A nano-corrosion-resistant conductive coating grounding material and its environmentally friendly preparation process
By employing an environmentally friendly preparation process for nano-corrosion-resistant conductive coating grounding materials, and utilizing dual-coating and electric field-oriented treatment, the corrosion problem of grounding materials in harsh environments has been solved, achieving a balance between conductivity and corrosion resistance, and reducing environmental pollution and resistivity.
Patent Information
- Application Number
- CN202611532874.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing grounding materials are prone to corrosion in harsh environments, making it difficult to balance conductivity and corrosion resistance. Traditional coating processes cause serious pollution and have low coating utilization rates.
An environmentally friendly manufacturing process for grounding materials using a nano-corrosion-resistant conductive coating is employed. Through double-coating and electric field orientation treatment, an interlocking structure is formed between the layers. Combined with environmentally friendly epoxy resin, nano-conductive carbon black, and other components, a balance between conductivity and corrosion resistance is achieved.
It reduces coating resistivity, improves resistance to media penetration, reduces environmental pollution, is suitable for continuous production, and significantly improves conductivity and corrosion resistance.
Smart Images

Figure CN123102601A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lightning protection grounding materials technology, and more specifically, to a nano-corrosion-resistant conductive coating grounding material, and also to an environmentally friendly preparation process for the nano-corrosion-resistant conductive coating grounding material. Background Technology
[0002] Lightning protection grounding systems are crucial for the safe operation of infrastructure in sectors such as power, petrochemicals, and communications. The conductivity and corrosion resistance of grounding materials directly determine the service life and operational reliability of the grounding system. Currently, the industry commonly uses ordinary hot-dip galvanized metal materials for traditional grounding. While these materials possess basic conductivity, the zinc coating thickness is only 30-40 μm, making them highly susceptible to corrosion in harsh environments such as the acidic and alkaline atmospheres of petroleum refining and the salt spray corrosion of coastal mudflats. This leads to increased grounding resistance, system failure, and a significantly shortened service life.
[0003] With the development of nanomaterials technology, existing technologies have begun to attempt to improve corrosion resistance and conductivity by preparing nano-coatings on the surface of grounding materials. However, existing solutions have many drawbacks. At the coating formulation level, the conductive fillers in conventional conductive coatings are randomly distributed, requiring a high filling threshold to form a continuous conductive path. However, high filling amounts degrade the coating's density, adhesion, and corrosion resistance, creating an inherent trade-off between conductivity and corrosion resistance. Moreover, at the manufacturing process level, the mainstream coating methods include liquid air pressure spraying, electrostatic spraying, and powder spraying, all of which generate a large amount of coating dust or volatiles, resulting in low coating utilization and serious environmental pollution. Furthermore, the coating cannot achieve a uniform effect after formation.
[0004] Therefore, there is an urgent need to develop a new technical solution to address the related issues in the production of grounding materials. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a nano-corrosion-resistant conductive coating grounding material and its environmentally friendly preparation process. The production and preparation process is relatively environmentally friendly and can solve the technical problem that the conductivity and corrosion resistance of existing grounding material coatings are difficult to balance.
[0006] To achieve the above objectives, the present invention adopts the following technical solution:
[0007] An environmentally friendly preparation process for a nano-corrosion-resistant conductive coating grounding material includes the following steps:
[0008] S1: The flat steel is leveled and straightened, and the surface of the flat steel is ground.
[0009] S2: Mix the raw materials of the nano-corrosion-resistant conductive coating according to the mass percentage, and disperse them in a disperser to obtain the nano-corrosion-resistant conductive coating.
[0010] S3: The flat steel surface is coated with a nano-anti-corrosion and conductive coating through the soft silicone feeder of the composite machine to form the first layer of coating;
[0011] S4: The flat steel coated with the first layer of paint is sent into the dryer and dried at a temperature of 50~60℃ for 110s~120s to make the first layer of paint reach the surface dry state.
[0012] S5: The surface of the flat steel in the surface-dry state is coated with a nano-anti-corrosion and conductive coating through the soft silicone feeder of the composite machine to form a second coating layer.
[0013] S6: The flat steel coated with the second layer of coating is sent into the dryer to dry. The first and second layers of coating together form a cured nano-anti-corrosion and conductive coating on the outside of the flat steel.
[0014] Further, in step S3, the thickness of the first coating layer is 70~80μm; in step S4, the thickness of the second coating layer is 70~80μm; in step S6, the thickness of the cured nano-anti-corrosion conductive coating is 150~160μm.
[0015] Furthermore, the nano-corrosion-resistant conductive coating is made from the following raw materials in the following mass percentages: 30-40% environmentally friendly epoxy resin, 4-8% silicone rubber, 6-10% nano-conductive carbon black, 5-9% conductive powder, 1-3% zinc powder, 0.5-1.5% anti-deposition agent, 2.5-4.5% accelerator, 1-3% leveling agent, 0.3-0.8% polymer wetting agent, 22-32% diluent, and 6-10% curing agent, with the sum of the mass percentages of each component being 100%.
[0016] Furthermore, the nano-corrosion-resistant conductive coating is made from the following raw materials in the indicated weight percentages: 35% environmentally friendly epoxy resin, 6% silicone rubber, 8% nano-conductive carbon black, 7% conductive powder, 2% zinc powder, 1% anti-deposition agent, 3.5% accelerator, 2% leveling agent, 0.5% polymer wetting agent, 27% diluent, and 8% curing agent.
[0017] Furthermore, the environmentally friendly epoxy resin is composed of 5% organosilicon resin, 56% glycidylamine epoxy resin, and 39% bisphenol A epoxy resin in a mass ratio; the diluent is one or a combination of two of environmentally friendly epoxy reactive diluent and xylene.
[0018] Furthermore, in step S2, a cooling device is installed on the outer periphery of the disperser cylinder. During the dispersion process, the temperature is maintained by cooling through this device. The mixing of the raw materials for the nano-corrosion-resistant conductive coating includes the following steps:
[0019] S21: Environmentally friendly epoxy resin and silicone rubber are added to a disperser in a certain proportion for dispersion; then diluent and anti-deposition material are added in a certain proportion for dispersion to form a base resin;
[0020] S22: Add nano-conductive carbon black, conductive powder, and zinc powder to a ball mill in proportion and grind them until the particle size is less than 1 micrometer to form conductive powder intermediate material;
[0021] S23: Add the ground conductive powder intermediate material to the well dispersed base resin in proportion and disperse it.
[0022] S24: Add accelerator, leveling agent and polymer wetting agent in proportion and disperse to obtain semi-finished coating;
[0023] S25: When using, add curing agent to the semi-finished coating in proportion, and then disperse it in a disperser to obtain nano-anti-corrosion and conductive coating.
[0024] Furthermore, the entire drying process from step S3 to step S4 is subjected to a first electric field orientation treatment; the conductive filler in the first layer of coating is oriented in a direction perpendicular to the surface of the flat steel under the continuous action of the DC electric field.
[0025] The entire drying process from step S5 to step S6 involves a second electric field orientation treatment; the conductive filler in the second coating layer migrates and accumulates on the outer surface, forming a highly conductive surface area, and some of the conductive filler is embedded in the microscopic depressions on the surface of the first coating layer, forming an interlayer interlocking structure between the first and second coating layers.
[0026] Furthermore, both the first and second electric field orientation treatments apply an electric field perpendicular to the surface of the flat steel. The flat steel serves as the negative electrode, and a mesh of positive electrodes is symmetrically arranged on both the upper and lower sides of the flat steel, with the mesh of positive electrodes maintaining a non-contact gap of 0.5~1mm with the surface of the flat steel. The DC electric field strength of the first electric field orientation treatment is 600~1200V / cm, and the DC electric field strength of the second electric field orientation treatment is 1200~2000V / cm.
[0027] Furthermore, in step S6, a stepped temperature curing process is adopted, first maintaining the temperature at 40~45℃ for 25~35s, and then raising the temperature to 55~60℃ for drying until it is completely cured and set.
[0028] The present invention also provides a nano-corrosion-resistant conductive coating grounding material, comprising a flat steel, wherein the flat steel is coated with a nano-corrosion-resistant conductive coating; prepared by the process described above.
[0029] In summary, the present invention has the following beneficial effects:
[0030] Environmentally friendly epoxy resin serves as the main film-forming agent, providing the coating with basic adhesion, mechanical strength, and corrosion protection. Blending silicone rubber with the epoxy system enhances the coating's weather resistance, crack resistance, and low-temperature flexibility. Nano-conductive carbon black, conductive powder, and zinc powder work synergistically to form a conductive network. Nano-conductive carbon black provides microscopic conductive pathways, conductive powder improves overall conductivity, and zinc powder provides cathodic protection in corrosive environments. Anti-deposition agents prevent conductive fillers from settling and stratifying during storage and application; accelerators accelerate epoxy curing and cross-linking; leveling agents improve coating surface smoothness; and polymeric wetting agents enhance the uniformity of filler dispersion in the resin. Diluents adjust the coating's application viscosity, and curing agents enable the epoxy system to cross-link and form a film. The synergistic effect of these components within the aforementioned proportions achieves a balance between conductivity and corrosion resistance, reduces coating resistivity, and provides excellent resistance to media penetration.
[0031] The coating process utilizes a soft silicone feeder on a laminating machine to coat the surface of flat steel. Two soft silicone rollers are stacked one on top of the other, with the flat steel passing between them. The rollers have grooves at their facets that are adapted to the size of the flat steel. The two rollers, when stacked together, form a gap cavity for coating, ensuring complete coverage of the flat steel and guaranteeing that its outer perimeter is fully coated. Furthermore, this coating process completely replaces traditional spraying techniques, eliminating paint splatter and dust emissions, significantly improving paint utilization, and greatly reducing environmental pollution during the coating process.
[0032] By employing a double-coating process, combined with a surface-drying process that involves drying the first layer, the coating is not fully cured inside the first layer and reaches a semi-cured state before the second layer is applied. This ensures molecular-level intersolubility and bonding between the two layers while preventing the coatings from mixing and causing thickness control issues. Low-temperature drying avoids blistering and substrate deformation caused by high temperatures, making it suitable for continuous production.
[0033] Between drying and curing, the coating is oriented using an electric field. In the first electric field orientation treatment, a DC electric field of 600~1200V / cm is continuously applied. The electric field drives the randomly distributed nano-conductive carbon black and conductive powder in the first coating layer to undergo polarization rotation, eventually aligning in an orderly manner perpendicular to the flat steel surface. The filler portion adheres tightly to the polished flat steel substrate surface, forming point-to-point metal contact, completely eliminating the interfacial contact resistance caused by the resin interface layer in traditional processes, resulting in a significant reduction in interfacial contact resistance. The vertically arranged conductive filler forms a continuous conductive framework within the first coating layer, providing a stable conductive channel for the entire coating, and significantly improving conductivity compared to processes without an electric field.
[0034] The second electric field orientation treatment mainly acts on the outer second coating layer, continuously applying a DC electric field of 1200~2000V / cm throughout the drying process. Since the first coating layer has reached a surface-dry state, the strong interfacial constraint on the substrate side disappears, and the electric field force drives the negatively charged conductive filler to migrate and accumulate to the outer surface of the coating, forming a highly conductive region on the outer surface. The concentration of conductive filler on the surface layer increases, the in-plane resistance decreases, and the current can be rapidly diffused and discharged on the coating surface.
[0035] Furthermore, under the influence of an electric field, some of the conductive filler at the bottom of the second coating layer can embed into the microscopic depressions on the surface of the first coating layer after it has dried and into the semi-cured viscous layer, forming a filler interlocking structure across the two layers. This not only improves the interlayer bonding force but also creates a continuous conductive path between the two coating layers, eliminating the inherent high interlayer resistance problem in the two-pass process.
[0036] During the second coating process, the semi-cured resin on the surface of the dry layer and the second layer of fresh coating can undergo molecular chain diffusion and entanglement, forming a continuous transition layer after curing rather than a clear separation interface. The interlayer bonding force is improved compared to coating after full drying. At the same time, the dry layer has sufficient strength and will not be dispersed or swollen by the second layer of coating. Moreover, the thickness of the two coatings is independently controllable, allowing for precise control of the total thickness. Furthermore, the semi-cured surface of the dry layer is compressible. During the coating process, pressure is applied to the semi-cured surface, allowing the second layer of fresh coating to be partially squeezed into the first layer. When the filler migrates driven by the second electric field, the filler can be pressed into the adhesive layer on the surface of the dry layer to form filler interlocking nails, achieving both mechanical interlocking and forming a cross-layer conductive path. Simultaneously, the dry layer prevents the second layer of filler from diffusing into the first layer, forming an integrated conductive framework.
[0037] Furthermore, this invention employs differentiated electric field strength configurations for the two electric fields. The first electric field uses a lower electric field strength of 600~1200V / cm, targeting the first wet coating layer that directly contacts the metal substrate. Under the strong interfacial constraint of the metal substrate, it primarily drives the conductive filler to rotate and orient itself, anchoring the filler ends to the surface of the flat steel substrate, thus constructing the underlying longitudinal conductive framework. After the first coating layer is surface-dried and semi-cured, the underlying conductive framework is locked by the semi-cured resin. The second electric field uses a higher electric field strength of 1200~2000V / cm. The second coating layer contacts the surface-dried first resin coating layer. The strong interfacial constraint from the metal substrate is significantly reduced. In addition to achieving vertical orientation of the filler, the higher electric field strength can drive the conductive filler to undergo long-distance electrophoretic migration. On the one hand, this causes the conductive filler to accumulate on the outer surface of the coating, forming a highly conductive surface area. On the other hand, some filler is pressed into the microscopic depressions on the surface of the first coating layer, forming an interlayer interlocking structure and eliminating interlayer interfacial resistance. By configuring different electric field strengths, it is possible to simultaneously ensure substrate interface adhesion, bottom layer longitudinal conductivity, surface layer conductive leakage, and interlayer resistance-free connection, achieving unexpected synergistic technical effects. Attached Figure Description
[0038] Figure 1 This is a flowchart of Example 1. Detailed Implementation
[0039] Example 1:
[0040] This embodiment discloses an environmentally friendly preparation process for a nano-corrosion-resistant conductive coating grounding material, which is prepared using a dual-layer soft silicone composite process. The specific steps are as follows:
[0041] S1: Select 50mm×5mm hot-dip galvanized flat steel as the base material. The hot-dip galvanized flat steel is leveled and straightened. Surface burrs, zinc nodules and oxide layers are removed by polishing and grinding to obtain a flat and clean base surface.
[0042] S2: Weigh the raw materials for the nano-corrosion-resistant and conductive coating by mass percentage, and disperse them in a disperser to obtain the nano-corrosion-resistant and conductive coating; during the dispersion process, the cooling device on the outer periphery of the disperser cylinder runs continuously to maintain a stable dispersion temperature.
[0043] In this embodiment, the nano-corrosion-resistant conductive coating is made from the following raw materials in the indicated weight percentages: 35% environmentally friendly epoxy resin, 6% silicone rubber, 8% nano-conductive carbon black, 7% conductive powder, 2% zinc powder, 1% anti-deposition agent, 3.5% accelerator, 2% leveling agent, 0.5% polymeric wetting agent, 27% diluent, and 8% curing agent. The environmentally friendly epoxy resin is composed of 5% organosilicon resin, 56% glycidyl amine epoxy resin, and 39% bisphenol A epoxy resin blended in the indicated weight ratio.
[0044] The specific mixing steps for the raw materials are as follows:
[0045] S21: Add environmentally friendly epoxy resin and silicone rubber to a disperser in proportion and disperse at 500 r / min for 35 min; then add diluent and anti-deposition material in proportion and disperse at 650 r / min for 65 min to form the base resin.
[0046] S22: Add nano-conductive carbon black, conductive powder and zinc powder to a ball mill and grind them until the particle size is less than 1 micrometer to form conductive powder intermediate material;
[0047] S23: Add the ground conductive powder intermediate material to the dispersed base resin and disperse at 1350 r / min for 210 min;
[0048] S24: Add accelerator, leveling agent and polymer wetting agent in proportion, disperse at 1350r / min for 70min to obtain semi-finished coating;
[0049] S25: Before use, add curing agent to the semi-finished coating in proportion, disperse at 1350r / min for 55min to obtain nano anti-corrosion and conductive coating for construction.
[0050] To reduce solvent evaporation, a cooling device is installed around the outer periphery of the disperser cylinder. During the dispersion process, the temperature is maintained by cooling through the cooling device to prevent excessive evaporation caused by excessive temperature, thereby reducing environmental pollution.
[0051] S3: Apply nano-anti-corrosion and conductive coating to the surface of flat steel using the soft silicone feeder of the composite machine to form the first layer of coating, and control the thickness of the first layer of coating to be 70~80μm.
[0052] S4: Send the flat steel coated with the first layer of paint into the dryer and dry it at a temperature of about 55°C for about 120 seconds to make the first layer of paint reach the surface dry state.
[0053] S5: The surface of the flat steel in the surface-dry state is coated with a nano-anti-corrosion and conductive coating through the soft silicone feeder of the composite machine to form a second coating layer. The thickness of the second coating layer is controlled to be 70~80μm.
[0054] S6: The flat steel coated with the second layer of coating is sent into the dryer for drying. The first and second layers of coating together form a cured nano-anti-corrosion and conductive coating on the outside of the flat steel, with a total thickness of about 150μm.
[0055] The performance of the sample in this embodiment was tested, and the results are as follows:
[0056] Coating adhesion: Tested according to GB / T1720-2020, it reaches level 1;
[0057] DC resistivity: Tested according to GB / T3048.2-2007, the DC resistivity is 0.10 Ω·mm. 2 / m, less than the standard requirement of 0.11Ω·mm 2 / m;
[0058] Corrosion resistance: According to GB / T9274-1988 (2004), the coating was tested for 10% HCl, 10% NaOH, 10% NaCl, 10% H2SO4 and 10% Na2S. The coating showed no blistering, peeling, cracking and discoloration.
[0059] Anti-aging performance: According to GB / T14522-2008, after 1000 hours of artificial climate aging test, the coating showed no blistering, peeling, cracking, or rust.
[0060] Example 2:
[0061] This embodiment discloses an environmentally friendly preparation process for a nano-corrosion-resistant conductive coating grounding material. Based on Example 1, a dual-channel differentiated electric field orientation treatment is added. The specific steps are as follows:
[0062] S1: Select 50mm×5mm hot-dip galvanized flat steel as the base material, and the surface pretreatment is the same as in Example 1.
[0063] S2: The coating formulation and preparation steps are the same as in Example 1.
[0064] S3: Apply nano-anti-corrosion and conductive coating to the surface of flat steel using the soft silicone feeder of the composite machine to form the first layer of coating, and control the thickness of the first layer of coating to be 70~80μm.
[0065] From step S3 to step S4, the entire drying process involves the first electric field orientation treatment. The DC electric field consists of a symmetrically arranged mesh positive electrode and a flat steel substrate as the negative electrode. The surface of the mesh positive electrode is covered with a high-temperature resistant layer, and the mesh positive electrode and the wet coating surface maintain a non-contact gap of 0.8 mm. The DC electric field strength of the first electric field orientation treatment is 900 V / cm. Under the continuous action of the DC electric field, the conductive filler in the first layer of coating is oriented in a direction perpendicular to the surface of the flat steel. The ends of the filler adhere to the surface of the flat steel substrate, forming an interface conductive anchoring structure and a bottom longitudinal conductive skeleton.
[0066] S4: The flat steel coated with the first layer of paint is sent into the dryer and dried at a temperature of about 55°C for 120 seconds to make the first layer of paint reach the surface dry state. The electric field continues to be applied until the coating is surface dry and set.
[0067] S5: The surface of the flat steel in the surface-dry state is coated with a nano-anti-corrosion and conductive coating through the soft silicone feeder of the composite machine to form a second coating layer. The thickness of the second coating layer is controlled to be 70~80μm.
[0068] From step S5 to step S6, the entire drying process is subjected to a second electric field orientation treatment. The electrode structure is consistent with the first electric field. The DC electric field strength of the second electric field orientation treatment is 1600V / cm. The conductive filler in the second coating migrates and accumulates to the outer surface, forming a highly conductive surface area. Some of the conductive filler is embedded in the microscopic depressions on the surface of the first coating, forming an interlayer interlocking structure between the first and second coatings.
[0069] S6: The flat steel coated with the second layer of coating is sent into the dryer and dried at a temperature of about 55°C for 120 seconds. The electric field continues to be applied until the coating is completely cured, with a total thickness of about 150μm.
[0070] To improve the adhesion of the second coating layer, a rough surface pretreatment is performed on the surface of the first coating layer before applying the second coating layer in step S5. This pretreatment creates a relatively rough surface for the first coating layer. Specifically, this can be achieved by brushing the surface of the first coating layer with a wire brush or by rolling it with a roller having a rough, uneven surface. This roughening pretreatment disrupts the smoothness of the first coating layer's surface, increasing the roughness of the contact surface between the first and second coating layers. Part of the second coating layer material can then be embedded into the rough surface, forming an interlocking structure, thus improving the bonding strength between the two layers. Furthermore, by roughening the surface structure of the first coating layer, the conductive material within it is directly exposed, facilitating contact with the conductive material in the second coating layer, thereby increasing the conductivity of both coating layers.
[0071] In traditional coating processes, a continuous resin interface layer inevitably exists between the substrate and the coating, which is a major component of the grounding resistance. In this embodiment, the electric field drives the filler to form point-to-point direct contact with the metal substrate, reducing the resin interface barrier and lowering the interface contact resistance. Vertically arranged conductive fillers form a continuous longitudinal conductive path within the first coating layer. Compared to randomly distributed fillers, this allows for the formation of a stable conductive network with a lower filler content, avoiding the degradation of coating density and corrosion resistance caused by high filler content.
[0072] Furthermore, by applying two electric fields, during the second electric field treatment, the first coating has reached a surface-dry state (semi-cured), with a significant increase in resin viscosity, resulting in a significantly enhanced constraint on the internal filler. The second coating is in a fresh, wet state, and the filler still possesses good fluidity. Applying a higher-intensity vertical DC electric field causes the negatively charged conductive filler in the second coating to experience an electric field force towards the positive electrode (outer surface of the coating), overcoming the resistance of resin viscosity and migrating to the outer surface, ultimately forming a high-concentration conductive filler enrichment zone on the coating surface. Some conductive fillers near the interlayer interface are driven by the electric field force to embed downwards into the surface micro-recesses and semi-cured viscous layer of the surface after the first coating has dried, forming a conductive nail structure spanning the two layers. Combined with the rough structure, this enables the construction of a smooth conductive structure between the two coating layers, improving the conductivity.
[0073] The samples in this embodiment were subjected to comparative testing under the same conditions, and the results are as follows:
[0074] Coating adhesion: Tested according to GB / T1720-2020, it reaches level 1, which is equivalent to the basic solution;
[0075] DC resistivity: Tested according to GB / T3048.2-2007, the DC resistivity is approximately 0.090 Ω·mm² / m, which is lower than that of Example 1;
[0076] Corrosion resistance: According to GB / T9274-1988 (2004), after 1000h immersion in the medium, the coating showed no blistering, peeling, cracking, or discoloration, which is comparable to Example 1;
[0077] Anti-aging performance: According to GB / T14522-2008, after 1100 hours of artificial climate aging test, the coating showed no blistering, peeling, cracking, or rusting, which is slightly better than Example 1.
[0078] Example 3:
[0079] This embodiment discloses an environmentally friendly preparation process for a nano-corrosion-resistant conductive coating grounding material. Based on Example 2, a stepped temperature curing process is adopted to further optimize the filler migration and orientation effects. The specific steps are as follows:
[0080] S1: Select 50mm×5mm hot-dip galvanized flat steel as the base material, and the surface pretreatment is the same as in Example 1.
[0081] S2: The coating formulation and preparation steps are the same as in Example 1.
[0082] S3: The first coating is the same as in Example 1; from S3 to S4 drying, the first electric field orientation treatment is performed, with an electric field strength of 900V / cm, and the electrode structure is the same as in Example 2.
[0083] S4: First drying stage, constant temperature drying at 55℃ for 120 seconds until surface dry, with continuous electric field application.
[0084] S5: The second coating is the same as in Example 1; from S5 to S6 drying, a second electric field orientation treatment is performed with an electric field strength of 1600V / cm, and the electrode structure is the same as in Example 2.
[0085] S6: Employs a stepped temperature curing process: First, maintain a temperature of approximately 42℃ for 30 seconds. During this low-temperature phase, the resin viscosity is relatively low. The second electric field drives the conductive filler to migrate and accumulate fully to the surface of the second coating layer, forming a gradient distribution structure with a higher concentration of conductive filler on the surface and a higher concentration of resin matrix in the inner layer. Then, raise the temperature to approximately 58℃ and dry for 90 seconds. The electric field continues to maintain the vertically oriented arrangement of the filler until the coating is completely cured and set. The total drying time for a single pass is approximately 120 seconds. The total thickness of the finished product is approximately 150μm.
[0086] By employing electric field treatment and stepped heating scraping process, the surface adhesion of the first layer is preserved to allow the second layer of filler to embed and form an interlock, while also having sufficient bulk strength to prevent the second layer of filler from diffusing into the bottom layer, ensuring the concentration gradient enriched on the surface and avoiding the loss of thickness control caused by the mixing of the two coating layers.
[0087] By combining a stepped temperature curing process, the resin viscosity is low in the initial low-temperature stage, the filler migration resistance is small, and the electric field can fully drive the filler to complete the directional arrangement and migration enrichment. Then, the temperature is increased to the rapid curing stage, which locks the ordered structure of the filler instantly, preventing the filler from returning to a random state due to Brownian motion during the curing process, thus maximizing the effect of electric field control.
[0088] The samples in this embodiment were subjected to comparative testing under the same conditions, and the results are as follows:
[0089] Coating adhesion: Tested according to GB / T1720-2020, it reaches level 1;
[0090] DC resistivity: Tested according to GB / T3048.2-2007, the DC resistivity is approximately 0.085 Ω·mm² / m, which is lower than that of Example 1;
[0091] Corrosion resistance: According to GB / T9274-1988 (2004), after 1000h immersion in the medium, the coating showed no blistering, peeling, cracking, or discoloration, which is slightly better than Example 1;
[0092] Anti-aging performance: According to GB / T14522-2008, after 1200 hours of artificial climate aging test, the coating showed no blistering, peeling, cracking, or rusting; slightly better than Example 1.
[0093] Example 4:
[0094] This embodiment discloses an environmentally friendly preparation process for a nano-corrosion-resistant conductive coating grounding material. The specific steps are as follows:
[0095] S1: Select 50mm×5mm hot-dip galvanized flat steel as the base material, and the surface pretreatment is completely consistent with that in Example 1.
[0096] S2: The nano-corrosion-resistant conductive coating is made from the following raw materials in the indicated weight percentages: 38% environmentally friendly epoxy resin, 7% silicone rubber, 7% nano-conductive carbon black, 6% conductive powder, 1.5% zinc powder, 0.8% anti-deposition agent, 3% accelerator, 1.5% leveling agent, 0.4% polymeric wetting agent, 28% diluent (xylene), and 6.8% curing agent. The composition of the environmentally friendly epoxy resin is the same as in Example 1.
[0097] The raw material mixing steps are the same as in Example 1, and the cooling device is turned on during the dispersion process.
[0098] S3: First coating, thickness 70~80μm; From S3 to S4 drying process, the first electric field orientation treatment is carried out, with an electric field strength of 800V / cm.
[0099] S4: Dry at 55℃ for 120 seconds until surface dry, with the electric field continuously applied.
[0100] S5: Second coating, thickness 70~80μm; From S5 to S6 drying process, a second electric field orientation treatment is performed, with an electric field strength of 1500V / cm.
[0101] S6: Dry at 55℃ for 120 seconds until fully cured, with the electric field continuously applied; the total thickness of the finished product is approximately 160μm.
[0102] The samples in this embodiment were subjected to comparative testing under the same conditions, and the results are as follows:
[0103] Coating adhesion: Tested according to GB / T1720-2020, it reaches level 1;
[0104] DC resistivity: Tested according to GB / T3048.2-2007, the DC resistivity is approximately 0.093 Ω·mm² / m, which meets the standard requirement of ≤0.11 Ω·mm² / m;
[0105] Corrosion resistance: According to GB / T9274-1988 (2004), after 1000 hours of immersion in the medium, the coating showed no blistering, peeling, cracking, or discoloration.
[0106] Anti-aging performance: According to GB / T14522-2008, after 1000 hours of artificial climate aging test, the coating showed no blistering, peeling, cracking, or rust.
[0107] Comparative Example 1:
[0108] This comparative example uses the exact same coating formulation as Example 1, and is prepared using a traditional air spraying process. The specific steps are as follows:
[0109] S1: Select 50mm×5mm hot-dip galvanized flat steel as the base material, and the surface grinding treatment is the same as in Example 1.
[0110] S2: The coating preparation is completely consistent with Example 1.
[0111] S3: The first coat is applied using an air spraying process at a pressure of 0.4 MPa, with the spray gun 20 cm away from the substrate. The thickness of the first coat is controlled at 70-80 μm. After leveling at room temperature for 10 minutes, it is dried at 60°C for 30 minutes. The spraying process generates a large amount of paint mist and dust.
[0112] S4: Perform the second air spray coating, controlling the thickness of the second coating to 70~80μm; after leveling at room temperature for 10 minutes, dry at 60℃ for 30 minutes, with a total thickness of approximately 150μm.
[0113] The performance of this comparative sample was tested, and the results are as follows:
[0114] Coating adhesion: Tested according to GB / T1720-2020, it is grade 2, indicating a decrease in the interfacial bonding strength with the substrate;
[0115] DC resistivity: Tested according to GB / T3048.2-2007, the DC resistivity is approximately 0.13 Ω·mm² / m, which is higher than that of the basic composite process;
[0116] Corrosion resistance: According to GB / T9274-1988 (2004), after immersion in 10% H2SO4 for 720 hours, the coating showed blistering and edge peeling.
[0117] Anti-aging performance: According to GB / T14522-2008, after 800 hours of artificial climate aging test, the coating showed minor cracks.
[0118] Comparative Example 2:
[0119] The only difference between this comparative example and Example 2 is that a 1600V / cm DC electric field is applied only in the second drying process, while no electric field is applied in the first drying process. The coating formulation and the remaining process steps are completely consistent with Example 2.
[0120] The comparative sample was tested under the same conditions, and the results are as follows:
[0121] Coating adhesion: Tested according to GB / T1720-2020, it is grade 2, indicating a decrease in the interfacial bonding strength with the substrate;
[0122] DC resistivity: Tested according to GB / T3048.2-2007, the DC resistivity is approximately 0.10 Ω·mm² / m, and the overall conductivity is lower than that of the dual-channel electric field scheme in Example 2;
[0123] Corrosion resistance: No obvious abnormalities were observed after 1000 hours of immersion in the medium;
[0124] Anti-aging performance: No obvious abnormalities were observed after 1000 hours of artificial climate aging test.
[0125] Comparative Example 3:
[0126] The only difference between this comparative example and Example 2 is that the electric field strength in both drying processes is set to 1200V / cm, without using differentiated strength configurations. The coating formulation and other process steps are completely consistent with Example 2.
[0127] The comparative sample was tested under the same conditions, and the results are as follows:
[0128] Coating adhesion: Tested according to GB / T1720-2020, it is level 3, indicating a decrease in the bonding strength between the substrate and the coating interface, and there is a risk of micro-defects at the interface of the first coating layer.
[0129] DC resistivity: Tested according to GB / T3048.2-2007, the DC resistivity is about 0.12Ω·mm² / m. The surface conductivity enrichment effect is insufficient, and the overall performance is weaker than the differentiated intensity scheme of Example 2.
[0130] The above description is merely a preferred embodiment of the present invention. The scope of protection of the present invention is not limited to the above embodiments. All technical solutions falling within the scope of the present invention's concept are within the scope of protection of the present invention. It should be noted that for those skilled in the art, any improvements and modifications made without departing from the principles of the present invention should also be considered within the scope of protection of the present invention.
Claims
1. An environmentally friendly preparation process for a nano-corrosion-resistant conductive coating grounding material, characterized in that, Includes the following steps: S1: The flat steel is leveled and straightened, and the surface of the flat steel is ground. S2: Mix the raw materials of the nano-corrosion-resistant conductive coating according to the mass percentage, and disperse them in a disperser to obtain the nano-corrosion-resistant conductive coating. S3: The flat steel surface is coated with a nano-anti-corrosion and conductive coating through the soft silicone feeder of the composite machine to form the first layer of coating; S4: The flat steel coated with the first layer of paint is sent into the dryer and dried at a temperature of 50~60℃ for 110s~120s to make the first layer of paint reach the surface dry state. S5: The surface of the flat steel in the surface-dry state is coated with a nano-anti-corrosion and conductive coating through the soft silicone feeder of the composite machine to form a second coating layer. S6: The flat steel coated with the second layer of coating is sent into the dryer to dry. The first and second layers of coating together form a cured nano-anti-corrosion and conductive coating on the outside of the flat steel.
2. The environmentally friendly preparation process of the nano-corrosion-resistant conductive coating grounding material according to claim 1, characterized in that, In step S3, the thickness of the first coating layer is 70~80μm; In step S4, the thickness of the second coating layer is 70~80μm; in step S6, the thickness of the cured nano-anti-corrosion conductive coating layer is 150~160μm.
3. The environmentally friendly preparation process of the nano-corrosion-resistant conductive coating grounding material according to claim 1, characterized in that, The nano-corrosion-resistant conductive coating is made from the following raw materials in the following mass percentages: 30-40% environmentally friendly epoxy resin, 4-8% silicone rubber, 6-10% nano-conductive carbon black, 5-9% conductive powder, 1-3% zinc powder, 0.5-1.5% anti-deposition agent, 2.5-4.5% accelerator, 1-3% leveling agent, 0.3-0.8% polymer wetting agent, 22-32% diluent, and 6-10% curing agent, with the sum of the mass percentages of each component being 100%.
4. The environmentally friendly preparation process of the nano-corrosion-resistant conductive coating grounding material according to claim 3, characterized in that, The nano-corrosion-resistant conductive coating is made from the following raw materials in the indicated weight percentages: 35% environmentally friendly epoxy resin, 6% silicone rubber, 8% nano-conductive carbon black, 7% conductive powder, 2% zinc powder, 1% anti-deposition agent, 3.5% accelerator, 2% leveling agent, 0.5% polymer wetting agent, 27% diluent, and 8% curing agent.
5. The environmentally friendly preparation process of the nano-corrosion-resistant conductive coating grounding material according to claim 3, characterized in that, The environmentally friendly epoxy resin is composed of 5% organosilicon resin, 56% glycidyl amine epoxy resin, and 39% bisphenol A epoxy resin in a mass ratio; the diluent is one or a combination of two of environmentally friendly epoxy reactive diluents and xylene.
6. The environmentally friendly preparation process of the nano-corrosion-resistant conductive coating grounding material according to claim 3, characterized in that, In step S2, a cooling device is installed on the outer periphery of the disperser cylinder. During the dispersion process, the temperature is maintained by cooling through this device. The mixing of the raw materials for the nano-corrosion-resistant conductive coating includes the following steps: S21: Environmentally friendly epoxy resin and silicone rubber are added to a disperser in a certain proportion for dispersion; then diluent and anti-deposition material are added in a certain proportion for dispersion to form a base resin; S22: Add nano-conductive carbon black, conductive powder, and zinc powder to a ball mill in proportion and grind them until the particle size is less than 1 micrometer to form conductive powder intermediate material; S23: Add the ground conductive powder intermediate material to the well dispersed base resin in proportion and disperse it. S24: Add accelerator, leveling agent and polymer wetting agent in proportion and disperse to obtain semi-finished coating; S25: When using, add curing agent to the semi-finished coating in proportion, and then disperse it in a disperser to obtain nano-anti-corrosion and conductive coating.
7. The environmentally friendly preparation process of the nano-corrosion-resistant conductive coating grounding material according to claim 1, characterized in that, The entire drying process from step S3 to step S4 is carried out through the first electric field orientation treatment; The conductive filler in the first layer of coating is oriented in a direction perpendicular to the surface of the flat steel under the continuous action of a DC electric field. The entire drying process from step S5 to step S6 is carried out through a second electric field orientation treatment; The conductive filler in the second coating migrates and accumulates on the outer surface, forming a highly conductive area on the surface. Some of the conductive filler is embedded in the microscopic depressions on the surface of the first coating, forming an interlayer interlocking structure between the first and second coatings.
8. The environmentally friendly preparation process of the nano-corrosion-resistant conductive coating grounding material according to claim 7, characterized in that, Both the first and second electric field orientation treatments apply an electric field perpendicular to the surface of the flat steel. The flat steel serves as the negative electrode, and a mesh of positive electrodes is symmetrically arranged on both the upper and lower sides of the flat steel, with a non-contact gap of 0.5~1mm between the mesh of positive electrodes and the surface of the flat steel. The DC electric field strength of the first electric field orientation treatment is 600~1200V / cm, and the DC electric field strength of the second electric field orientation treatment is 1200~2000V / cm.
9. The environmentally friendly preparation process of the nano-corrosion-resistant conductive coating grounding material according to claim 7, characterized in that, In step S6, a stepped temperature curing process is adopted. First, the temperature is maintained at 40~45℃ for 25~35s, and then the temperature is increased to 55~60℃ for drying until it is completely cured and set.
10. A nano-corrosion-resistant conductive coating grounding material, characterized in that, The product includes flat steel coated with a nano-corrosion-resistant and conductive coating; and is prepared by the process described in any one of claims 1-9.