A molybdenum nitride cocatalyst-supported carbon nitride composite material and its preparation method

By constructing a Mo2N-Mo16N7 heterojunction molybdenum nitride cocatalyst and a two-dimensional carbon nitride composite material, the problems of photogenerated carrier recombination and limited specific surface area in photocatalytic water splitting were solved, and a highly efficient photocatalytic hydrogen production effect was achieved.

CN123102402APending Publication Date: 2026-11-17JIANGSU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611626959.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing photocatalytic water splitting materials, rapid recombination occurs during the migration of photogenerated carriers, which prevents electrons from effectively participating in the catalytic reaction and limits the efficiency of photocatalytic hydrogen production. Furthermore, traditional bulk g-C3N4 suffers from limited specific surface area and high recombination rate of photogenerated electron-hole pairs.

Method used

A two-dimensional-two-dimensional heterostructure was formed by constructing a Mo2N-Mo16N7 heterojunction molybdenum nitride cocatalyst and a two-dimensional carbon nitride composite material. The heterostructure between Mo2N and Mo16N7 enhances the separation efficiency of photogenerated carriers and optimizes the electron transport capability.

Benefits of technology

It significantly improved the photocatalytic hydrogen production performance, with a hydrogen production rate of 17.15 mmol·g⁻¹·h⁻¹, which is 8.8 times and 214.4 times that of the single molybdenum nitride structure, respectively, thus improving the photogenerated carrier separation efficiency and hydrogen evolution reaction kinetics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102402A_ABST
    Figure CN123102402A_ABST
Patent Text Reader

Abstract

This invention relates to a molybdenum nitride cocatalyst-supported carbon nitride composite material and its preparation method. The molybdenum nitride cocatalyst-supported carbon nitride composite material comprises two-dimensional carbon nitride nanosheets and a molybdenum nitride-based cocatalyst supported on the surface of the two-dimensional carbon nitride nanosheets; the molybdenum nitride-based cocatalyst contains a Mo₂N crystalline phase and Mo. 16 N7 crystal phase, and Mo2N crystal phase is similar to Mo 16 Heterogeneous interfaces are formed between the N7 crystalline phases; a two-dimensional-two-dimensional composite structure is formed between the molybdenum nitride-based cocatalyst and the two-dimensional carbon nitride nanosheets. This invention utilizes Mo2N and Mo... 16 N7 forms a biphase molybdenum nitride cocatalyst, which can provide synergistic active centers with different electronic structures, which is beneficial to optimizing the electron transfer behavior in the hydrogen evolution reaction process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of photocatalytic materials technology, specifically relating to a molybdenum nitride cocatalyst-supported carbon nitride composite material and its preparation method, based on two-dimensional carbon nitride nanosheets and Mo2N-Mo. 16 This paper describes a heterogeneous composite photocatalytic material constructed using N7 heterojunction molybdenum nitride cocatalyst and its preparation method, and discusses the application of this composite material in visible light photocatalytic water splitting for hydrogen production. Background Technology

[0002] With increasing fossil fuel consumption and growing environmental pollution, developing clean and sustainable new energy systems has become a crucial research direction in the energy field. Hydrogen, with its high energy density and combustion product consisting solely of water, is considered a promising clean energy carrier. Photocatalytic water splitting driven by solar energy can directly convert solar energy into chemical energy, representing a significant technological pathway for achieving green hydrogen production.

[0003] In photocatalytic water splitting, semiconductor photocatalytic materials absorb light energy to generate photogenerated electrons and holes. Photogenerated electrons migrate to the catalyst surface to participate in the hydrogen evolution reaction, while photogenerated holes are consumed by sacrificial agents or participate in oxidation reactions. However, due to rapid recombination during photogenerated carrier migration, a large number of electrons cannot participate in the surface catalytic reaction, limiting the efficiency of photocatalytic hydrogen production. Therefore, constructing a co-catalyst / semiconductor composite structure to improve the separation efficiency of photogenerated carriers and reduce the surface reaction energy barrier is an important strategy for improving photocatalytic performance.

[0004] Graphitic carbon nitride (g-C3N4) is widely used in photocatalytic water splitting due to its advantages such as visible light response, good chemical stability, low preparation cost, and tunable structure. However, traditional bulk g-C3N4 still suffers from problems such as limited specific surface area, easy stacking of sheets, and high recombination rate of photogenerated electron-hole pairs, which limit its actual photocatalytic efficiency.

[0005] Currently, improving the catalytic performance of two-dimensional carbon nitride-based cocatalysts by constructing composite structures of two-dimensional carbon nitride and transition metal-based cocatalysts has become a research hotspot. For example, previous studies have supported molybdenum nitride nanoparticles on the surface of carbon nitride to form composite photocatalysts, utilizing the metallic properties of molybdenum nitride to improve electron transport capabilities, thereby reducing carrier recombination probability and enhancing hydrogen production performance. However, most existing molybdenum nitride-based cocatalysts are still dominated by a single crystalline phase or a single molybdenum nitride phase, with limited active center types and interfacial electronic regulation capabilities.

[0006] Furthermore, existing studies have employed Mo-Mo2C heterostructures or other molybdenum-based composite materials as cocatalysts. For example, current technology discloses a nanoscale carbon-coated Mo-Mo2C heterostructure nanoparticle, its preparation method, and its applications, which enhance photocatalytic performance through the Mo-Mo2C heterostructure. However, this system belongs to a molybdenum carbide composite system, and its Fermi level, d-band electronic structure, and surface active sites differ from those of molybdenum nitride heterojunctions, and it does not involve Mo2N and Mo. 16 The construction of heterogeneous interfaces between N and 7 has been studied. Meanwhile, previous studies have reported MoS2 / g-C3N4 composite materials and defect-engineered systems to improve hydrogen production performance by introducing sulfur vacancies. However, these systems are mainly based on sulfide co-catalysts or defect-engineering strategies, and do not involve Mo2N and Mo... 16 Construction of N7 biphase molybdenum nitride heterointerface. Summary of the Invention

[0007] Existing technologies lack a method that can simultaneously utilize Mo2N / Mo 16 A molybdenum nitride-based cocatalyst composite system exhibiting synergistic effects of multiple active centers at the N7 biphase heterostructure interface, enhanced interfacial electron transport capability, and promoted spatial separation of photogenerated carriers.

[0008] To address the above problems, this invention provides a Mo2N-Mo 16 The N7 heterojunction molybdenum nitride cocatalyst supports a two-dimensional carbon nitride composite material. By constructing a two-phase molybdenum nitride hetero interface and forming a 2D-2D composite structure with two-dimensional carbon nitride, the photogenerated carrier separation efficiency is improved and the hydrogen evolution reaction kinetics are enhanced.

[0009] To achieve the above objectives, the present invention provides a molybdenum nitride cocatalyst-supported carbon nitride composite material, which includes two-dimensional carbon nitride nanosheets and a molybdenum nitride-based cocatalyst supported on the surface of the two-dimensional carbon nitride nanosheets; The molybdenum nitride-based cocatalyst contains Mo2N crystalline phase and Mo. 16 N7 crystal phase, and Mo2N crystal phase is similar to Mo 16 Heterogeneous interfaces are formed between the N7 crystalline phases; The molybdenum nitride-based cocatalyst forms a two-dimensional-two-dimensional heterocomposite structure with the two-dimensional carbon nitride nanosheets.

[0010] In a preferred embodiment, the two-dimensional carbon nitride nanosheets are obtained from the nitrogen-containing precursor g-C3N4 through thermal polymerization and exfoliation. The two-dimensional carbon nitride nanosheets have a layered two-dimensional structure, which is used to provide a molybdenum nitride cocatalyst loading interface and a photogenerated carrier transport channel.

[0011] In a preferred embodiment, the molybdenum nitride-based cocatalyst contains Mo2N crystal phase and Mo... 16The N7 crystal phases together form a dual active center structure, and the electronic structure of the composite material is adjusted through the interfacial electronic coupling between the two molybdenum nitride crystal phases. The molybdenum nitride-based cocatalyst is dispersed on the surface of two-dimensional carbon nitride nanosheets to reduce the stacking of two-dimensional carbon nitride nanosheets and increase the number of photocatalytic reaction active sites.

[0012] In a preferred embodiment, the molybdenum nitride-based co-catalyst contains Mo2N crystal phase and Mo 16 The mass ratio of N7 crystal phase is 1:10 to 10:1, preferably 1:3 to 3:1.

[0013] In a preferred embodiment, the molybdenum nitride-based cocatalyst is loaded in the composite material at a rate of 1–50 wt%, preferably 5–30 wt%.

[0014] This invention also provides a method for preparing a molybdenum nitride co-catalyst-supported carbon nitride composite material, which includes the following steps: Step 1: Preparation of two-dimensional carbon nitride nanosheets (CN): A nitrogen-containing precursor is subjected to thermal polymerization to obtain graphitic carbon nitride g-C3N4; g-C3N4 is subjected to ultrasonic exfoliation combined with secondary calcination to obtain CN; Step 2: MoN x Preparation of heterojunction molybdenum nitride co-catalyst: A precursor system is formed by mixing a molybdenum source, a zinc salt, and an alkaline modifier, and then dried to obtain an intermediate product. The intermediate product is then heat-treated in a nitrogen-containing reducing atmosphere to form MoN2. x Heterojunction molybdenum nitride co-catalyst; the MoN x Composed of Mo2N crystal phase and Mo 16 N7 crystal phase composition; Step 3: Composite material preparation: The MoN x The heterojunction molybdenum nitride co-catalyst is liquid-phase composited with CN and then dried to obtain MoN. x / CN composite materials: In the preferred solution, The nitrogen-containing precursor is melamine; in the preparation of CN, melamine is mixed with a surfactant and heat-treated at 450-550℃ to obtain graphitic carbon nitride. CN was then obtained by ultrasonic exfoliation combined with secondary calcination. The key step in the secondary calcination is controlling the heating rate to ≤2℃ / min. When the heating rate exceeds 2℃ / min, the rapid increase in internal temperature of the two-dimensional carbon nitride nanosheets easily leads to rapid shrinkage and local sintering of the sheet structure, reducing the integrity of the two-dimensional structure and increasing the degree of defect disorder. This is not conducive to the formation of a two-dimensional carbon nitride support with a high specific surface area and stable interface, thereby reducing the uniform loading effect of the subsequent molybdenum nitride co-catalyst and the photocatalytic performance of the composite material.

[0015] In the preferred embodiment, the molybdenum source is ammonium heptamolybdate tetrahydrate; The zinc salt is zinc nitrate hexahydrate; The alkalinity regulator is ammonia water; The heat treatment process uses a N2 / H2 mixed atmosphere, and the heat treatment temperature is 650-750℃. The volume ratio of N2 / H2 is 50:50 to 95:5, preferably 90:10; The flow rate of the mixed atmosphere is 0.1 L / min to 10 L / min, preferably 1 to 5 L / min; The molar ratio of the molybdenum source to the zinc salt is 1:2 to 1:20, preferably 1:5 to 1:10; In the liquid-phase composite, the MoN x The ratio of heterojunction molybdenum nitride co-catalyst to CN is 1:99 to 1:1, preferably 5:95 to 30:70.

[0016] The present invention also provides an application of the aforementioned molybdenum nitride cocatalyst supported carbon nitride composite material in photocatalytic hydrogen production.

[0017] In a preferred embodiment, the photocatalytic hydrogen production is visible light-driven water splitting for hydrogen production; The composite material is used to promote photogenerated electron transfer, improve photogenerated carrier separation efficiency and / or enhance hydrogen evolution reaction kinetics; The hydrogen production rate of the composite material is 17.15 mmol·g. -1 ·h -1 .

[0018] The beneficial effects of this invention are as follows: 1. Enhanced catalytic activity through a molybdenum nitride heterostructure: This invention utilizes Mo2N and Mo... 16 N7 forms a biphase molybdenum nitride cocatalyst, which, compared to a single molybdenum nitride structure, can provide synergistic active centers with different electronic structures, which is beneficial for optimizing electron transfer behavior during the hydrogen evolution reaction.

[0019] 2. Improve the separation efficiency of photogenerated carriers: Mo2N-Mo 16The N7 heterojunction forms a tight interfacial contact with CN, which can promote interfacial electron migration, reduce the probability of photogenerated electron-hole recombination, and improve the effective electron utilization rate.

[0020] 3. Maintaining the stability of the two-dimensional structure: CN, as a support, can disperse molybdenum nitride co-catalyst particles, reduce the stacking of two-dimensional materials, and increase the contact area of ​​reactants.

[0021] 4. Improved photocatalytic hydrogen production performance: Experimental results show that the MoN obtained in this invention... x The / CN composite material exhibits high hydrogen production performance under visible light conditions, with a hydrogen production rate reaching 17.15 mmol·g. -1 h -1 CN and MoN respectively x It is 8.8 times and 214.4 times that of the co-catalyst. Attached Figure Description

[0022] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0023] Figure 1 a) CN; b) MoN x c) MoN x d) SEM image of CN; e, f) TEM image of CN; x TEM and HRTEM images of / CN.

[0024] Figure 2 for Mo 16 N7 / CN, MoN x XRD patterns of / CN and Mo2N / CN.

[0025] Figure 3 For a) CN, MoN x and MoN x a) XPS full spectrum of / CN; b) C1s spectrum; c) N1s spectrum; d) Mo 3d spectrum.

[0026] Figure 4 For a. steady-state fluorescence spectrum of PL, b. time-resolved fluorescence decay curve of TRPL, and c. transient photocurrent response curve.

[0027] Figure 5 For theoretical calculations of a) CN, b) MoN xand c) MoN x / CN adsorption energy for H2O. Detailed Implementation

[0028] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0029] This invention first provides a molybdenum nitride cocatalyst-supported carbon nitride composite material, which includes two-dimensional carbon nitride nanosheets and a molybdenum nitride-based cocatalyst supported on the surface of the two-dimensional carbon nitride nanosheets; The molybdenum nitride-based cocatalyst contains Mo2N crystalline phase and Mo. 16 N7 crystal phase, and Mo2N crystal phase is similar to Mo 16 Heterogeneous interfaces are formed between the N7 crystalline phases; The molybdenum nitride-based cocatalyst forms a two-dimensional-two-dimensional heterocomposite structure with the two-dimensional carbon nitride nanosheets.

[0030] As a preferred embodiment, the two-dimensional carbon nitride nanosheets are obtained by thermal polymerization and exfoliation of the nitrogen-containing precursor g-C3N4; the two-dimensional carbon nitride nanosheets have a layered two-dimensional structure, which is used to provide a molybdenum nitride cocatalyst loading interface and a photogenerated carrier transport channel.

[0031] In the molybdenum nitride-based cocatalyst, the Mo2N crystal phase and Mo 16 The N7 crystal phases together form a dual active center structure, and the electronic structure of the composite material is adjusted through the interfacial electronic coupling between the two molybdenum nitride crystal phases. The molybdenum nitride-based cocatalyst is dispersed on the surface of two-dimensional carbon nitride nanosheets to reduce the stacking of two-dimensional carbon nitride nanosheets and increase the number of photocatalytic reaction active sites.

[0032] In a preferred embodiment, the molybdenum nitride-based co-catalyst contains Mo2N crystal phase and Mo 16 The mass ratio of the N7 crystal phase is 1:10 to 10:1, preferably 1:3 to 3:1. The loading of the molybdenum nitride-based co-catalyst in the composite material is 1 to 50 wt%, preferably 5 to 30 wt%.

[0033] For specific preparation examples, please refer to the following content: Example 1: Preparation of two-dimensional carbon nitride nanosheets (CN): This embodiment provides a method for preparing CN, the specific steps of which are as follows: (1) Weigh 2 g of melamine and add it to deionized water. Stir magnetically at room temperature to fully dissolve the melamine and form a uniform and transparent solution. Add sodium dodecyl sulfate (SDS) to the above solution. The amount of SDS added is 5 to 20 wt% of the mass of melamine. This is used to control the particle size during the precursor polymerization process and reduce agglomeration during the subsequent heat treatment process.

[0034] (2) The obtained mixed solution was evaporated and dried at 60°C to obtain a white solid precursor. The solid precursor was placed in a muffle furnace and heated to 450-550°C at a heating rate of 2-5°C / min in air atmosphere, and held at the temperature for 4-8 h to allow melamine to undergo a thermal polycondensation reaction to obtain bulk graphitic carbon nitride (g-C3N4).

[0035] (3) The obtained blocky g-C3N4 was ground into powder and dispersed in deionized water, and then subjected to ultrasonic treatment for interlayer exfoliation. The ultrasonic power was 200 W and the ultrasonic time was 2 to 8 h. After ultrasonic exfoliation, a two-dimensional carbon nitride suspension was obtained.

[0036] (4) The obtained suspension was filtered and the collected solid was dried. Then the temperature was increased to 450-550℃ at a rate of 2℃ / min and held for 1-2 h to obtain two-dimensional carbon nitride nanosheets (CN).

[0037] Example 2: Preparation of Mo2N co-catalyst: This embodiment provides a method for preparing a single-phase Mo2N cocatalyst for subsequent performance comparison.

[0038] The specific steps are as follows: (1) Prepare 100 mL of an aqueous solution containing 14 mmol of zinc nitrate hexahydrate (Zn(NO3)3·6H2O). Simultaneously prepare 200 mL of an aqueous solution containing 2 mmol of ammonium heptamolybdate tetrahydrate (AMH, (NH4)6Mo7O). 24 A mixed solution of 4H2O and 2.5 mL of ammonia was prepared to obtain a molybdenum source solution.

[0039] (2) Under magnetic stirring conditions, Zn(NO3)3·6H2O solution was added dropwise to the above molybdenum source solution and stirred continuously for 3 h to obtain a uniform precursor solution.

[0040] (3) The obtained precursor solution was freeze-dried for 6 h to obtain the dried intermediate product.

[0041] (4) Weigh 50 mg of the intermediate product and place it in a tube furnace for heat treatment under a N2 / H2 mixed atmosphere. The treatment conditions are as follows: heating rate 5℃ / min; calcination temperature 750℃; holding time 5 h; N2 / H2 volume ratio 90:10; and mixed atmosphere flow rate 2 L / min. After heat treatment, Mo2N co-catalyst is obtained.

[0042] Example 3: Mo2N-Mo 16 N7 heterojunction co-catalyst (MoN) x Preparation of ) This embodiment provides a Mo2N-Mo 16 Preparation method of N7 biphase molybdenum nitride heterojunction co-catalyst.

[0043] The specific steps are as follows: (1) Prepare molybdenum-based precursor (dried intermediate product) according to the method of Example 2.

[0044] (2) 100 mg of the obtained precursor was placed in a tube furnace and heat-treated in a N2 / H2 mixed atmosphere. Treatment conditions: heating rate 5℃ / min; temperature: 750℃; time: 5 h; N2 / H2 volume ratio 90:10; flow rate of mixed atmosphere 2L / min.

[0045] (3) During the heat treatment process, the molybdenum-based precursor undergoes a nitriding reaction and forms a Mo2N crystalline phase and Mo 16 A two-phase molybdenum nitride heterostructure composed of N7 crystalline phases. The resulting product is denoted as MoN. x .

[0046] Example 4: Mo 16 Preparation of N7 cocatalyst: This embodiment provides a Mo 16 Preparation method of N7 biphase molybdenum nitride heterojunction co-catalyst.

[0047] The specific steps are as follows: (1) Prepare molybdenum-based precursors according to the method of Example 2.

[0048] (2) 300 mg of the obtained precursor was placed in a tube furnace and heat-treated in a N2 / H2 mixed atmosphere. Treatment conditions: heating rate 5℃ / min; temperature: 750℃; time: 5 h; N2 / H2 volume ratio 90:10; flow rate of mixed atmosphere 2L / min.

[0049] (3) During the heat treatment process, the molybdenum-based precursor undergoes a nitriding reaction, and Mo is obtained after the heat treatment is completed. 16 N7 cocatalyst.

[0050] In Examples 2 to 4, by adjusting the loading amount of molybdenum-based precursor during the heat treatment process, the ratio between the precursor and the nitrogen-containing reducing atmosphere in the reaction system can be changed, thereby regulating the local nitriding degree and the diffusion and reconstruction behavior of Mo species, achieving Mo2N crystal phase and Mo2N / Mo. 16 N7 biphase structure and Mo 16 Controllable preparation of N7 crystal phase.

[0051] Under low precursor loading conditions (50 mg of intermediate product was weighed and placed in a tube furnace in Example 2), the system has a high gas-solid contact efficiency, and active nitrogen species can fully participate in the reaction, causing Mo species to tend to be fully nitrided, and finally forming a stable Mo2N crystal phase. When the precursor loading is increased to a moderate level (100 mg of intermediate product was weighed and placed in a tube furnace in Example 3), a certain degree of nitriding gradient is formed inside the system. Mo species in different regions undergo different nitriding pathways, thereby producing Mo2N and Mo. 16 A two-phase structure with N7 coexistence.

[0052] Under high precursor loading conditions (Example 4: 300 mg of intermediate product was weighed and placed in a tube furnace), the precursor layer thickness increased, limiting the diffusion of nitriding gas into the interior, creating a relatively nitrogen-poor environment in the local system, and promoting the formation of Mo with a lower nitrogen content. 16 N7 crystal phase.

[0053] In summary, by changing the precursor loading amount alone, without altering the overall atmosphere ratio, the local nitrogen potential within the sample can be modified; a low loading amount enriches the nitrogen-rich environment to generate Mo2N, while a medium loading amount creates a nitriding gradient, resulting in Mo2N / Mo2N. 16 N7 biphase, high-volume lean nitrogen production of Mo 16 N7. During the experiment, the precursor loading amount or the flow rate of the N2 / H2 mixed atmosphere can be adjusted as needed to obtain the desired substance.

[0054] Example 5: MoN x Preparation of / CN composite photocatalytic materials: This embodiment provides a MoN x A method for preparing heterojunction-supported two-dimensional carbon nitride composite materials.

[0055] The specific steps are as follows: (1) Weigh 50 mg of CN obtained in Example 1 and add it to 50 mL of deionized water. Disperse by ultrasonication for 2 h to obtain a uniform CN dispersion.

[0056] (2) Prepare MoN with a concentration of 0.5 mg / mL x Aqueous dispersion. MoN was mixed under magnetic stirring. xThe MoN dispersion was added dropwise to the CN dispersion. Stirring was continued for 12 h to allow the MoN to mature. x Fully loaded onto the surface of CN nanosheets.

[0057] (3) The obtained mixture was freeze-dried for 6 h to obtain MoN. x / CN composite photocatalytic materials.

[0058] In the above preparation process, the molar ratio of the molybdenum source to the zinc salt is 1:2 to 1:20, preferably 1:5 to 1:10; for example, in other specific embodiments, the molar ratio of the molybdenum source to the zinc salt is 1:5, 1:6, 1:7, 1:8, 1:9, or 1:10. MoN x The mass ratio of MoN to CN is 1:99 to 1:1, preferably 5:95 to 30:70; in a specific embodiment, MoN x The feeding ratio of CN is 5:90, 5:70, 5:50, 5:30, 5:15 or 30:70.

[0059] Example 6: Photocatalytic hydrogen production performance test: This embodiment also provides an application of the molybdenum nitride cocatalyst-supported carbon nitride composite material in photocatalytic hydrogen production.

[0060] In a preferred embodiment, the photocatalytic hydrogen production is visible light-driven water splitting; the composite material is used to promote photogenerated electron transfer, improve photogenerated carrier separation efficiency, and / or enhance hydrogen evolution reaction kinetics; the hydrogen production rate of the composite material is 17.15 mmol·g. -1 ·h -1 .

[0061] For specific experimental steps, please refer to the implementation process below: The hydrogen production performance of the obtained composite material was tested using a visible light photocatalytic system.

[0062] The specific testing method is as follows: A certain mass of catalyst sample is weighed and added to the reaction system, water is used as the hydrogen source, and a sacrificial agent is added to promote the effective utilization of photogenerated carriers. Irradiation is performed using a visible light source with a wavelength greater than 420 nm. The gases generated during the reaction are detected by gas chromatography. The test samples include: (1) CN; (2) MoN. x (3) MoN x / CN and comparative samples (4) Mo2N; (5) Mo2N / CN; (6) Mo 16 N7; (7) Mo 16 N7 / CN.

[0063] Comparative Example 1: Mo2N / CN composite material: Using the method in Example 5, Mo2N was used to replace MoN. x Mo2N / CN composite material was obtained.

[0064] This was used to evaluate the effect of a single Mo2N cocatalyst on improving CN performance.

[0065] Comparative Example 2: Mo 16 N7 / CN composite material: Using the method of Example 5, Mo 16 N7 replaces MoN x Obtain Mo 16 N7 / CN composite material.

[0066] Used to evaluate a single Mo 16 The effect of N7 co-catalyst on improving CN performance.

[0067] Experimental characterization and results analysis To verify the Mo2N-Mo prepared in this invention 16 N7 heterojunction molybdenum nitride co-catalyst and MoN x The structural characteristics, interfacial interactions, and photocatalytic hydrogen production performance of the / CN composite material were investigated. Scanning electron microscopy, transmission electron microscopy, X-ray diffraction, and X-ray photoelectron spectroscopy analyses were performed on the samples obtained in the examples. The performance was evaluated based on first-principles calculations and photocatalytic hydrogen production experiments. Unless otherwise stated, the following MoN... x It indicates that it is composed of Mo2N crystal phase and Mo 16 Mo2N-Mo composed of N7 crystal phase 16 N7 heterojunction molybdenum nitride cocatalyst, CN represents two-dimensional carbon nitride nanosheets.

[0068] Material morphology and heterogeneous interface characterization CN and MoN were analyzed using scanning electron microscopy (SEM) and transmission electron microscopy (TEM), respectively. x and MoN x The morphology of the / CN composite material was characterized, and the results are as follows: Figure 1 As shown. Among them, Figure 1 a is the SEM image of CN. Figure 1 b is MoN x SEM image, Figure 1 c is MoN x SEM image of / CN composite material; Figure 1 d is the TEM image of CN. Figure 1 e, 1f is MoN x TEM and high-resolution transmission electron microscopy (HRTEM) images of the / CN composite material.

[0069] Figure 1a is the SEM image of CN. Figure 1 b is MoN x SEM image, Figure 1 c is MoN x SEM image of / CN composite material; Figure 1 d is the TEM image of CN. Figure 1 e, 1f is MoN x TEM and high-resolution transmission electron microscopy (HRTEM) images of the / CN composite material. (By...) Figure 1 a and Figure 1 As can be seen from d, the prepared CN exhibits a loose two-dimensional layered structure, with relatively porous morphology formed between the layers. This two-dimensional structure is beneficial for increasing the contact area between the catalytic material and the reaction medium, and for providing a loading interface for the co-catalyst. Figure 1 b shows that the prepared MoN x It mainly exhibits a two-dimensional sheet-like structure with a relatively uniform overall morphology. Figure 1 c shows that MoN x After being combined with CN, the two two-dimensional materials come into contact and overlap, and the resulting composite material still maintains a relatively loose two-dimensional lamellar structure without obvious large-scale block agglomeration. Further... Figure 1 e shows that MoN x The distribution and loading of MoN on the surface of CN sheets demonstrate that the liquid-phase composite method of this invention can realize MoN x Effective interfacial contact between MoN and CN. CN acts as a two-dimensional carrier in the composite structure, which is beneficial to MoN. x The dispersion of layers can reduce the direct stacking between two-dimensional sheets to some extent. Figure 1 The HRTEM results of f further revealed two different sets of lattice fringes, corresponding to the Mo2N and Mo crystal phases, respectively. 16 The N7 crystalline phase exhibits a clear phase interface between the two lattice regions. The SEM and TEM results above collectively demonstrate that this invention successfully constructed MoN₂. x A 2D-2D composite structure in contact with CN.

[0070] This demonstrates that the MoN obtained by this invention... x Not a single Mo2N or a single Mo 16 The N7 crystal phase is actually composed of Mo2N and Mo. 16 N7 is composed of two molybdenum nitride phases, with a heterogeneous interface between them, demonstrating the microstructure of Mo2N-Mo. 16 The N7 heterojunction co-catalyst was successfully constructed.

[0071] Crystal phase structure characterization Mo was examined using an X-ray diffractometer. 16N7 / CN, MoN x Crystal phase structure analysis was performed on / CN and Mo2N / CN samples, and the obtained XRD patterns are shown below. Figure 2 As shown.

[0072] Depend on Figure 2 It can be seen that all composite samples exhibit characteristic diffraction peaks belonging to the (002) crystal plane of CN around approximately 27.5°, indicating that the CN main crystal phase structure was preserved during the composite processing. For MoN... x The / CN sample exhibits both Mo2N and Mo2N, respectively, within the 40°–45° range. 16 Characteristic diffraction peaks of the N7 crystalline phase. These results are consistent with HRTEM observations, further confirming that MoN... x / CN contains both Mo2N and Mo phases. 16 N7 crystal phase. Comparatively, Mo2N / CN and Mo... 16 Compared to N7 / CN, MoN x / CN simultaneously exhibits structural characteristics of two molybdenum nitride phases, thus further proving the effectiveness of the MoN used in this invention. x It is not a single molybdenum nitride cocatalyst, but a two-phase heterostructure composed of two molybdenum nitride crystalline phases. Combined with the HRTEM results of Experimental Example 1, the Mo2N-Mo structure can be confirmed at both the lattice scale and the overall crystal phase level. 16 Formation of N7 heterojunction.

[0073] MoN x / CN interface electronic interaction characterization X-ray photoelectron spectroscopy (XPS) was used to analyze CN and MoN. x and MoN x Surface elemental composition and chemical state analysis were performed on the / CN sample, and the results are as follows: Figure 3 As shown. Among them, Figure 3 a represents CN and MoN x and MoN x XPS full spectrum of / CN; Figure 3 b is the high-resolution XPS image of C1s; Figure 3 c represents the N 1s high-resolution XPS spectrum; Figure 3 d represents the high-resolution XPS image of Mo 3d.

[0074] 1. XPS full spectrum analysis Depend on Figure 3 a can be seen from MoN x Mo, C, N, and O elemental signals were simultaneously detected in the / CN sample. C and N elements primarily originated from CN, while Mo and N elements were derived from MoN. xThe above results further prove, from the perspective of elemental composition, that MoN is relevant. x The CN composite system has been successfully introduced.

[0075] 2. C 1s energy dispersive spectroscopy analysis The C 1s spectrum of CN shows that the binding energy peak at approximately 288.3 eV belongs to the NC=N group in the carbon nitride structure. When CN binds to MoN... x After recombination, the characteristic peak shifted from approximately 288.3 eV to approximately 288.7 eV, representing a shift of about 0.4 eV towards a higher binding energy; simultaneously, the binding energies related to CC and C-NH2 did not change significantly. These results indicate that MoN... x The introduction of this mainly affects the electronic environment around specific nitrogen-containing conjugated structures in CN, rather than causing overall destruction of the CN host chemical structure.

[0076] 3. N 1s energy spectrum analysis In the N 1s spectrum of CN, the binding energy peak at approximately 400.9 eV is attributed to NHx-related groups. CN and MoN x After recombination, the peak shifted to approximately 401.0 eV, also exhibiting a shift towards higher binding energies, while the peak positions for N-(C)3 and CN=C remained largely unchanged. The shift of the binding energies of specific chemical groups in C 1s and N 1s towards higher binding energies indicates that CN binds more efficiently with MoN. x After the interface contact is formed, its local electronic environment changes.

[0077] 4. Mo 3d energy dispersive spectroscopy analysis As can be seen from the high-resolution spectrum of Mo 3d, MoN x and MoN x Mo in the / CN sample exists in multiple chemical states, including Mo 6 + Mo γ+ and Mo δ+ , where: 3<γ<4; 2<δ<3. MoN x The peak at approximately 232.0 eV is attributed to Mo. 6+ The peak positions of the relevant components remained essentially unchanged after recombination with CN. MoN x At approximately 229.1 eV, it belongs to Mo. γ+ The peak shifts to approximately 229.0 eV after the formation of the MoNx / CN composite structure; the peak at approximately 228.4 eV is attributed to Mo. δ+ The peaks in the formation of MoN x The V value shifts to approximately 228.3 eV after recombination. This means that some of the lower valence state components of Mo shift towards the direction of lower binding energy after recombination.

[0078] 5. Analysis of interfacial electronic interactions Comparing the binding energy changes of C 1s, N 1s, and Mo 3d, it can be found that the binding energy of specific C and N groups in CN shifts towards higher binding energies; meanwhile, MoN x The binding energy of some Mo species in the middle part shifts towards lower binding energies.

[0079] The two change in opposite directions. Considering the electron shielding effect, CN and MoN can be considered... x After the formation of a tight interface, an interfacial electron redistribution occurred, with the electrons generally shifting from the CN side to the MoN side. x The trend of lateral migration. Therefore, MoN x The interaction between CN and MoN is not a simple mechanical mixing, but rather involves significant interfacial electronic interactions. These interactions facilitate the transfer of photogenerated electrons from CN to MoN. x Migration provides interfacial channels, which is beneficial for the interfacial migration and spatial separation of photogenerated carriers, and enables electrons to further participate in the surface hydrogen evolution reaction.

[0080] Characterization of photogenerated carrier separation and transport dynamics To further reveal the photophysical and electrochemical aspects of Mo2N-Mo 16 The effects of N7 heterojunction co-catalysts on the separation and transport behavior of CN photogenerated carriers, respectively, on 2D-C3N4, Mo2N / CN, and Mo 16 N7 / CN and MoN x The CN composite material was subjected to photoluminescence (PL) spectroscopy, time-resolved photoluminescence (TRPL) decay curves, and transient photocurrent response tests. The results are as follows: Figure 4 As shown.

[0081] 1. Steady-state photoluminescence (PL) spectroscopy analysis Figure 4 a represents the steady-state photoluminescence emission spectrum of each sample. Photoluminescence intensity primarily reflects the recombination rate of photogenerated electron-hole pairs in semiconductor materials; lower fluorescence intensity generally indicates a lower recombination rate of photogenerated carriers and higher separation efficiency. Figure 4 As can be seen, pure CN exhibits the strongest fluorescence emission peak, indicating a relatively fast photogenerated electron-hole recombination rate. When combined with single-phase Mo₂N and Mo... 16 After N7, Mo2N / CN and Mo 16 The PL emission intensity of N7 / CN gradually decreases; while for the dual-phase heterojunction composite material MoN of this invention... x / CN, its fluorescence emission intensity decreased significantly, reaching the lowest level among all tested samples. This result proves that Mo2N-Mo 16After the N7 heterojunction cocatalyst forms a composite structure with CN, it can most effectively suppress the recombination of photogenerated electrons and holes, and significantly improve the spatial separation efficiency of photogenerated carriers.

[0082] 2. Time-Resolved Photoluminescence (TRPL) Lifetime Analysis Figure 4 b represents the TRPL fluorescence lifetime decay curves for each sample. The average lifetime of photogenerated carriers can be assessed by fitting the fluorescence lifetime. Figure 4 As can be seen from b, the fluorescence decay rates of each composite material change compared to pure CN. Among them, MoN... x The / CN composite exhibits faster fluorescence decay behavior, indicating that photogenerated electrons can transfer more rapidly from the CN matrix to Mo2N-Mo. 16 The N7 heterojunction surface. Combined with the electron migration from CN to MoN observed in the aforementioned XPS,... x The TRPL results further confirm from a kinetic perspective that the two-phase heterostructure provides a high-speed channel for the efficient migration of photogenerated carriers, thereby reducing the unproductive recombination of carriers within the bulk phase.

[0083] 3. Transient photocurrent response test and analysis Figure 4 c represents the transient photocurrent response curves (current density-time curves, It curves) of each sample under intermittent visible light irradiation. The photocurrent response intensity and stability directly reflect the material's responsiveness to light energy and the interfacial separation and transport rate of photogenerated electron-hole pairs. Higher photocurrent density indicates better charge separation and transport performance. Figure 4 As can be seen from c, all samples exhibited sensitive and stable photocurrent response characteristics across multiple illumination on / off cycles. Specifically, pure CN showed extremely weak photocurrent response; after introducing a single-phase co-catalyst, Mo2N / CN and Mo... 16 The photocurrent density of N7 / CN is improved; the MoN of this invention... x / CN composites exhibit the highest photocurrent density.

[0084] Theoretical calculations of water molecule adsorption performance To further evaluate MoN x The effect of CN complexation on the adsorption behavior of surface reactants was calculated using first-principles calculations for CN and MoN. x and MoN x The adsorption energy of H2O molecules in the / CN system. The calculation results are as follows: Figure 5 As shown in the figure, E ads This is the adsorption energy.

[0085] Calculation results show that MoN xThe adsorption energy of / CN for H2O is −0.975 eV, which is higher than that of CN (−0.913 eV) and MoN. x -0.675 eV. Under the above calculation model and evaluation system, MoN x / CN exhibits a more favorable H2O adsorption state, indicating that MoN x The formation of a complex interface with CN alters the local electronic structure of the system and enhances the interaction between the complex system and H2O molecules. Therefore, Mo2N-Mo 16 The N7 heterojunction can not only participate in interfacial electronic regulation, but also further improve the adsorption state of water molecules on the catalyst surface after being combined with CN, thus providing favorable conditions for subsequent water molecule activation and photocatalytic hydrogen evolution reaction.

[0086] Visible photocatalytic hydrogen production performance of different samples To evaluate Mo2N-Mo 16 The effect of N7 heterojunction co-catalyst on CN photocatalytic hydrogen production performance, under the same test conditions, on CN and MoN x Mo2N / CN, Mo 16 N7 / CN and MoN x / CN was used to test the visible light catalytic hydrogen production performance. During the test, Pt was used as an auxiliary co-catalyst and triethanolamine as a sacrificial agent. The photocatalytic reaction was carried out under visible light irradiation with a wavelength λ≥420 nm, and the generated hydrogen was detected by gas chromatography.

[0087]

[0088] Table 1 shows that the CN hydrogen production rate of the unsupported Mo-based co-catalyst is 1.95 mmol·g. -1 ·h -1 And biphase MoN x The hydrogen production rate of the co-catalyst itself is only 0.08 mmol·g. -1 ·h -1 MoN x After being loaded onto CN, the resulting MoN x The hydrogen production rate of the CN composite material was significantly increased to 17.15 mmol·g. -1 ·h -1 Approximately CN and MoN x The 8.8 times and 214.4 times that when used alone indicate that MoN x The combination with CN produced a significant synergistic effect, and this performance improvement was not due to MoN. x A simple contribution to the self-catalytic activity.

[0089] To further determine whether the aforementioned performance improvement is solely due to the conventional "molybdenum nitride co-catalyst supported on CN" effect, this invention further incorporates Mo2N / CN and Mo... 16 Two single-phase molybdenum nitride composites, N7 and CN, were used as controls. The results showed that single-phase Mo2N and Mo... 16 The hydrogen production rates of N7 itself are only 0.06 and 0.07 mmol·g, respectively. -1 ·h -1 After being loaded with CN, Mo2N / CN and Mo 16 The hydrogen production rates of N7 / CN increased to 5.67 and 9.44 mmol·g, respectively. -1 ·h -1 This indicates that both single-phase molybdenum nitrides can promote the photocatalytic hydrogen evolution performance of CN to some extent. However, the simultaneous presence of Mo2N / and Mo... 16 MoN₂ with two phases forming a heterogeneous interface x / CN, with a hydrogen production rate of 17.15 mmol·g -1 ·h -1 The values ​​are approximately Mo2N / CN and Mo, respectively. 16 The N7 / CN composites are 3.0 times and 1.8 times higher than the two single-phase molybdenum nitride / CN composites.

[0090] The above comparative results show that the MoN of the present invention... x The excellent photocatalytic hydrogen evolution performance exhibited by / CN cannot be simply attributed to the conventional co-catalytic effect of "supporting molybdenum nitride on CN," but rather to the interaction between Mo2N and Mo. 16 The two-phase heterostructure formed by the coexistence of N7 phases is closely related, especially in Mo2N / CN and Mo. 16 With both N7 and CN showing some promoting effect, MoN x / CN still achieved further and significant performance improvements, indicating that Mo2N-Mo 16 The construction of N7 heterogeneous interfaces produces synergistic effects and technical effects that are different from those of single-phase loading and non-simple superposition.

[0091] Combining HRTEM, XRD, and XPS results, Mo2N and Mo can be confirmed. 16 The formation and interface structure of the two phases N7; further combined with PL, TRPL and transient photocurrent test results, it can be considered that the two-phase Mo2N-Mo 16 N7 heterogeneous interface and MoN xThe composite interface between MoN and CN jointly regulates the interfacial electronic structure and photogenerated carrier behavior of the system, which is beneficial for suppressing the recombination of photogenerated electron-hole pairs and promoting interfacial charge migration. First-principles calculations further demonstrate from a theoretical perspective that this heterointerface can modulate the interfacial electron distribution and related adsorption / reaction processes. The above structural characterization, photoelectric performance tests, and theoretical calculation results corroborate each other, indicating that MoN... x / CN compared to single-phase Mo2N / CN and Mo 16 The N7 / CN exhibits significant performance advantages.

[0092] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A molybdenum nitride co-catalyst-supported carbon nitride composite material, characterized in that, It includes two-dimensional carbon nitride nanosheets and a molybdenum nitride-based cocatalyst supported on the surface of the two-dimensional carbon nitride nanosheets; The molybdenum nitride-based cocatalyst contains Mo2N crystalline phase and Mo. 16 N7 crystal phase, and Mo2N crystal phase is similar to Mo 16 Heterogeneous interfaces are formed between the N7 crystalline phases; The molybdenum nitride-based cocatalyst forms a two-dimensional-two-dimensional heterocomposite structure with the two-dimensional carbon nitride nanosheets.

2. The molybdenum nitride co-catalyst-supported carbon nitride composite material according to claim 1, characterized in that, The two-dimensional carbon nitride nanosheets were obtained by thermal polymerization and exfoliation of the nitrogen-containing precursor g-C3N4. The two-dimensional carbon nitride nanosheets have a layered two-dimensional structure, which is used to provide a molybdenum nitride cocatalyst loading interface and a photogenerated carrier transport channel.

3. The molybdenum nitride co-catalyst-supported carbon nitride composite material according to claim 1, characterized in that, In the molybdenum nitride-based cocatalyst, the Mo2N crystal phase and Mo 16 The N7 crystal phases together form a dual active center structure, and the electronic structure of the composite material is adjusted through the interfacial electronic coupling between the two molybdenum nitride crystal phases. The molybdenum nitride-based cocatalyst is dispersed on the surface of two-dimensional carbon nitride nanosheets to reduce the stacking of two-dimensional carbon nitride nanosheets and increase the number of photocatalytic reaction active sites.

4. The molybdenum nitride co-catalyst-supported carbon nitride composite material according to claim 1, characterized in that, In the molybdenum nitride-based cocatalyst, the Mo2N crystal phase and Mo 16 The mass ratio of N7 crystal phase is 1:10 to 10:1, preferably 1:3 to 3:

1.

5. The molybdenum nitride co-catalyst-supported carbon nitride composite material according to claim 1, characterized in that, The molybdenum nitride-based cocatalyst is loaded in the composite material at a rate of 1–50 wt%, preferably 5–30 wt%.

6. A method for preparing a molybdenum nitride co-catalyst-supported carbon nitride composite material, characterized in that, Includes the following steps: Step 1: Preparation of two-dimensional carbon nitride nanosheets (CN): A nitrogen-containing precursor is subjected to thermal polymerization to obtain graphitic carbon nitride g-C3N4; g-C3N4 is subjected to ultrasonic exfoliation combined with secondary calcination to obtain CN; Step 2: MoN x Preparation of heterojunction molybdenum nitride co-catalysts: A precursor system is formed by mixing a molybdenum source, a zinc salt, and an alkaline modifier, and then dried to obtain an intermediate product. The intermediate product is then heat-treated in a nitrogen-containing reducing atmosphere to form MoN2. x Heterojunction molybdenum nitride co-catalyst; the MoN x Composed of Mo2N crystal phase and Mo 16 N7 crystal phase composition; Step 3: Composite material preparation: The MoN x The heterojunction molybdenum nitride co-catalyst is liquid-phase composited with CN and then dried to obtain MoN. x / CN composite materials.

7. The method for preparing the molybdenum nitride co-catalyst-supported carbon nitride composite material according to claim 6, characterized in that, The nitrogen-containing precursor is melamine; in the preparation of CN, melamine is mixed with a surfactant and heat-treated at 450-550℃ to obtain graphitic carbon nitride. CN was then obtained by ultrasonic exfoliation combined with secondary calcination. The key step in secondary calcination is controlling the heating rate to ≤2℃ / min.

8. The method for preparing the molybdenum nitride co-catalyst-supported carbon nitride composite material according to claim 7, characterized in that, The molybdenum source is ammonium heptamolybdate tetrahydrate; The zinc salt is zinc nitrate hexahydrate; The alkalinity regulator is ammonia water; The heat treatment process uses a N2 / H2 mixed atmosphere, and the heat treatment temperature is 650-750℃. The volume ratio of N2 / H2 is 50:50 to 95:5, preferably 90:10; The flow rate of the mixed atmosphere is 0.1 L / min to 10 L / min, preferably 1 to 5 L / min; The molar ratio of the molybdenum source to the zinc salt is 1:2 to 1:20, preferably 1:5 to 1:10; in the liquid phase composite, the ratio of the MoNx heterojunction molybdenum nitride co-catalyst to CN is 1:99 to 1:1, preferably 5:95 to 30:

70.

9. The application of a molybdenum nitride cocatalyst-supported carbon nitride composite material as described in any one of claims 1 to 5 in photocatalytic hydrogen production.

10. The application according to claim 9, characterized in that, The photocatalytic hydrogen production is visible light-driven water splitting for hydrogen production. The composite material is used to promote photogenerated electron transfer, improve photogenerated carrier separation efficiency and / or enhance hydrogen evolution reaction kinetics; The hydrogen production rate of the composite material is 17.15 mmol·g. -1 ·h -1 .