to generate ethylene through hydrolysis, iodination and elimination reactions under metal-free conditions. The iodine generated by hydrogen reduction is then recycled to utilize the catalyst.
It achieves highly selective conversion of polyester materials into ethylene with high yield and selectivity, simplifies the process, reduces energy consumption, and broadens the scope of chemical recycling of waste plastics.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid waste resource utilization, specifically to a catalytic system for the depolymerization of polymers containing diol structural units to prepare ethylene and its application. Background Technology
[0002] Plastic products are widely used in daily consumer goods and industrial production due to their excellent properties. However, the vast majority of plastic products are discarded after their lifespan, and the current mainstream incineration and landfill disposal methods not only waste resources but also cause environmental pollution. Chemically, waste plastics are mainly composed of carbon and hydrogen elements, with some varieties containing oxygen heteroatoms. The bonding structure and monomer units in their polymer chains share intrinsic similarities with lignocellulosic biomass, possessing the potential to replace fossil fuels and be converted into liquid fuels or fine chemicals. Through resource recovery methods such as directed catalytic conversion, the selective transformation of waste plastics into high-value products can be achieved, providing a feasible pathway for solid waste pollution control.
[0003] Among various polyester plastics, polyethylene terephthalate (PET) has the largest production volume and the widest application, making it a key target for plastic pollution control. PET hardly biodegrades in natural environments, and traditional mechanical recycling processes lead to molecular chain breakage, deteriorating the mechanical properties of recycled products and making recycling difficult. Chemical recycling routes depolymerize PET into monomers such as terephthalic acid (TPA) and ethylene glycol (EG) through reactions such as hydrolysis and alcoholysis, but existing catalytic systems have significant limitations.
[0004] EG, as a bulk chemical, has limited added value and is not economically viable. Ethylene, on the other hand, is an important basic olefin platform compound, widely used in downstream materials such as polyethylene and ethylene oxide. While converting EG to ethylene via multiple steps is theoretically feasible, the process is lengthy and has low atom economy. Currently, industrial ethylene production mainly relies on petroleum or ethane steam cracking, resulting in high energy consumption and a large carbon footprint. Therefore, researching methods for depolymerizing polyester and converting it to ethylene has significant scientific and practical value.
[0005] Patent document CN104774154A discloses a method for the depolymerization of polyethylene terephthalate using a superbase ionic liquid as a catalyst. The method uses a diol as a solvent and a superbase ionic liquid as a catalyst to depolymerize the polyethylene terephthalate. The mechanism focuses on the accelerated kinetics of the breakage between the diol and the terephthalate, but the products are monomers such as BHET or TPS, without involving further directional conversion to olefins.
[0006] Patent document CN122145296A discloses a method for preparing various organic acids by depolymerization of polyester and its application. The method involves mixing polyester material, a metal catalyst, an iodine-containing catalytic aid, and a solvent, then introducing carbon monoxide to obtain various organic acids. However, the depolymerization process relies on a metal catalyst, and the product is an organic acid.
[0007] Among the aforementioned existing technologies, some studies rely on transition metal catalysts, and none of them involve the highly selective conversion of polyester diol structural units to ethylene. Therefore, constructing a catalytic system synergistically combining iodine-containing compounds and hydrogen donors to achieve the direct and highly selective depolymerization of PET to ethylene under mild conditions possesses both scientific innovation and industrial application value. Summary of the Invention
[0008] This invention addresses the need for targeted upgrading of waste polyester plastics and the thermodynamic limitations that cannot be overcome in existing chemical depolymerization processes. It provides a catalytic system for depolymerizing polymers containing glycol structural units, and a method for preparing ethylene by iodine-containing catalytic depolymerization of polyester or polyethylene glycol using the catalytic system. This achieves highly selective depolymerization of polyester materials and targeted preparation of ethylene without the need for metal catalysts, and has good application prospects in the treatment of waste polyester plastics.
[0009] A catalytic system for the depolymerization of a polymer containing diol structural units, wherein the polymer comprises polyester and polyethylene glycol, and the catalytic system comprises an iodine-containing compound, hydrogen gas, and a solvent, wherein the molar ratio of the iodine-containing compound to the hydrogen gas is 1:(5-35).
[0010] Preferably, the polyester comprises polyethylene terephthalate, polyethylene naphthalate, polyethylene succinate, or polyethylene adipate.
[0011] Preferably, the iodine-containing compound is one or more of hydroiodic acid, elemental iodine, zinc iodide, and sodium iodide.
[0012] Preferably, the solvent is acetic acid or propionic acid. Acetic acid and propionic acid are polar organic acids that are miscible with water and iodine-containing compounds, ensuring that the reaction system is homogeneous and facilitating the dispersion and mass transfer of iodide ions; at the same time, they have good solubility for polymer depolymerization intermediates, which can further improve the reaction efficiency.
[0013] Preferably, the molar ratio of the iodine-containing compound to hydrogen is 1:(9-24). Further controlling the molar ratio of the iodine-containing compound to hydrogen within an appropriate range ensures that the hydrogen concentration is sufficient to maintain the iodide ion concentration, promoting the depolymerization reaction of the polymer and the iodination process of ethylene glycol and its derivatives. Simultaneously, it inhibits the side reaction of excessive hydrogenation of ethylene to ethane, thereby promoting the conversion of the polymer to ethylene.
[0014] This invention also provides a method for preparing ethylene by iodine-containing catalytic depolymerization of polyester or polyethylene glycol using the above-described catalytic system, comprising: Ethylene and the corresponding organic acid are prepared by reacting polyester or polyethylene glycol with the catalytic system at 150-190 °C for 0.25-10 h.
[0015] Taking polyester materials as an example, under heating and a hydrogen atmosphere, the depolymerization reaction of polyester materials is coupled with the iodination-elimination reaction of the depolymerization products. Simultaneously, hydrogen can reduce the iodine generated in the elimination reaction in situ, enabling the polyester repeating units in the reaction system to be completely converted into ethylene and organic acid monomers in one step, ensuring the continuous and efficient progress of the reaction and overcoming thermodynamic limitations. Specifically, the iodine-containing catalyst mediates the iodination and elimination reactions of the depolymerized monomers to generate ethylene, while hydrogen reduces the iodine generated in the elimination reaction, allowing the reaction to continue in a continuous cycle.
[0016] The specific reaction principle is as follows: In the initial stage of the reaction, the polyester undergoes hydrolysis under the catalysis of an iodine-containing compound, such as hydroiodic acid, to generate ethylene glycol and organic carboxylic acid monomers. Using acetic acid as a solvent, ethylene glycol undergoes an esterification equilibrium reaction with acetic acid, partially generating ethylene glycol esterification derivatives (ethylene glycol diacetate and 2-hydroxyethyl acetate). Further, the iodine-containing compound releases iodide ions, where elemental iodine is reduced by hydrogen gas to generate hydrogen iodide. Iodide ions, acting as nucleophiles, simultaneously undergo nucleophilic substitution reactions with the reactive sites (hydroxyl or ester groups) of ethylene glycol and its derivatives, generating 2-iodoethanol and 2-acetoxyiodoethane. At least one of these two intermediates can be further converted to diiodoethane, and ultimately undergoes a dehalogenation reaction to generate ethylene. Through this pathway, the polyester carbon chain is effectively broken down, while the iodine component is recycled, thus enabling the continuous progress of the catalytic depolymerization process.
[0017] The specific reaction process is as follows: (1) Esterification equilibrium reaction: (2) Primary iodination reaction: (3) Secondary iodination reaction: (4) Dehalogenation reaction: Preferably, the heating temperature is 170~180 ℃, and the reaction time is 4~8 h. When the heating temperature is higher than 170 ℃ and the reaction time is greater than 4 h, the polyester or polyethylene glycol can be completely depolymerized, the concentration of ethylene glycol monomer in the reaction process is high, and the ethylene glycol iodide dehalogenation to ethylene reaction can proceed efficiently.
[0018] Preferably, the molar ratio of the iodine-containing compound to the repeating unit in the diol-containing polymer is 0.01 to 0.5:1.
[0019] More preferably, the molar ratio of the iodine-containing compound to the repeating unit in the glycol-containing polymer is 0.4~0.5:1. As a key nucleophile catalyzing the depolymerization of the glycol-containing polymer and the iodination-dehalogenation of ethylene glycol, when the molar ratio of the iodine-containing compound to the repeating unit in the glycol-containing polymer is within the aforementioned range, the iodide ion concentration in the reaction system is sufficient, which can promote the depolymerization of the glycol-containing polymer and the iodination reaction of ethylene glycol and its derivatives, inhibit side reactions, and thus improve the yield and selectivity of ethylene.
[0020] Preferably, when the polyester material is polyethylene terephthalate, the product is ethylene and terephthalic acid; when the polyester material is polyethylene naphthalate, the product is ethylene and 2,6-naphthalic acid; when the polymer is polyethylene glycol, the product is ethylene; when the polyester material is polyethylene succinate, the product is ethylene and succinic acid; when the polyester material is polyethylene adipate, the product is ethylene and adipic acid.
[0021] The present invention also provides the application of the above-mentioned catalytic system in the chemical recycling treatment of waste polyester or polyethylene glycol waste liquid.
[0022] The waste polyester includes PET bottle flakes, polyester fibers, polyester films, or polyester-based composite materials. The waste polyester is pre-crushed into flakes, granules, or powder before processing.
[0023] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) This invention does not require a metal catalyst. A catalytic system consisting of an iodine-containing catalyst, hydrogen, and a solvent can be used to achieve the depolymerization of polyester or polyethylene glycol and the conversion of the depolymerization products. Under the action of the iodine-containing catalyst, the depolymerization product ethylene glycol undergoes iodination and elimination reactions to generate ethylene. Hydrogen promotes the regeneration of iodine-containing active species during the reaction, enabling the iodine-containing catalytic system to function cyclically, thereby avoiding the termination of the reaction due to the consumption of iodine species and improving the sustainability of the conversion of ethylene glycol structural units to ethylene. Taking PET as an example, the yield of terephthalic acid (TPA) obtained from its conversion can reach 100%, the yield of ethylene can reach more than 94%, and the ethylene selectivity can reach 96%.
[0024] (2) This invention is applicable to the directional depolymerization and conversion of various polyester waste plastics, such as various PET sealed cans, PET transparent films, PET cups, PET woven belts, PET bottles, and fabrics with different PET contents. It can achieve efficient directional conversion and produce ethylene with high yield. The method and process are simple and economically efficient. It realizes the green and high-value utilization of polyester materials and chemical recycling, and reduces the potential negative impact on the environment during the ethylene production process.
[0025] (3) The present invention can also process a variety of polymer materials containing diol structural units, including polyethylene terephthalate, polyethylene naphthalate, polyethylene succinate, polyethylene glycol or polyethylene glycol oxalate, etc., which broadens the scope of waste plastic chemical recycling materials. Under the premise of ensuring high depolymerization efficiency and rapid reaction time, the corresponding conversion can be completed to obtain the platform compound ethylene. Detailed Implementation
[0026] To make the objectives, features, and advantages of this invention more apparent and understandable, a detailed description is provided below through specific embodiments. Many specific details are set forth in the following description to provide a thorough understanding of the invention. However, the invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below. Technical features in various embodiments of the invention can be combined appropriately without mutual conflict.
[0027] Unless otherwise specified, the operating methods in the following examples are generally performed under conventional conditions or as recommended by the manufacturer. Contents not described in detail in this specification are prior art known to those skilled in the art. Unless otherwise specified, the experimental materials used in the examples below can be purchased from conventional biochemical reagent companies.
[0028] Example 1 PET powder with 2 mmol repeating units, 0.8 mmol hydroiodic acid, and 3 mL acetic acid were added to an autoclave reactor equipped with an electromagnetic stirrer, thermocouple, and programmable temperature controller. The autoclave reactor was then closed and hydrogen gas was introduced to achieve a molar ratio of hydroiodic acid to hydrogen of 1:19. After placing the autoclave reactor in place, stirring and heating were started. The reaction system was heated to 180 °C and reacted at this temperature for 5 h. After the reaction was completed, the mixture was cooled to room temperature, headspace gas was collected, and the ethylene yield was determined by GC. The resulting mixture was allowed to stand, and the precipitate was collected. An appropriate amount of 2 mmol / L NaOH was added, with deuterium water as the deuteration reagent and sodium fumarate as the internal standard. The precipitate was then analyzed by liquid chromatography. 1¹H NMR determination of terephthalic acid yield. Results showed that in this example, the PET decomposition rate was 100%, and the TPA yield was 100%. The NMR data for terephthalic acid are as follows: 1 H NMR (500 MHz, D2O) δ 7.89 (s, 4H), ethylene yield 94%.
[0029] The reaction equation in this embodiment is as follows: Example 2-14 The only difference between Examples 2-14 and Example 1 is that the PET powder was replaced with an equal mass of PET waste (the corresponding PET waste was crushed to the centimeter level beforehand). All other reaction conditions and steps were the same as in Example 1. The results are shown in Table 1.
[0030] Table 1. Depolymerization effect of different PET wastes Examples 15-18 The only difference between Examples 15-18 and Example 1 is that the PET powder was replaced with equimolar amounts of polyethylene naphthalate powder, polyethylene glycol powder, polyethylene succinate powder, and polyethylene adipate powder, respectively. All other reaction conditions and steps were the same as in Example 1. The results are shown in Table 2.
[0031] Table 2. Depolymerization effect of polymers containing different diol structural units Examples 19-21 The only difference between Examples 19-21 and Example 1 is that the iodide-containing compounds were replaced with equimolar amounts of elemental iodine, a mixture of hydroiodic acid and zinc iodide, and a mixture of hydroiodic acid and sodium iodide, respectively. All other reaction conditions and steps were the same as in Example 1. The results are shown in Table 3.
[0032] Table 3. Depolymerization effect of PET under different iodine-containing compound conditions Example 22 The only difference between Example 22 and Example 1 is that the solvent acetic acid was replaced with an equal volume of propionic acid. All other reaction conditions and steps were the same as in Example 1. The results are shown in Table 4.
[0033] Table 4. Depolymerization effect of PET under different solvent conditions Examples 23-25 The only difference between Examples 23-25 and Example 1 is that the amount of hydroiodic acid added is 0 mmol, 0.5 mmol, and 1 mmol, respectively. All other reaction conditions and steps are the same as in Example 1. The results are shown in Table 5.
[0034] Table 5. Depolymerization effect of PET under different molar amounts of hydroiodic acid Examples 26-30 The only difference between Examples 26-30 and Example 1 is that after hydrogen gas is introduced, the molar ratio of hydroiodic acid to hydrogen is 1:0, 1:9, 1:13, 1:16, and 1:24, respectively. All other reaction conditions and steps are the same as in Example 1. The results are shown in Table 6.
[0035] Table 6. Depolymerization effect of PET under different hydrogen molar amounts Examples 31-34 The only difference between Examples 31-34 and Example 1 is that the reaction temperatures were set to 150℃, 160℃, 170℃, and 190℃, respectively. All other reaction conditions and steps were the same as in Example 1. The results are shown in Table 7.
[0036] Table 7. Depolymerization effect of PET at different reaction temperatures Examples 35-43 The only difference between Examples 35-43 and Example 1 is that the reaction times were set to 0.25 h, 0.5 h, 0.75 h, 1 h, 2 h, 3 h, 4 h, 8 h, and 10 h, respectively. All other reaction conditions and steps were the same as in Example 1. The results are shown in Table 8.
[0037] Table 8. Depolymerization effect of PET at different reaction times Examples 23 and 26 correspond to the cases where no iodine-containing compound is added to the reaction system and the cases where no hydrogen is added, respectively. Compared with the product distribution of Example 1, it can be seen that when no iodine-containing compound is added to the reaction system, the polyester material hardly undergoes a depolymerization reaction, the TPA yield is only 6%, and the generation of ethylene glycol depolymerization monomers is also limited, so the ethylene yield in the product is only 1%. When no hydrogen is added to the reaction system, the polyester material still undergoes a depolymerization reaction, and the TPA yield in the product can reach 84%, but the ethylene yield is only 9%. This shows that without hydrogen participating in the reaction, the iodine-containing compound in the system becomes ineffective after participating in the iodination reaction of the ethylene glycol depolymerization monomers and cannot be reused, which greatly reduces the final yield of the reaction product.
[0038] Therefore, only a catalytic system composed of iodine-containing compounds and hydrogen can be used to depolymerize PET materials, thus realizing the cyclic process of polyester depolymerization-iodination elimination-iodine reduction.
[0039] The embodiments described above provide a detailed explanation of the technical solutions of the present invention. It should be understood that the above descriptions are merely specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, additions, or similar substitutions made within the scope of the principles of the present invention should be included within the scope of protection.
Claims
1. A catalytic system for the depolymerization of a polymeric material comprising diol structural units, said polymeric material comprising a polyester and polyethylene glycol, characterized in that, The catalytic system comprises an iodine-containing compound, hydrogen gas, and a solvent, wherein the molar ratio of the iodine-containing compound to hydrogen gas is 1:(5-35).
2. In the catalytic system according to claim 1, the molar ratio of the iodine-containing compound to hydrogen is 1:(9-24).
3. The catalytic system according to claim 1, characterized in that, The polyester comprises polyethylene terephthalate, polyethylene naphthalate, polyethylene succinate, or polyethylene adipate.
4. The catalytic system according to claim 1, characterized in that, The iodine-containing compound is one or more of hydroiodic acid, elemental iodine, zinc iodide, or sodium iodide.
5. The catalytic system according to claim 1, characterized in that, The solvent is acetic acid or propionic acid.
6. A method for preparing ethylene by iodine-containing catalytic depolymerization of polyester or polyethylene glycol using the catalytic system according to any one of claims 1-5, comprising: Ethylene is prepared by reacting polyester or polyethylene glycol with the catalytic system at 150-190 °C for 0.25-10 h.
7. The method for preparing ethylene by iodine-containing catalytic depolymerization of polyester or polyethylene glycol according to claim 6, characterized in that, In the catalytic system, the molar ratio of the iodine-containing compound to the repeating unit in the diol-containing polymer is 0.01~0.5:
1.
8. The method for preparing ethylene by iodine-containing catalytic depolymerization of polyester or polyethylene glycol according to claim 6, characterized in that, The heating temperature is 170-180 ℃, and the heating time is 4-8 h.
9. The application of the catalytic system according to any one of claims 1-5 in the treatment of waste polyester or polyethylene glycol waste liquid.
10. The application according to claim 9, characterized in that, The waste polyester includes PET bottle flakes, polyester fibers, polyester films, or polyester-based composite materials.
Citation Information
Patent Citations
Method for catalytic alcoholysis of polyethylene glycol terephthalate with super-strong alkaline ionic liquid
CN104774154A
Method for preparing various organic acids through polyester depolymerization and application thereof
CN122145296A