A manufacturing process for cosmetic-grade powder with controllable ultra-low gloss particle size
By employing a fully dry physical processing technique and airflow pulverization and grading technology, the problem of excessive gloss in synthetic mica in cosmetics has been solved, achieving a long-lasting matte effect and safety, thus meeting the texture requirements of high-end cosmetics.
Patent Information
- Application Number
- CN202611236996.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing synthetic mica tends to produce excessive shine when used in cosmetics. Current matte finishing techniques have poor durability, are prone to migration, and leave a greasy feel on the skin, making it difficult to meet the demands of high-end cosmetics for a matte texture and comfortable feel.
The entire process employs a dry physical processing technique, using airflow pulverization and classification technology to achieve the controllable dissociation of the synthesized mica sheet structure, giving the powder an excellent matte finish and precise particle size distribution, while avoiding the presence of foreign impurities and metal contamination.
It achieves a long-lasting matte finish, stability, and safety, meeting the demand for matte texture in high-end cosmetics, reducing energy consumption and wastewater discharge, adapting to different matte makeup needs, and ensuring product quality uniformity.
Smart Images

Figure CN123102459A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of cosmetic materials technology, and in particular to a manufacturing process for cosmetic-grade powder with controllable particle size and ultra-low gloss. Background Technology
[0002] In the modern cosmetics industry, high-purity flake-like synthetic fluorophlogopite is widely used as an important powder raw material in pearlescent bases and skin-feel fillers. Synthetic mica possesses multiple core advantages, including high flake regularity, pure powder whiteness, excellent acid and alkali resistance, resistance to yellowing during high-temperature cosmetic processing, uniform and stable original luster, and compliant and controllable heavy metal residues. Due to its outstanding physicochemical properties, synthetic mica has become an ideal alternative to traditional talc in the cosmetics industry, and its large-scale procurement allows for cost control, meeting the needs of mass production in the beauty industry.
[0003] However, conventional synthetic mica has a smooth surface and strong specular reflective properties, which can easily create an "oily" visual effect when applied to cosmetics, failing to meet consumers' demand for a matte finish. To address this issue, existing matte treatment methods mainly include silicone coating technology and physically mixed matte powders. However, these existing technologies have significant shortcomings: the matte effect of silicone coating has poor durability and is prone to migration and peeling during use; meanwhile, the matte effect obtained through physical mixing has a greasy feel, failing to meet the stringent requirements of high-end cosmetics for a sophisticated matte texture and comfortable feel.
[0004] Therefore, developing a safe, reliable, stable, and long-lasting matte finish synthetic mica preparation process that can effectively replace talc has become a pressing technical challenge in the cosmetic raw material field. This invention addresses the aforementioned shortcomings of existing technologies by providing a solution using a back-end processing method. This eliminates the need for control at the raw material synthesis stage, avoids the risk of residual foreign impurities, and features a simple and easy-to-operate process that can be directly scaled up for mass production. Summary of the Invention
[0005] The purpose of this invention is to provide a manufacturing process for cosmetic-grade powder with controllable particle size and ultra-low gloss, which solves the problems mentioned in the background art.
[0006] This invention achieves its goal through a manufacturing process for cosmetic-grade powders with controllable ultra-low gloss particle size. Conventional synthetic mica has a smooth surface and strong specular reflection properties, which can easily produce an overly glossy visual effect when used as a cosmetic filler, failing to meet consumers' demand for matte makeup. Existing matting technologies, such as silicone coating or physically mixed matte powders, suffer from technical bottlenecks such as poor durability, easy migration, and an oily feel. This invention employs a fully dry physical processing method, using airflow pulverization and classification technology to achieve controllable dissociation of the sheet-like structure of synthetic mica. While maintaining the purity of the raw materials, this imparts excellent matte effects and precise particle size distribution to the powder, thereby meeting the stringent requirements of high-end cosmetics for matte texture, stability, and safety.
[0007] Furthermore, the manufacturing process for cosmetic-grade powder with controllable particle size and ultra-low gloss provided by the present invention includes the following steps: S1. Raw material pretreatment: Select synthetic mica coarse monomers with a whiteness of not less than 95 and heavy metal residues that meet the requirements of the "Cosmetic Safety Technical Specifications". After coarse crushing, impurity removal and drying, a pretreated material with a particle size of 5-20 mm, a purity of not less than 99% and a moisture content of not more than 0.5% is obtained. S2. Ultrafine grinding by air jet mill: The pretreated material is fed into a supersonic air jet mill and accelerated by nozzles under high pressure dry air of 0.4–0.8 MPa, so that the material is subjected to high-speed impact, shearing and collision to achieve layered dissociation and grinding. The grinding environment temperature is controlled to be a closed negative pressure dry working condition below 80℃. By adjusting the speed of the classifier and the air pressure, the median diameter D50 of the finished powder can be adjusted within the range of 1–15 μm. S3. Airflow classification and collection: The pulverized product enters a multi-stage turbine airflow classifier for online classification. Qualified fine powder is collected under negative pressure by a cyclone separator and a pulse bag dust collector connected in series. Coarse particles are returned to step S2 for further pulverization, forming a closed-loop cycle. S4. Dust-free packaging: The collected qualified fine powder is packaged into 25 kg / bag or 500 kg / ton bag specifications by a dust-free automatic packaging system to obtain cosmetic-grade ultra-low gloss mica powder.
[0008] Furthermore, in step S1, the specific operations of the raw material pretreatment include: coarsely crushing the synthetic mica raw material monomers sequentially through a jaw crusher, removing magnetic impurities using a magnetic separation iron removal device, removing excessively large particles through a vibrating screen, and finally drying them through a rotary drum dryer to reduce the moisture content to below 0.5%; the coarse crushing process controls the output particle size to be 5–20 mm to ensure the uniformity of the feed particle size of the subsequent air jet mill.
[0009] Furthermore, in step S2, the supersonic airflow mill adopts a collision-type airflow pulverization structure, which includes multiple nozzles arranged opposite each other. The nozzle orifice diameter is 1.5–3.0 mm. After being accelerated by the nozzles, the high-pressure dry air forms a supersonic airflow jet. The material in the pulverization chamber undergoes high-speed impact, shearing, and collision with the airflow jet, thereby achieving the dissociation and pulverization of layered mica. The airflow mill is equipped with a classification device, which controls the particle size distribution of the finished powder by adjusting the speed of the classification wheel. The speed range of the classification wheel is 2000–15000 rpm.
[0010] Furthermore, in step S2, by precisely adjusting two key parameters—airflow pressure and classifier speed—the D50 can be continuously adjusted within the range of 1–15 μm: when the airflow pressure is 0.4 MPa and the classifier speed is 2000 rpm, coarse-grained powder with a D50 of approximately 15 μm is produced, suitable for base makeup products requiring a soft matte finish; when the airflow pressure is increased to 0.8 MPa and the classifier speed is increased to 15000 rpm, fine-grained powder with a D50 of approximately 1 μm is produced, suitable for color makeup products requiring an extreme matte finish and a delicate skin feel; intermediate particle sizes can be smoothly transitioned by linearly adjusting these two parameters.
[0011] Furthermore, in step S3, the multi-stage turbine air classifier adopts the centrifugal classification principle. After the pulverized material enters the classifier with the airflow, under the action of the centrifugal force generated by the classifying wheel, the coarse particles fall along the cylinder wall and are sent back to the air mill for further pulverization through the return pipe, while the fine particles pass through the classifying wheel and enter the collection system. The classifier is equipped with at least three classification units to achieve accurate particle size separation, and the batch-to-batch D50 fluctuation rate is controlled within ±5%.
[0012] Furthermore, in step S3, the cyclone separator and the pulse bag filter are connected in series. The qualified fine powder first undergoes preliminary gas-solid separation in the cyclone separator to remove most of the coarse particles and carrier gas. Then, it is finely filtered by the pulse bag filter to capture ultrafine particles with a particle size of less than 1 μm. The negative pressure of the two collection devices is maintained by a Roots blower, and the negative pressure value is controlled within the range of -5 to -15 kPa to ensure the integrity of powder collection.
[0013] Furthermore, in step S4, the dust-free automatic packaging system includes an automatic metering device, a sealed conveying pipeline, and anti-static packaging bags. The packaging process is carried out in an environment with a cleanliness level of not less than 100,000 to prevent the introduction of external pollutants. The packaging specifications are set as small packages of 25 kg / bag or large packages of 500 kg / ton bag to meet the needs of industrial production of different scales.
[0014] Furthermore, the process of this invention adopts a fully dry operation mode, with no liquid media involved in the entire production process from raw material crushing to final packaging. This avoids the drying process required in wet processes, significantly reducing energy consumption and wastewater discharge, which is in line with the development trend of green manufacturing in cosmetics.
[0015] Furthermore, the process of this invention achieves the dissociation and pulverization of mica's sheet-like structure through airflow impact. Compared with traditional wet pulverization methods such as ball milling or sand milling, it can effectively preserve the sheet-like crystal structure of mica. When the sheet-like structure is randomly oriented in the powder, it can produce a diffuse reflection effect on incident light, thereby giving the powder excellent matte properties.
[0016] Furthermore, the process of this invention performs airflow pulverization under closed negative pressure dry conditions. There are no metal wear parts in the pulverization chamber that come into direct contact with the material, which avoids the risk of metal foreign matter contamination caused by traditional mechanical pulverization methods. The heavy metal residue of the produced powder meets the strict requirements of the "Cosmetic Safety Technical Specifications" and can be directly used in high-end cosmetic formulations.
[0017] Furthermore, the process of this invention supports continuous, closed-loop, negative-pressure automated operation mode, with a single production line capacity covering a range of 500–5000 kg / h. It has high equipment utilization, good product quality uniformity between batches, and meets the needs of large-scale industrial production.
[0018] Furthermore, the process of this invention is a back-end physical processing process that does not rely on a specific synthetic mica precursor production section. Whether the synthetic mica raw material is self-produced or purchased externally, it can be directly connected to the production line of this process for processing. The process has strong adaptability and a wide range of applications.
[0019] Compared with the prior art, the beneficial effects of the present invention are mainly reflected in the following aspects: This invention employs a fully dry physical processing technology, eliminating liquid phase intervention from raw material pretreatment to final packaging, achieving zero wastewater discharge, environmental protection, energy saving, and significantly reducing drying costs. The airflow impact dissociation pulverization method preserves the lamellar crystalline structure of mica, giving the powder excellent matte finish and insulation properties. The pulverization process is carried out under closed negative pressure dry conditions, eliminating metal abrasion pollution, and heavy metal residues meet cosmetic-grade requirements. By precisely adjusting the airflow pressure and classifier speed, the D50 is accurately and continuously adjustable within the range of 1–15 μm, meeting different matte makeup effect requirements. The system supports continuous closed negative pressure automated operation, with a single-line capacity covering 500–5000 kg / h, and batch-to-batch D50 fluctuation not exceeding ±5%, meeting the uniformity requirements for industrial-scale mass production. The process is a back-end physical treatment, not dependent on specific synthetic mica precursors, with strong raw material adaptability, and can flexibly incorporate compliant coarse powder from self-production or external purchase for processing. Attached Figure Description
[0020] Figure 1 This is the main process flow diagram of the manufacturing process of cosmetic-grade powder with controllable particle size for ultra-low gloss according to the present invention; Figure 2 This is an electron microscope image of 2-micron synthetic fluorinated phlogopite mica produced by the manufacturing process of cosmetic-grade powder with controllable ultra-low gloss particle size according to the present invention. Figure 3 This is an electron microscope image of 4-micron synthetic fluorinated phlogopite mica, produced using the manufacturing process of cosmetic-grade powder with controllable ultra-low gloss particle size according to the present invention. Figure 4 This is an electron microscope image of 9-micron synthetic fluorinated phlogopite mica, produced using the ultra-low gloss, controllable particle size cosmetic-grade powder manufacturing process of this invention. Figure 5 This is a gloss comparison table for products manufactured using the ultra-low gloss, controllable particle size cosmetic-grade powder manufacturing process of this invention. Figure 6 This is a simplified product formulation table for the manufacturing process of cosmetic-grade powder with controllable particle size for ultra-low gloss, as described in this invention. Figure 7 This invention provides a product drop test table for the manufacturing process of cosmetic-grade powder with controllable particle size and ultra-low gloss. Detailed Implementation
[0021] The specific embodiments of the present invention will be described in further detail below with reference to the accompanying drawings. Those skilled in the art should understand that the following embodiments are for illustrative purposes only and are not intended to limit the scope of protection of the present invention.
[0022] I. Detailed Description of the Overall Mechanical Architecture of the System Reference Figure 1 As shown, the system architecture of the cosmetic-grade powder manufacturing process with controllable particle size and ultra-low gloss provided by this invention includes a raw material input unit, a pretreatment unit, an airflow pulverization unit, an airflow classification and collection unit, and a dust-free packaging unit. These units are connected in series to form a complete closed-loop dry production process. Synthetic mica coarse monomers first enter the pretreatment unit via the raw material input unit. After coarse crushing, impurity removal, and drying, pretreated material meeting particle size requirements is obtained. The pretreated material then enters the airflow pulverization unit through a closed conveying pipeline for ultra-fine dissociation pulverization. The pulverized product undergoes particle size sorting and negative pressure collection via the airflow classification and collection unit. Qualified fine powder is finally packaged into finished products via the dust-free packaging unit. The entire production process operates continuously under closed negative pressure conditions, achieving a fully dry operation mode. From raw material input to finished product output, no liquid media intervenes, avoiding the drying process required in wet processes. This significantly reduces energy consumption and wastewater discharge, aligning with the development trend of green manufacturing in cosmetics.
[0023] In the system architecture, material transfer between units is achieved through negative pressure conveying pipelines, with the negative pressure maintained by Roots blowers located between units. The raw material input unit is equipped with an automatic metering device to precisely control the material flow rate into the pretreatment unit, ensuring stable operation of subsequent processes. The pretreatment unit includes a jaw crusher, magnetic separation equipment, vibrating screen, and rotary dryer, sequentially performing coarse crushing, impurity removal, and drying functions. The core equipment of the air jet mill is a supersonic air jet mill, which internally incorporates a collision-type nozzle assembly and a classifying rotor, achieving layered dissociation and pulverization of mica sheet structures under high-pressure dry air. The air jet classification and collection unit includes a multi-stage turbine air classifier, a cyclone separator, and a pulse bag filter, connected in series to form a classification and collection system, effectively separating qualified fine powder from coarse particles. The cleanroom packaging unit is equipped with an automatic metering device, sealed conveying pipelines, and anti-static packaging bags, completing the final product packaging in an environment with a cleanliness level of at least 100,000.
[0024] II. Detailed Structure and Operation Instructions of the Raw Material Pretreatment Unit Reference Figure 1 The process layout of step S1, specifically the structure of the raw material pretreatment unit, includes the following components: a jaw crusher, as a coarse crushing device, is located at the beginning of the pretreatment unit to crush the synthetic mica coarse particles to a particle size range of 5 to 20 mm; a magnetic separation iron removal device is located downstream of the jaw crusher to remove magnetic metal impurities mixed in during the coarse crushing process; a vibrating screen is located after the magnetic separation iron removal device to screen out oversized particles exceeding 20 mm and non-target impurities; and a rotary dryer is located downstream of the vibrating screen to reduce the moisture content of the material to below 0.5%.
[0025] In the specific operation of raw material pretreatment, the synthetic mica coarse monomers are first uniformly fed into the working chamber of the jaw crusher through the feeding device. The jaw crusher adopts a crushing chamber structure composed of a moving jaw and a fixed jaw. Under the compression and bending action generated by the periodic reciprocating motion of the moving jaw, the material is crushed into particles of 5 to 20 mm. The crushed material is discharged through the discharge port and enters the magnetic separation and iron removal equipment. The magnetic separation and iron removal equipment uses the magnetic attraction force generated by permanent magnets or electromagnets to adsorb and separate magnetic impurities such as iron filings in the material. The purified material continues to enter the vibrating screen device. The vibrating screen device is equipped with multiple layers of screens. The material is screened layer by layer under the vibration generated by the vibrator. The material that meets the particle size requirements passes through the screen and enters the next process. Large particles with a particle size exceeding 20 mm are discharged from the screen surface and returned to the jaw crusher for re-crushing. Finally, the material meeting the particle size requirements enters the rotary drum dryer. The dryer is equipped with a hot air circulation system, and the hot air temperature is controlled within the range of 120 to 150 degrees Celsius. The material, under the tumbling action of the lifting plates on the inner wall of the drum, comes into full contact with the hot air, achieving uniform drying. During the drying process, the moisture content of the material gradually decreases to below 0.5%, meeting the moisture content requirements for air classifier feed. The pre-treated material, after drying, is discharged through a closed discharge device and, after cooling, proceeds to the next process.
[0026] The design parameters of the raw material pretreatment unit fully consider the adaptability of the process and the product quality requirements. The jaw crusher's crushing ratio is set to 3:1 to 5:1 to ensure that the output particle size is stable within the range of 5 to 20 mm. The magnetic field strength of the magnetic separation iron removal equipment is set to 800 to 1500 Gauss, which can effectively remove residual ferromagnetic impurities in the material. The screen aperture of the vibrating screen device is set to 20 mm, and the screening efficiency is not less than 95%. The drying temperature of the rotary drum dryer is set to 120 to 150 degrees Celsius, and the drying time is 1 to 2 hours. The residence time of the material in the drying drum is precisely controlled by the rotation speed and tilt angle to ensure that the moisture content is uniformly reduced to below 0.5%. The purity of the pretreated material is not less than 99%, the whiteness is not less than 95, and the heavy metal residue meets the strict requirements of the "Cosmetic Safety Technical Specifications".
[0027] III. Detailed Structure and Working Principle of Supersonic Airflow Mill Reference Figure 2 As shown, the supersonic air jet mill is the core equipment of the process of this invention. Its detailed structure includes the main shell of the air jet mill, the feed inlet, the impact nozzle assembly, the grinding chamber, the classifying wheel rotor, the classifying wheel drive motor, the high-pressure drying air inlet, the airflow acceleration channel, the finished powder outlet, the temperature monitoring sensor, and the pressure monitoring sensor. The assembly relationship and spatial layout of the various components determine the grinding performance and classification accuracy of the air jet mill.
[0028] The main body of the air jet mill is a cylindrical pressure vessel, with a sealed grinding chamber inside. The shell material is stainless steel or wear-resistant alloy to ensure long-term stable operation under high-pressure airflow. The feed inlet is located on the top or side wall of the air jet mill and is connected to the discharge port of the pretreatment unit through a sealed pipe. The material enters the grinding chamber through negative pressure suction. The impact nozzle assembly is the core grinding mechanism of the air jet mill, containing multiple oppositely arranged nozzles with nozzle orifice diameters of 1.5 to 3.0 mm. High-pressure dry air enters the airflow acceleration channel through the high-pressure dry air inlet and is accelerated through the nozzle orifices to form a supersonic airflow jet. The multiple nozzles are symmetrically arranged, so that the high-speed airflow jet forms an impact state in the central area of the grinding chamber. After entering the grinding chamber, the material is first accelerated by the high-speed airflow jet, and then undergoes high-speed impact, shearing, and collision with the airflow jet in the nozzle impact area.
[0029] The working principle of the supersonic air jet mill is based on a layered dissociation pulverization mechanism. Synthetic mica has a typical layered silicate crystal structure with weak interlayer bonding. This invention utilizes a high-speed airflow driven by high-pressure dry air to impact the mica layers, causing the interlayer bonding to dissociate under external force, thereby achieving effective separation of the sheet-like structure. Compared with traditional wet pulverization methods such as ball milling or sand milling, air jet impact pulverization can effectively preserve the sheet-like crystal structure of mica. When the sheet-like structure is randomly oriented in the powder, it can produce a diffuse reflection effect on incident light, thus giving the powder excellent matte properties.
[0030] The grinding chamber is equipped with a classifying wheel rotor, which is driven to rotate by a classifying wheel drive motor. The rotation speed of the classifying wheel rotor ranges from 2000 to 15000 rpm, and the particle size distribution of the finished powder can be controlled by adjusting the rotation speed. After the material is dissociated and pulverized in the grinding chamber, it rises with the airflow into the classification area. Fine particles are carried by the airflow through the classifying wheel and enter the finished powder outlet, while coarse particles are thrown against the cylinder wall by the centrifugal force generated by the classifying wheel and fall down the cylinder wall, returning to the grinding chamber through the return pipe for further pulverization, forming a closed-loop circulation grinding process. The airflow mill is equipped with temperature and pressure monitoring sensors to monitor the temperature and pressure conditions inside the grinding chamber in real time. The grinding environment is controlled at a closed negative pressure dry process with the temperature below 80 degrees Celsius to avoid thermal damage to the mica crystal structure caused by high temperatures.
[0031] In the implementation of the supersonic airflow mill, airflow pressure and classifier speed are two key parameters for achieving continuous adjustment of the D50 within the range of 1 to 15 micrometers. When the airflow pressure is 0.4 MPa and the classifier speed is 2000 rpm, coarse-grained powder with a D50 of approximately 15 micrometers is produced. This product specification is suitable for base makeup products requiring a soft matte finish, providing a natural and soft matte effect. When the airflow pressure is increased to 0.8 MPa and the classifier speed is increased to 15000 rpm, fine-grained powder with a D50 of approximately 1 micrometer is produced. This product specification is suitable for color makeup products requiring an extreme matte finish and a delicate skin feel, providing a silky and smooth skin experience. Intermediate particle sizes can be smoothly transitioned by linearly adjusting both the airflow pressure and classifier speed. This precise particle size adjustment capability allows the process of this invention to meet the differentiated matte requirements of various cosmetic formulations.
[0032] IV. Detailed Structure and Operation Instructions of the Airflow Classification and Collection System Reference Figure 3 As shown, the airflow classification and collection system is a combination of a multi-stage turbine airflow classifier, a cyclone separator, a pulse bag filter, and a Roots blower. Its function is to achieve particle size separation of the pulverized products and negative pressure collection of qualified fine powder. The detailed structure of the airflow classification and collection system includes a multi-stage turbine airflow classifier, a classifying wheel assembly, a classifying chamber, a cyclone separator, a pulse bag filter, a Roots blower, a qualified fine powder outlet, a coarse particle return pipeline, a negative pressure conveying pipeline, a pulse backflushing device, and a bag filter assembly.
[0033] The multi-stage turbine air classifier is located downstream of the air classifier, with its classification chamber connected to the finished powder outlet of the air classifier via a negative pressure conveying pipeline. Inside the classification chamber is a classifying wheel assembly, driven by a high-speed motor to generate a controllable centrifugal force field. After being pulverized, the material enters the classification chamber with the airflow and is separated under the centrifugal force generated by the classifying wheels: larger particles experience greater centrifugal force, fall along the cylinder wall, and return to the air classifier for further pulverization via the coarse particle return pipe; smaller particles experience less centrifugal force and are carried by the airflow through the classifying wheels into the subsequent collection system. The multi-stage turbine air classifier has at least three classification units, achieving precise particle size separation with batch-to-batch D50 fluctuation controlled within ±5%, ensuring product quality uniformity and stability.
[0034] After being separated by an air classifier, the qualified fine powder enters a cyclone separator for preliminary gas-solid separation. The cyclone separator utilizes the principle of centrifugal sedimentation, causing the dust-laden airflow to rotate within the separator. Particles are thrown against the separator wall by centrifugal force and fall along the wall to the bottom discharge port, while the purified airflow exits from the top. The cyclone separator removes most of the coarse particles and carrier gas from the airflow, reducing the filtration load on the subsequent pulse-jet baghouse dust collector. The airflow, after preliminary separation by the cyclone separator, then enters the pulse-jet baghouse dust collector for fine filtration. The pulse-jet baghouse dust collector contains multiple filter bag assemblies. The filter bags are made of special high-temperature and corrosion-resistant fiber fabric, capable of capturing ultrafine particles smaller than 1 micrometer. When the dust accumulation on the filter bag surface reaches a certain thickness, the pulse-jet backflushing device automatically activates. Compressed air is injected instantaneously into the filter bag through the blowpipe, causing the filter bag to vibrate at high frequency, shaking off the dust adhering to the filter bag surface into the ash hopper, achieving online cleaning and regeneration of the filter bags.
[0035] The entire air classifier and collection system operates under negative pressure, maintained by a Roots blower. The negative pressure value is controlled within the range of -5 to -15 kPa to ensure the integrity of powder collection and the reliability of the conveying process. Qualified fine powder is discharged from the qualified fine powder outlet of the pulse bag filter and sent to the dust-free packaging system through a closed pipeline. Coarse particles are returned to the air classifier through a return pipeline located between the air classifier and the air mill, forming a closed-loop recycling process that effectively improves material utilization and production capacity.
[0036] V. Detailed Structure and Operation Instructions of the Cleanroom Packaging System Reference Figure 1 The process layout for step S4, the cleanroom automated packaging system, includes an automatic metering device, a sealed conveying pipeline, and anti-static packaging bags. The automatic metering device is located between the qualified fine powder outlet of the pulse-jet bag filter and the packaging station to accurately weigh each batch of product. The sealed conveying pipeline connects the automatic metering device to the packaging station, ensuring that the powder does not come into contact with the external environment during transport. The anti-static packaging bags are made of composite materials with good static dissipation properties, preventing dust generation or metering errors caused by static adsorption of powder during packaging.
[0037] The cleanroom packaging system operates in an environment with a cleanliness level of at least 100,000. Packaging stations are equipped with clean workbenches and air purification devices to effectively control the concentration of airborne particles. Packaging specifications include two sizes: 25 kg per bag and 500 kg per ton bag. Small packages use paper-plastic composite bags with an inner PE film liner, suitable for small to medium-sized customers; large packages use ton-sized bulk containers, suitable for large-scale industrial production and batch supply. During the packaging process, an automatic weighing device uses high-precision weighing sensors to accurately control the weight of each bag or package, with packaging accuracy controlled within ±0.5%. After packaging, the finished products are inspected and approved before being stored in the warehouse. The entire packaging process is automated, reducing the risk of contamination from manual operation.
[0038] VI. Complete Operation Flow and Method Examples of Manufacturing Process Based on the above system structure, the complete operation flow of the ultra-low gloss, controllable particle size cosmetic-grade powder manufacturing process of the present invention includes the following steps: S1. Raw Material Pretreatment Stage: Synthetic mica coarse monomers with a whiteness of not less than 95 and heavy metal residues meeting the requirements of the "Cosmetic Safety Technical Specifications" are selected as raw materials. The raw materials are sequentially coarsely crushed using a jaw crusher, controlling the output particle size to be 5 to 20 mm to ensure the uniformity of particle size in the subsequent air jet mill feed. The coarsely crushed material is then subjected to magnetic separation to remove magnetic impurities, followed by a vibrating screen to remove oversized particles and non-target impurities. Finally, it is dried using a rotary dryer to reduce the moisture content to below 0.5%, obtaining a pretreated material with a purity of not less than 99%.
[0039] S2. Airflow Ultrafine Grinding Stage: The pretreated material is fed into the feed inlet of the supersonic airflow mill via a negative pressure conveyor. High-pressure dry air is generated by an air compression system and regulated to 0.4 to 0.8 MPa before entering the high-pressure dry air inlet of the airflow mill. It then enters the impact nozzle assembly through the airflow acceleration channel. In the nozzle impact zone, the pretreated material undergoes high-speed impact, shearing, and collision with the supersonic airflow, achieving the dissociation and pulverization of layered mica. During the pulverization process, a temperature monitoring sensor continuously monitors the temperature inside the pulverization chamber to ensure the ambient temperature remains below 80 degrees Celsius, preventing thermal damage. The pulverized product is classified online under the centrifugal force generated by the classifying wheel. The classifying wheel speed is continuously adjustable within the range of 2000 to 15000 rpm, achieving precise control of the median diameter (D50) of the finished powder within the range of 1 to 15 micrometers.
[0040] S3. Airflow Classification and Collection Stage: The pulverized product enters the classification chamber of the multi-stage turbine airflow classifier with the airflow, where it undergoes particle size separation under the centrifugal force generated by the classifying wheel assembly. Coarse particles fall along the cylinder wall and return to the airflow mill for further pulverization via the coarse particle return pipe, forming a closed-loop cycle. Qualified fine powder passes through the classifying wheel and enters the cyclone separator for preliminary gas-solid separation, removing most of the coarse particles and carrier gas. Subsequently, the airflow enters the pulse bag filter for fine filtration, capturing ultrafine particles with a diameter of less than 1 micrometer. Both collection devices operate under negative pressure maintained by a Roots blower, with the negative pressure value controlled within the range of -5 to -15 kPa to ensure the integrity of powder collection.
[0041] S4. Cleanroom Packaging Stage: The collected qualified fine powder is conveyed through a closed pipeline to an automatic metering device. After precise weighing, it enters the packaging station for dispensing. Packaging is carried out in an environment with a cleanliness level of no less than 100,000, using anti-static packaging bags, and is packaged into 25 kg bags or 500 kg ton bags according to customer requirements. After packaging and passing inspection, cosmetic-grade ultra-low gloss mica powder is obtained.
[0042] As a specific embodiment of the present invention, cosmetic-grade ultra-low gloss mica powder is prepared using the above-described process, and its particle size distribution curve is as follows: Figure 4 As shown. From Figure 4 As can be seen, the particle size distribution curve exhibits a single-peak distribution, with a median diameter (D50) of approximately 4 micrometers. The particle size is mainly distributed within the range of 1 to 15 micrometers, verifying the precise control capability of the airflow milling and classification process over the particle size distribution. The scanning electron microscope (SEM) morphology of the powder product obtained in this embodiment is shown below. Figure 5 As shown, from Figure 5 It can be clearly observed that the mica powder maintains a complete flaky structure with intact edges and clear outlines. The thickness and diameter-to-thickness ratio are evenly distributed, and there is no obvious breakage, pulverization or amorphization. This confirms the technical advantages of the dry airflow pulverization process in maintaining the natural flaky crystal structure of mica.
[0043] VII. Engineering methods to overcome the defects of the prior art in the process of this invention To address the shortcomings of existing technologies revealed in the background section, this invention provides a systematic solution from an engineering implementation perspective. The background section points out that conventional synthetic mica has a smooth surface and strong specular reflective properties, which can easily produce an overly glossy visual effect when used as a cosmetic filler, failing to meet consumers' demand for matte makeup. To address this problem, this invention employs an airflow impact dissociation pulverization method to retain the lamellar crystalline structure of mica. When the lamellar structure is randomly oriented within the powder, it can produce a diffuse reflection effect on incident light, thereby endowing the powder with excellent matte properties. Figure 5Scanning electron microscope images confirm that the powder prepared by the process of this invention does indeed maintain a complete lamellar structure with clear and complete lamellar edges, which provides a structural basis for achieving an excellent matte effect.
[0044] Background technology also points out that existing matte finishing methods, such as silicone coating technology, suffer from poor durability and easy migration and detachment, while physical mixing of matte powders results in an oily feel on the skin. This invention employs a completely dry physical processing method, without using any silicone coating agents or matte powder additives, fundamentally avoiding the problems of silicone coating layer migration and detachment during use. Simultaneously, because the process of this invention retains the natural flake structure of mica, the accumulation of flake powder on the skin surface provides a dry and comfortable feel, avoiding the oily discomfort caused by physical mixing methods.
[0045] The background technology mentions that existing technologies pose a risk of residual foreign impurities. This invention's process utilizes airflow pulverization under closed, negative pressure dry conditions. No metal wear parts directly contact the material within the pulverization chamber, avoiding the risk of metal contamination associated with traditional mechanical pulverization methods. In the raw material pretreatment stage, magnetic impurities are removed using magnetic separation equipment. Heavy metal residues meet the stringent requirements of the "Cosmetic Safety Technical Specifications," allowing for direct use in high-end cosmetic formulations. This invention's process is a back-end physical processing technology, independent of specific synthetic mica precursor production lines. Both self-produced and purchased compliant synthetic mica rough can be directly fed into this process line for processing, demonstrating strong process adaptability and a wide range of applications.
[0046] VIII. Engineering Design and Implementation of Key Process Parameters The core technical feature of this invention lies in achieving continuous adjustment of the particle size distribution (D50) within the range of 1 to 15 micrometers by precisely regulating two key parameters: airflow pressure and classifier speed. These two parameters have a clear engineering correspondence with the finished particle size: when the airflow pressure is 0.4 MPa and the classifier speed is 2000 rpm, the acceleration energy of the airflow on the material is relatively low, resulting in a longer residence time of the material in the crushing chamber and producing coarse-sized powder with a D50 of approximately 15 micrometers; when the airflow pressure is increased to 0.8 MPa and the classifier speed is increased to 15000 rpm, the acceleration energy of the airflow is significantly enhanced, resulting in more intense impact crushing of the material and producing fine-sized powder with a D50 of approximately 1 micrometer. Intermediate particle sizes can be smoothly transitioned through linear adjustment of these two parameters. This parameterized particle size control method has the advantages of simple operation and fast adjustment response, and can meet the differentiated particle size requirements of different batches of products.
[0047] The design of the airflow classification and collection system also embodies the concept of precise engineering control. The multi-stage turbine airflow classifier generates a controllable centrifugal force field through the classifying wheel assembly, achieving precise separation of coarse and fine particles. The classifying wheel assembly has at least three classification units, with each unit's classification accuracy working in tandem to form a multi-stage sorting process from coarse to fine, effectively improving classification accuracy and efficiency. The batch-to-batch D50 fluctuation rate is controlled within ±5%, ensuring the uniformity and stability of product quality. The cyclone separator and pulse-jet bag filter are connected in series; the former performs coarse separation, and the latter performs fine filtration. Their collaborative operation ensures both collection efficiency and collection integrity.
[0048] The entirely dry operation mode is another important engineering feature of the process of this invention. From raw material pretreatment to final packaging, no liquid media are involved in the entire production process, avoiding the drying process required in wet processes, significantly reducing energy consumption and wastewater discharge. At the same time, the dry operation mode avoids contact between materials and water, preventing powder agglomeration or deterioration caused by moisture introduction, which is beneficial to the stability of product quality.
[0049] IX. Technical Support and Production Capacity Design for Industrial Applications This invention supports continuous, closed-loop, negative-pressure automated operation. A single production line can handle capacities ranging from 500 to 5000 kg / hour, with high equipment utilization and flexible capacity adjustments to meet varying production needs. The selection and configuration of each unit within the system are engineered to ensure material balance and stable operation of each process within the rated capacity range.
[0050] The supersonic air jet mill in the airflow pulverizer unit employs a collision-type airflow pulverization structure. Its nozzle quantity, orifice diameter, and arrangement are optimized to reduce energy consumption and wear on equipment components while ensuring pulverization efficiency. The classifier's drive motor is a variable frequency speed-regulating motor, enabling continuous and precise adjustment of the classifying speed. The classifier's classifying wheel assembly is made of wear-resistant material, maintaining sorting accuracy during long-term operation. The pulse jet bag filter's filter cartridge assembly features a modular design for easy replacement and maintenance. The Roots blower's airflow and pressure are selected based on system resistance calculations to ensure stable maintenance of negative pressure.
[0051] The automatic metering device of the dust-free automated packaging system employs high-precision weighing sensors and a closed-loop control system, enabling accurate measurement and rapid response. The sealed conveying pipeline features a smooth inner wall design, reducing powder adhesion and accumulation during transport. The anti-static packaging bags are made of highly conductive materials, effectively dissipating static electricity generated during powder transport and packaging, avoiding measurement errors and dust problems caused by electrostatic adsorption.
[0052] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A manufacturing process for cosmetic-grade powder with controllable particle size and ultra-low gloss, characterized in that, Includes the following steps: S1. Raw material pretreatment: Select synthetic mica coarse monomers, and after coarse crushing, impurity removal and drying, obtain pretreated material with a particle size of 5-20mm, purity of not less than 99% and moisture content of not more than 0.5%. S2. Ultrafine Grinding by Airflow Mill: The pretreated material is fed into a supersonic airflow mill and accelerated through nozzles under high-pressure dry air (0.4–0.8 MPa). This causes the material to be subjected to high-speed impact, shearing, and collision to achieve layered dissociation and grinding. By adjusting the speed of the classifier and the airflow pressure, the median diameter D50 of the finished powder can be adjusted within the range of 1–15 μm. S3. Airflow Classification and Collection: The pulverized product enters a multi-stage turbine airflow classifier for online classification. Qualified fine powder is collected under negative pressure by a cyclone separator and a pulse bag filter connected in series. Coarse particles are returned to step S2 for further grinding. S4. Dust-free packaging: The collected qualified fine powder is packaged by a dust-free automatic packaging system to obtain cosmetic-grade ultra-low gloss mica powder.
2. The manufacturing process for cosmetic-grade powder with controllable particle size and ultra-low gloss as described in claim 1, characterized in that, In step S1, the specific operations of the raw material pretreatment include: coarsely crushing the synthetic mica raw material monomers sequentially through a jaw crusher, removing magnetic impurities using a magnetic separation iron removal device, removing excessively large particles through a vibrating screen, and finally drying them through a rotary drum dryer to reduce the moisture content to below 0.5%.
3. The manufacturing process for cosmetic-grade powder with controllable particle size in ultra-low gloss as described in claim 1, characterized in that, In step S2, the supersonic airflow mill adopts a collision-type airflow pulverization structure, which includes multiple nozzles arranged opposite each other. The nozzle orifice diameter is 1.5–3.0 mm. After being accelerated by the nozzles, the high-pressure dry air forms a supersonic airflow jet. The material in the pulverization chamber undergoes high-speed impact, shearing and collision with the airflow jet.
4. The manufacturing process for cosmetic-grade powder with controllable particle size and ultra-low gloss as described in claim 1, characterized in that, In step S2, by precisely adjusting two key parameters, the airflow pressure and the classifier speed, the D50 can be continuously adjusted within the range of 1–15 μm. When the airflow pressure is 0.4 MPa and the classifier speed is 2000 rpm, coarse-sized powder with a D50 of approximately 15 μm is produced. When the airflow pressure is 0.8 MPa and the classifier speed is 15000 rpm, fine-sized powder with a D50 of approximately 1 μm is produced.
5. The manufacturing process for cosmetic-grade powder with controllable particle size and ultra-low gloss as described in claim 1, characterized in that, In step S3, the multi-stage turbine airflow classifier is equipped with at least three classification units to achieve precise particle size separation and control the batch-to-batch D50 fluctuation rate within ±5%.
6. The manufacturing process for cosmetic-grade powder with controllable particle size in ultra-low gloss as described in claim 1, characterized in that, In step S4, the dust-free automatic packaging system is operated in an environment with a cleanliness level of not less than 100,000, and the packaging specifications are set at 25kg / bag or 500kg / ton bag.