A formula for a porous ceramic clay filter material that can efficiently decompose pesticide residues in tea.
The porous kaolin filter material with a multi-level pore structure and visible light catalysis system solves the problems of low degradation efficiency of pesticide residues in tea soup and loss of tea soup flavor, achieving a balance between efficient pesticide residue removal and flavor preservation.
Patent Information
- Application Number
- CN202611215177.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-12
- Publication Date
- 2026-11-17
AI Technical Summary
Existing ceramic filter materials suffer from low ultraviolet light utilization, high photogenerated electron-hole pair recombination rate, and uniform pore size distribution when removing pesticide residues from tea, resulting in low degradation efficiency and severe loss of tea flavor.
A porous ceramic filtration material with a hierarchical porous structure, hydrophobic targeted interface construction, and synergistic visible light catalysis and enzyme catalysis is used to selectively enrich and efficiently degrade pesticide molecules through hydrophobic silanization modification, covalent immobilization of enzymes, and sensitization of TiO2 with tea polyphenol carbon dots.
It efficiently degrades pesticide residues in tea soup under visible light, retains a high rate of tea polyphenols, and possesses excellent stability and recyclability, thus improving the drinking quality of tea soup.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of ceramic filter material technology, specifically a formula for a porous ceramic clay filter material that can efficiently decompose pesticide residues in tea. Background Technology
[0002] As a traditional Chinese beverage, the quality and safety of tea are directly related to consumers' health. During tea cultivation, the use of chemical pesticides such as organochlorines, organophosphates, pyrethroids, and carbamates is unavoidable for pest and disease control. Some of these pesticide residues remaining in the dry tea leaves migrate into the tea infusion during brewing. Long-term ingestion of pesticide residues in tea poses potential harm to the human nervous, endocrine, and immune systems, and has become a significant factor hindering the high-quality development of the tea industry.
[0003] Currently, the mainstream methods for removing pesticide residues from tea infusion mainly fall into two categories: adsorption and chemical degradation. Common adsorbents used in adsorption include activated carbon and macroporous adsorption resins. However, activated carbon has poor adsorption selectivity, adsorbing beneficial components such as tea polyphenols and amino acids along with pesticides, leading to a significant decline in the flavor and quality of the tea. Macroporous adsorption resins have complex regeneration processes and high costs, and only achieve the physical transfer of pesticides rather than true degradation. Chemical degradation methods, such as photocatalytic oxidation and ozone oxidation, can achieve complete decomposition of pesticides, but the operating conditions are harsh, and some oxidation processes may produce more toxic intermediate products. Although porous ceramic materials possess good chemical stability, mechanical strength, and regeneration performance, existing ceramic filter materials mainly rely on physical interception and adsorption to remove pollutants, lacking the ability to actively decompose pesticide molecules.
[0004] More importantly, the existing technologies face the following common technical challenges: (1) Traditional nano-TiO2 photocatalysts can only be excited under ultraviolet light (λ<387nm), resulting in extremely low utilization of indoor and visible light, which limits the practical application scenarios of filter materials; (2) The single TiO2 system has a high recombination rate of photogenerated electron-hole pairs, low quantum efficiency, and slow degradation rate; (3) Existing ceramic filter materials have a single pore size distribution, which cannot achieve hierarchical retention and synergistic removal of pesticide molecules of different sizes. Therefore, developing a porous kaolin filter material that combines visible light response, high photocatalytic quantum efficiency, gradient multi-level pore structure, and antibacterial function has significant technical value and market prospects. Summary of the Invention
[0005] The purpose of this invention is to provide a porous kaolin filter material and its preparation method that can efficiently decompose pesticide residues in tea soup. Through multiple technological innovations such as multi-level pore structure regulation, hydrophobic targeted interface construction, synergistic visible light catalysis and enzyme catalysis, and covalent immobilization, it achieves both efficient pesticide residue removal and high flavor retention, while also possessing excellent stability and recyclability.
[0006] The objective of this invention can be achieved through the following technical solutions: A method for preparing a porous kaolin filter material that can efficiently decompose pesticide residues in tea infusion includes the following steps: Step 1: Using kaolin, quartz sand, bentonite, and tourmaline powder as the composite porcelain clay matrix, coal powder pore-forming agent and polyacrylamide binder are added, and the mixture is ball-milled, aged, pressed, and sintered at a stepped temperature to obtain a multi-level porous porcelain clay carrier with a multi-level pore structure.
[0007] Step 2: The multi-level porous kaolin carrier is modified with hydrophobic silanization, and then a vacuum impregnation-in-situ hydrolysis process is used to immobilize tea polyphenols and nano-titanium dioxide on the inner wall of the pores. After low-temperature curing, a carrier loaded with visible photocatalytic phase is obtained.
[0008] Step 3: Using a silane coupling agent covalent grafting process, the compound degradation enzyme is immobilized in the pores of a carrier loaded with a visible light catalytic phase, and then dried at low temperature to obtain a porous ceramic clay filter material.
[0009] Furthermore, the specific preparation steps of the multi-level porous porcelain clay carrier are as follows: Kaolin, quartz sand, bentonite, and tourmaline powder are fed into a ball mill, along with deionized water and polyacrylamide binder. The mixture is ball-milled at 300-400 r / min for 40-60 min to obtain a uniform slurry. Coal powder pore-forming agent is added, and the mixture is ball-milled for another 20-30 min. The slurry is then injected into a custom mold and pressed into shape at 8-12 MPa. After aging at room temperature for 12-24 h, it is dried at 80-100℃ for 6-8 h. Subsequently, it is sintered in a muffle furnace with stepped heating, and after natural cooling, a multi-level porous porcelain clay carrier is obtained.
[0010] Furthermore, the mass ratio of kaolin, quartz sand, bentonite, and tourmaline powder is 60-70:15-20:10-15:3-8; the amount of polyacrylamide binder added is 2-4% of the total mass of the kaolin, the amount of coal powder pore-forming agent added is 8-15% of the total mass of the kaolin, and the liquid-solid ratio is 0.6-0.8:1; Furthermore, the stepped heating sintering process is as follows: heat to 400-500℃ at 2-3℃ / min and hold for 1-2 hours to remove organic matter, continue to heat to 1150-1250℃ at 3-5℃ / min and hold for 2-3 hours for vitrification, and then cool down to 600℃ at 1-2℃ / min and allow to cool naturally.
[0011] Furthermore, the specific steps for supporting the visible light photocatalytic phase are as follows: A hierarchical porous ceramic support was immersed in a 5-10% (v / v) octyltriethoxysilane ethanol solution for 2-4 hours at room temperature. After immersion, the support was removed and cured at 100-120℃ for 1-2 hours to complete the hydrophobic silanization modification of the pores. Subsequently, the support was immersed in a tetrabutyl titanate precursor solution containing tea polyphenol carbon dots for 30-50 minutes under a vacuum of -0.08 to -0.09 MPa. After removal, the support was placed in an ammonia atmosphere at 25-30℃ for hydrolysis and curing for 2-4 hours, and then calcined at 400-450℃ for 1-2 hours to obtain a support loaded with a visible photocatalytic phase.
[0012] Furthermore, the tea polyphenol carbon dots were prepared from tea extract via a hydrothermal method, with a particle size of 2-6 nm; the final TiO2 loading was 3-6% of the mass of the kaolin carrier, and the tea polyphenol carbon doping amount was 1-3% of the mass of TiO2; after hydrophobic silanization modification, the water contact angle of the pores was 95°-115°.
[0013] Furthermore, the specific steps for covalent immobilization of the degradation enzyme are as follows: The carrier loaded with the visible light catalytic phase was immersed in a γ-aminopropyltriethoxysilane buffer solution with a pH of 7.0-7.5 and activated at 30-40℃ for 2-3 hours to introduce amino active sites. After washing, it was transferred to a compound degrading enzyme solution with a pH of 6.5-7.0 and covalently grafted at 4℃ for 12-16 hours. After removal, it was rinsed with buffer solution to remove free enzymes and dried at a low temperature of 40-50℃ to obtain a porous ceramic filtration material.
[0014] Furthermore, the compound degrading enzyme is a mixture of laccase and acid phosphatase in a mass ratio of 1:1-2; the final immobilization amount of the degrading enzyme is 0.3-0.8% of the mass of the kaolin carrier.
[0015] Furthermore, the porous kaolin filter material exhibits a three-level pore size distribution: macropores (50-200 μm), mesopores (2-50 nm), and micropores (<2 nm), with a total porosity of 40-55% and a compressive strength of 15-25 MPa. Under visible light, it achieves a degradation rate of ≥90% for chlorpyrifos and cypermethrin, and a tea polyphenol retention rate of ≥94%.
[0016] Furthermore, the porous ceramic clay filter material has a dual-mode regeneration capability: after adsorption saturation, it is calcined at 500-600℃ for 1-2 hours, and the inorganic catalytic phase and pore adsorption performance are completely restored; after being soaked in enzyme solution for 1-2 hours, the biodegradation activity can be restored, and the overall performance retention rate is ≥88% after 10 cycles.
[0017] The beneficial effects of this invention are: 1. This invention breaks through several technical bottlenecks of traditional tea filter materials through integrated innovation of interface selective design, visible light catalytic system construction, covalent enzyme immobilization and functional combination. It achieves a synergistic leap in pesticide residue degradation efficiency, flavor retention, service stability and circular economy, and has significant innovation and unexpected technical effects.
[0018] 2. This invention constructs a hydrophobic targeted modification interface on the inner wall of the pores of porcelain clay. Utilizing the difference between the strong hydrophobicity of organophosphorus and pyrethroid pesticides and the hydrophilicity of flavor compounds such as tea polyphenols and theanine, it achieves selective enrichment of pesticide molecules and low retention of flavor components, fundamentally overcoming the industry's inherent prejudice that "removing pesticide residues inevitably damages flavor." Compared to traditional indiscriminate adsorption filter materials, this solution improves pesticide residue removal rates while simultaneously increasing tea polyphenol retention to over 94%, with minimal impact on the aroma and taste of the tea. Furthermore, the natural tourmaline micropowder introduced into the matrix generates a spontaneously polarized micro-electric field, enhancing the directional mass transfer rate of pesticide molecules within the pores, improving catalytic reaction efficiency, and also moderately mineralizing and softening the water quality, reducing the bitterness of the tea and bringing additional improvements to the drinking quality.
[0019] 3. This invention uses nitrogen-doped TiO2 sensitized with tea polyphenol carbon dots as a visible light catalytic phase, extending the photoresponse range of TiO2 from the ultraviolet region to the visible light region. Indoor natural light and artificial light in everyday brewing environments can efficiently stimulate the generation of active free radicals, eliminating the need for an additional ultraviolet light source and significantly improving degradation efficiency in practical applications. Simultaneously, an active site is introduced into the pore walls through a silane coupling agent, allowing the degrading enzyme to be covalently anchored to the matrix. The binding strength is far higher than physical adsorption, resulting in almost no enzyme protein loss during brewing, significantly improving food safety and catalytic stability. Photocatalysis is responsible for the broad-spectrum degradation of various pesticides and the destruction of their macromolecular structures, while enzyme catalysis is responsible for the directional cleavage of characteristic functional groups such as phosphate ester bonds. The two processes complement each other and their efficiency is synergistic, achieving a pesticide residue removal rate of over 96% even at a gentle tea infusion temperature. Detailed Implementation
[0020] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0021] Example 1: A method for preparing a porous kaolin filter material that can efficiently decompose pesticide residues in tea infusion, comprising the following steps: S1: 60g of kaolin, 15g of quartz sand, 10g of bentonite, and 3g of tourmaline powder were put into a ball mill, along with 52.8g of deionized water and 1.76g of polyacrylamide binder. The mixture was ball-milled at 300r / min for 40min to obtain a uniform slurry. 7.04g of coal powder pore-forming agent was added and the mixture was ball-milled for another 20min. The slurry was then injected into a mold and pressed at 8MPa. After aging at room temperature for 12h, the mixture was dried at 80℃ for 6h. Subsequently, the temperature was increased to 400℃ at 2℃ / min and held for 1h, then increased to 1150℃ at 3℃ / min and held for 2h. The temperature was then decreased to 600℃ at 1℃ / min and allowed to cool naturally to obtain a multi-level porous porcelain clay carrier.
[0022] S2: The hierarchical porous ceramic support was immersed in a 5% (v / v) octyltriethoxysilane ethanol solution for 2 h at room temperature and then cured at 100 °C for 1 h to complete the hydrophobic silanization modification; then immersed in a tetrabutyl titanate precursor solution containing tea polyphenol carbon dots, impregnated under vacuum of -0.08 MPa for 30 min, hydrolyzed and cured under an ammonia atmosphere at 25 °C for 2 h, and calcined at 400 °C for 1 h to obtain a support loaded with a visible photocatalytic phase; wherein the TiO2 loading amount was 3% of the support mass and the carbon doping amount was 1% of the TiO2 mass.
[0023] S3: The carrier loaded with the visible light catalytic phase was immersed in KH-550 buffer solution at pH 7.0 and activated at 30℃ for 2h to introduce amino sites; after washing, it was transferred to a compound degrading enzyme (laccase: acid phosphatase = 1:1) at pH 6.5, grafted at 4℃ for 12h, and dried at 40℃ to obtain porous porcelain clay filter material; the enzyme loading was 0.3% of the carrier mass.
[0024] Example 2: A method for preparing a porous kaolin filter material that can efficiently decompose pesticide residues in tea infusion, comprising the following steps: S1: 70g kaolin, 20g quartz sand, 15g bentonite, and 8g tourmaline powder were put into a ball mill, along with 90.9g deionized water and 4.52g polyacrylamide binder. The mixture was ball-milled at 400r / min for 60min to obtain a uniform slurry. 16.95g coal powder pore-forming agent was added and the mixture was ball-milled for another 30min. The mixture was then pressed into shape at 12MPa, aged at room temperature for 24h, and dried at 100℃ for 8h. Subsequently, the temperature was increased to 500℃ at 3℃ / min and held for 2h, then increased to 1250℃ at 5℃ / min and held for 3h. The temperature was then decreased to 600℃ at 2℃ / min and allowed to cool naturally to obtain a multi-level porous porcelain clay carrier.
[0025] S2: The hierarchical porous ceramic support was immersed in a 10% (v / v) octyltriethoxysilane ethanol solution for 4 h at room temperature and then cured at 120 °C for 2 h to complete the hydrophobic silanization modification; then immersed in a tetrabutyl titanate precursor solution containing tea polyphenol carbon dots, impregnated under vacuum of -0.09 MPa for 50 min, hydrolyzed and cured at 30 °C under an ammonia atmosphere for 4 h, and calcined at 450 °C for 2 h to obtain a support loaded with a visible photocatalytic phase; wherein the TiO2 loading amount was 6% of the support mass and the carbon doping amount was 3% of the TiO2 mass.
[0026] S3: The carrier loaded with the visible light catalytic phase was immersed in KH-550 buffer solution at pH 7.5 and activated at 40℃ for 3h to introduce amino sites; after washing, it was transferred to a compound degrading enzyme (laccase: acid phosphatase = 1:2) at pH 7.0, grafted at 4℃ for 16h, and dried at 50℃ to obtain porous porcelain clay filter material; the enzyme loading was 0.8% of the carrier mass.
[0027] Example 3: A method for preparing a porous kaolin filter material that can efficiently decompose pesticide residues in tea infusion, comprising the following steps: S1: 70g kaolin, 20g quartz sand, 15g bentonite, and 8g tourmaline powder were put into a ball mill, along with 90.9g deionized water and 4.52g polyacrylamide binder. The mixture was ball-milled at 400r / min for 60min to obtain a uniform slurry. 16.95g coal powder pore-forming agent was added and the mixture was ball-milled for another 30min. The mixture was then pressed into shape at 12MPa, aged at room temperature for 24h, and dried at 100℃ for 8h. Subsequently, the temperature was increased to 500℃ at 3℃ / min and held for 2h, then increased to 1250℃ at 5℃ / min and held for 3h. The temperature was then decreased to 600℃ at 2℃ / min and allowed to cool naturally to obtain a multi-level porous porcelain clay carrier.
[0028] S2: The hierarchical porous ceramic support was immersed in a 10% (v / v) octyltriethoxysilane ethanol solution for 4 h at room temperature and then cured at 120 °C for 2 h to complete the hydrophobic silanization modification; then immersed in a tetrabutyl titanate precursor solution containing tea polyphenol carbon dots, impregnated under vacuum of -0.09 MPa for 50 min, hydrolyzed and cured at 30 °C under an ammonia atmosphere for 4 h, and calcined at 450 °C for 2 h to obtain a support loaded with a visible photocatalytic phase; wherein the TiO2 loading amount was 6% of the support mass and the carbon doping amount was 3% of the TiO2 mass.
[0029] S3: The carrier loaded with the visible light catalytic phase was immersed in KH-550 buffer solution at pH 7.5 and activated at 40℃ for 3h to introduce amino sites; after washing, it was transferred to a compound degrading enzyme (laccase: acid phosphatase = 1:2) at pH 7.0, grafted at 4℃ for 16h, and dried at 50℃ to obtain porous porcelain clay filter material; the enzyme loading was 0.8% of the carrier mass.
[0030] Comparative Example 1: Based on Example 3, the hydrophobic silanization modification, tea polyphenol carbon dot sensitization, and enzyme covalent immobilization steps were omitted. Only pure TiO2 was loaded and the enzyme was physically adsorbed and degraded. All other process parameters were the same as in Example 3.
[0031] Comparative Example 2: Based on Example 3, the multi-stage pore-forming process was omitted to prepare a dense porcelain clay carrier, and the remaining process parameters were the same as in Example 3.
[0032] Comparative Example 3: Based on Example 3, the original process route was adopted: the enzyme and TiO2 precursor were directly mixed into the porcelain clay slurry and then sintered at high temperature simultaneously, with the amount of other components remaining the same.
[0033] Performance tests were conducted on Examples 1-3 and Comparative Examples 1-3, using chlorpyrifos and cypermethrin as target pesticide residues (initial concentration 1 mg / L). The pesticide residue removal rate after filtration was tested under simulated brewing conditions with visible light indoors. The flavor retention rate was calculated by detecting the tea polyphenol content before and after filtration. The overall performance retention rate was tested after 5 cycles. The results are shown in Table 1. Table 1
[0034] As shown in Table 1, Examples 1-3 exhibited excellent performance in pesticide residue removal rate, flavor retention rate, and cycle stability, achieving a balance between "highly efficient pesticide residue removal and high flavor retention." Comparative Example 1, lacking hydrophobic silanization modification and visible light sensitization, not only had low degradation efficiency but also suffered from severe tea polyphenol retention; Comparative Example 2, lacking a hierarchical porous structure, experienced a significant decrease in both water flux and purification efficiency; Comparative Example 3, employing a simultaneous sintering process, resulted in complete enzyme inactivation and significant performance degradation. This fully demonstrates that this solution, through multiple technological innovations, achieved unexpected technical effects, possessing outstanding substantive characteristics and significant progress.
[0035] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the invention.
Claims
1. A method for preparing a porous kaolin filter material that can efficiently decompose pesticide residues in tea infusion, characterized in that, Includes the following steps: Step 1: Using kaolin, quartz sand, bentonite, and tourmaline powder as the composite porcelain clay matrix, coal powder pore-forming agent and polyacrylamide binder are added, and the mixture is ball-milled, aged, pressed into shape, and sintered by step heating to obtain a multi-level porous porcelain clay carrier with a multi-level pore structure. Step 2: The multi-level porous kaolin carrier is modified with hydrophobic silanization, and then a vacuum impregnation-in-situ hydrolysis process is used to immobilize tea polyphenols and nano titanium dioxide on the inner wall of the pores. After low-temperature curing, a carrier loaded with visible photocatalytic phase is obtained. Step 3: Using a silane coupling agent covalent grafting process, the compound degradation enzyme is immobilized in the pores of a carrier loaded with a visible light catalytic phase, and then dried at low temperature to obtain a porous ceramic clay filter material.
2. The preparation method of a porous kaolin filter material capable of efficiently decomposing pesticide residues in tea soup according to claim 1, characterized in that, The specific preparation steps of the multi-level porous porcelain clay carrier are as follows: Kaolin, quartz sand, bentonite, and tourmaline powder are fed into a ball mill, along with deionized water and polyacrylamide binder. The mixture is ball-milled at 300-400 r / min for 40-60 min to obtain a uniform slurry. Coal powder pore-forming agent is added, and the mixture is ball-milled for another 20-30 min. The slurry is then injected into a custom mold and pressed into shape at 8-12 MPa. After aging at room temperature for 12-24 h, it is dried at 80-100℃ for 6-8 h. Subsequently, it is sintered in a muffle furnace with stepped heating, and after natural cooling, a multi-level porous porcelain clay carrier is obtained.
3. The method for preparing a porous kaolin filter material capable of efficiently decomposing pesticide residues in tea soup according to claim 2, characterized in that, The mass ratio of the kaolin, quartz sand, bentonite, and tourmaline powder is 60-70:15-20:10-15:3-8; The amount of polyacrylamide binder added is 2-4% of the total mass of the kaolin, the amount of coal powder pore-forming agent added is 8-15% of the total mass of the kaolin, and the liquid-solid ratio is 0.6-0.8:1; The stepped heating sintering process is as follows: heat to 400-500℃ at 2-3℃ / min and hold for 1-2 hours to remove organic matter, continue to heat to 1150-1250℃ at 3-5℃ / min and hold for 2-3 hours for vitrification, and then cool down to 600℃ at 1-2℃ / min and allow to cool naturally.
4. The preparation method of a porous kaolin filter material capable of efficiently decomposing pesticide residues in tea soup according to claim 1, characterized in that, The specific steps for using the support with the visible photocatalytic phase are as follows: A hierarchical porous ceramic support was immersed in a 5-10% (v / v) octyltriethoxysilane ethanol solution for 2-4 hours at room temperature. After immersion, the support was removed and cured at 100-120℃ for 1-2 hours to complete the hydrophobic silanization modification of the pores. Subsequently, the support was immersed in a tetrabutyl titanate precursor solution containing tea polyphenol carbon dots for 30-50 minutes under a vacuum of -0.08 to -0.09 MPa. After removal, the support was placed in an ammonia atmosphere at 25-30℃ for hydrolysis and curing for 2-4 hours, and then calcined at 400-450℃ for 1-2 hours to obtain a support loaded with a visible photocatalytic phase.
5. The preparation method of a porous kaolin filter material capable of efficiently decomposing pesticide residues in tea soup according to claim 4, characterized in that, The tea polyphenol carbon dots are prepared from tea extract by a hydrothermal method, with a particle size of 2-6 nm; the final TiO2 loading is 3-6% of the mass of the kaolin carrier, and the tea polyphenol carbon doping amount is 1-3% of the mass of TiO2; after hydrophobic silanization modification, the water contact angle of the pores is 95°-115°.
6. The preparation method of a porous kaolin filter material capable of efficiently decomposing pesticide residues in tea soup according to claim 1, characterized in that, The specific steps for covalently immobilizing the degradation enzyme are as follows: The carrier loaded with the visible light catalytic phase was immersed in a γ-aminopropyltriethoxysilane buffer solution with a pH of 7.0-7.5 and activated at 30-40℃ for 2-3 hours to introduce amino active sites. After washing, it was transferred to a compound degrading enzyme solution with a pH of 6.5-7.0 and covalently grafted at 4℃ for 12-16 hours. After removal, it was rinsed with buffer solution to remove free enzymes and dried at a low temperature of 40-50℃ to obtain a porous ceramic filtration material.
7. The preparation method of a porous kaolin filter material capable of efficiently decomposing pesticide residues in tea soup according to claim 6, characterized in that, The compound degrading enzyme is a mixture of laccase and acid phosphatase in a mass ratio of 1:1-2; the final immobilization amount of the degrading enzyme is 0.3-0.8% of the mass of the kaolin carrier.
8. The preparation method of a porous kaolin filter material capable of efficiently decomposing pesticide residues in tea soup according to claim 1, characterized in that, The porous ceramic clay filter material has a three-level pore size distribution: macropores 50-200μm, mesopores 2-50nm, and micropores <2nm, with a total porosity of 40-55% and a compressive strength of 15-25MPa; under visible light, it has a degradation rate of ≥90% for chlorpyrifos and cypermethrin, and a tea polyphenol retention rate of ≥94%.
9. The preparation method of a porous kaolin filter material capable of efficiently decomposing pesticide residues in tea soup according to claim 1, characterized in that, The porous ceramic clay filter material has a dual-mode regeneration capability: after adsorption saturation, it is calcined at 500-600℃ for 1-2 hours, and the inorganic catalytic phase and pore adsorption performance are completely restored; after being soaked in enzyme solution for 1-2 hours, the biodegradation activity can be restored, and the overall performance retention rate is ≥88% after 10 cycles.
10. A porous kaolin filter material that can efficiently decompose pesticide residues in tea infusion, characterized in that, The porous porcelain clay filter material capable of efficiently decomposing pesticide residues in tea soup is prepared by any one of claims 1-9.