A method, system and application of EVA separation in photovoltaic modules based on salt solution induced separation
By using a method of soaking in a soluble inorganic salt solution and cutting with a medium-temperature hot knife in photovoltaic modules, the problem of EVA film being difficult to peel off at low temperatures has been solved, achieving efficient and non-destructive EVA separation, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202611223223.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-13
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot efficiently and non-destructively peel off the EVA film from photovoltaic modules under low-temperature conditions, and they also pose risks of high energy consumption, environmental damage, and material damage, making it difficult to meet the demand for high-value recycling of retired photovoltaic modules.
Photovoltaic modules are immersed in a soluble inorganic salt solution at medium and low temperatures. The adhesion between EVA and glass is reduced by ion penetration and interface polarity adjustment. Efficient EVA peeling is achieved by combining medium-temperature thermal softening and hot knife cutting.
It significantly reduces the interfacial adhesion between EVA and glass under medium and low temperature conditions, reduces energy consumption, improves material integrity, is suitable for continuous industrial production, reduces carbon emissions, and enhances the reuse value of recycled materials.
Smart Images

Figure CN123102706A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the fields of renewable energy equipment recycling, solid waste resource utilization and material separation engineering technology, specifically to a method, system and application of EVA separation in photovoltaic modules based on salt solution induced separation. Background Technology
[0002] With the continued rapid growth of global photovoltaic (PV) power generation, a large number of crystalline silicon PV modules installed between 2005 and 2012 are gradually entering their retirement period. As the number of retired PV modules increases, a vast "urban mine" is gradually forming, primarily composed of renewable resources such as glass, aluminum, silicon wafers, silver, and copper. Among these, silicon wafers and silver paste are high-value resources and are currently the two categories with the highest recycling value in the industry. PV modules have a high-strength, multi-layered composite structure. How to safely, efficiently, and environmentally remove the ethylene-vinyl acetate copolymer (EVA) encapsulant film is one of the most critical and challenging technical bottlenecks in the current PV recycling industry chain.
[0003] EVA is copolymerized from ethylene and vinyl acetate monomers. Through lamination at 150-160℃ during the photovoltaic module encapsulation process, it undergoes cross-linking, giving it strong adhesion, good transparency, heat resistance, oxidation resistance, UV resistance, and anti-aging properties. These advantages ensure the reliability of the module for over 25 years, but also make it difficult to achieve structural destruction at low temperatures during recycling and dismantling. EVA forms a strong interface with glass and silicon wafers through polar groups (-COO-), hydrogen bonds, and van der Waals forces, resulting in adhesion forces typically as high as 1500-2000 N. Existing technologies typically employ the following methods for peeling: 1) traditional high-temperature pyrolysis; 2) organic solvent methods; 3) pure thermal softening peeling; 4) hydrothermal methods and acid-base methods. None of these methods can reduce the bonding force between EVA and glass / silicon wafers to a peelable region under mild conditions, and all have various drawbacks. For example, (1) Traditional high-temperature pyrolysis method (500-600℃): The most widely used industrial method at present is pyrolysis, which decomposes EVA into small molecules at continuous high temperature to achieve the purpose of removal. The main defects of this method include: 1) High energy consumption and cost: High temperature operation leads to extremely high energy consumption, and the corresponding recycling cost accounts for about 40%-60% of the total recycling cost, which seriously restricts the economic efficiency of the process; 2) Low material reuse value: High temperature easily leads to devitrification of glass cover and a significant increase in microcracks in silicon wafers, which greatly reduces the purity and reuse value of recycled materials; 3) High environmental pressure: Organic fumes will be released during the pyrolysis process, which requires an expensive tail gas treatment system, increasing the complexity of the process and environmental costs; 4) Limited large-scale application: The overall process route does not conform to the green and low-carbon development concept and is difficult to meet the high-efficiency and environmentally friendly recycling needs of large-scale retired photovoltaic modules. (2) Organic solvent method (toluene, petroleum ether, etc.): The organic solvent method is another common EVA separation technology. It uses organic solvents such as toluene and petroleum ether to swell or partially dissolve EVA, destroy its cross-linked structure, and thus achieve the separation of EVA from glass, silicon wafers and other components. The main defects of this method include: 1) Safety and environmental risks: Most of the organic solvents used are flammable, toxic and volatile, posing serious safety hazards and not meeting environmental protection regulations; 2) Poor economic efficiency: The solvent recycling cost is high and the consumption is large, resulting in high recycling costs; 3) Low efficiency: The swelling or dissolution process takes a very long time, with a process cycle of 8-72 hours, resulting in extremely low production efficiency; 4) Limited large-scale application: It is difficult to meet the needs of efficient and continuous processing of large-scale retired photovoltaic modules. (3) Pure thermal softening and peeling method (120-150℃): In recent years, researchers have proposed that when the encapsulation material EVA is in the temperature range of 80-120℃, obvious viscous flow characteristics will appear. Based on this, the pure thermal softening and peeling method has been developed. This method involves heating retired photovoltaic modules to 120-150℃ to thermally soften the EVA, and then using mechanical means to separate the EVA from other modules.The main drawbacks of this method include: 1) Difficulty in interface separation: Thermal softening alone cannot significantly reduce the bonding energy between EVA and glass, silicon wafers, etc. The separation process still requires a large mechanical force, which can easily cause silicon wafers to break; 2) Poor aging applicability: It is not suitable for aged EVA after long-term outdoor service. The increased cross-linking caused by aging will significantly weaken the thermal softening effect; 3) Limited purity of recycled products: After separation, the EVA adhesive layer remaining on the surface of silicon wafers and glass is serious and difficult to completely remove, which has an adverse effect on subsequent processes such as silver electrode recycling. (4) Hydrothermal method and acid-base method: The hydrothermal method and acid-base method destroy the polar groups in the EVA molecular chain under high temperature and high pressure or strong acid and base environment, thereby degrading its structure and realizing the separation of EVA from other components. The main drawbacks of this method include: 1) High corrosivity: The process medium is highly corrosive, which places stringent requirements on the equipment materials and can easily lead to equipment damage and safety hazards; 2) Difficulty in large-scale operation: The reaction conditions are harsh and the operation process is complex, making it unsuitable for large-scale, continuous recycling of decommissioned components; 3) High equipment cost: The requirements for equipment materials and anti-corrosion design are high, resulting in high initial investment and maintenance costs; 4) Risk of material damage: The highly corrosive environment can easily cause irreversible damage to the silicon wafer substrate and silver wires, reducing the reuse value of the recycled materials.
[0004] National regulations require that the recycling of decommissioned photovoltaic modules meet core requirements such as high-value recycling, low energy consumption, environmental friendliness, and no damage to the structure of raw materials. However, existing EVA separation technologies cannot simultaneously meet all of these requirements, as shown in Table 1 below: Table 1
[0005] (Note: √ indicates that the requirements are met; Δ indicates that the requirements are partially met or that there are obvious limitations; × indicates that the requirements are not met) It is evident that existing technologies have significant shortcomings in terms of low-temperature non-toxicity, low energy consumption, material integrity, and large-scale application, making it difficult to simultaneously meet national policy guidance and actual industrial needs. Therefore, achieving efficient and non-destructive stripping of EVA in the medium- and low-temperature range requires a novel interface control mechanism to overcome existing technological bottlenecks and develop a new recycling technology route that combines environmental friendliness, economic efficiency, and high-value potential. Summary of the Invention
[0006] This invention aims to at least solve one of the technical problems existing in the prior art. To this end, this invention proposes a method for separating EVA from photovoltaic modules based on salt solution induction, which can achieve efficient and non-destructive stripping of EVA within a low-temperature range.
[0007] The present invention also proposes a system for implementing the above method.
[0008] The present invention also proposes applications of the above-mentioned methods and systems.
[0009] According to one aspect of the present invention, a method for EVA separation in a photovoltaic module based on salt solution-induced separation is proposed, comprising the following steps: S1. Salt solution-induced interface weakening: The photovoltaic module is immersed in a solution containing soluble inorganic salts at 60~100℃; the soluble inorganic salts include cations and anions, the cations include at least one of alkali metal ions, alkaline earth metal ions or aluminum ions; the anions include chloride ions; S2. Medium-temperature heat softening and hot knife cutting: After immersion treatment, the temperature of the photovoltaic module is controlled at 80~100℃. Hot cutting can be used to separate the EVA layer from other parts of the photovoltaic module.
[0010] In the EVA separation method of this invention, the photovoltaic module is immersed in an immersion solution containing soluble inorganic salts under medium-low temperature conditions. The immersion treatment utilizes the directional penetration of ions in the solution to the bonding interface between the glass and EVA, thereby weakening the interfacial adhesion force (the adhesion force can be reduced from 1500~2000N to 300~500N). At the same time, microbubbles will be generated near the silver wires of the solar cells inside the photovoltaic module to promote debonding. The temperature of the photovoltaic module after immersion is then controlled within a specific medium temperature range, which causes the EVA film to change from a highly elastic state to a viscous flow state with extremely low interfacial bonding energy. Then, thermal cutting can quickly peel the EVA layer off from other parts. Thermal cutting does not require strong mechanical separation and has a protective effect on both the glass and the silicon wafer.
[0011] EVA, as a typical nonionic polymer, lacks strongly polar groups in its molecular structure and is theoretically not easily affected by inorganic salt solutions. However, this invention unexpectedly discovered through numerous experiments that although EVA is insoluble in water, the polar groups present at its interface (especially the aged interface formed by long-term outdoor service) are significantly weakened by the strong ionic environment created by inorganic salt solutions. At the same time, the ions ionized in the solution can specifically interfere with interfacial hydrogen bonds and uncrosslinked segments in the EVA molecule, thereby significantly reducing interfacial adhesion.
[0012] The core technology of this invention is not a simple combination of "immersion + hot knife cutting" processes in existing technologies, but rather achieves efficient and non-destructive peeling of EVA through the synergistic effect of "salt-induced interface weakening - medium-temperature thermal softening - hot knife cutting". The specific synergistic mechanism is as follows: 1) Salt-induced interface weakening: By using ion penetration and polarity adjustment of specific inorganic salt solutions, the interfacial bonding energy between EVA and glass is reduced, laying the foundation for subsequent peeling. 2) Medium-temperature thermal softening: The processing temperature is controlled in the medium-low temperature range, which causes EVA to swell slightly and its viscosity to decrease, further reducing the peeling resistance; 3) Hot knife cutting: With the help of a hot knife, the weakened EVA layer is quickly separated, avoiding material damage caused by applying high-intensity mechanical force.
[0013] The three processes described above work together and enhance each other, resulting in a significant improvement in peeling effect, efficiency, and material integrity.
[0014] The interface weakening effect of the present invention does not stem from the general effect of the "ionic strength" of inorganic salts, but rather from the special compatibility between the soluble salts of the specific composition of the present invention and the polar groups of the EVA interface, silver wires, etc.
[0015] According to some embodiments of the present invention, the cation includes Na. + K + Mg 2+ Ca 2+ Or Al 3+ At least one of them.
[0016] According to some embodiments of the present invention, the anion further includes at least one of sulfate ions or carbonate ions.
[0017] According to some embodiments of the present invention, the soluble inorganic salt contains at least two anions or at least two cations.
[0018] According to some embodiments of the present invention, the cation contains at least two of the following: alkali metal ions, alkaline earth metal ions, or aluminum ions.
[0019] According to some embodiments of the present invention, the chloride salt accounts for 50-100% of the mass of the soluble inorganic salt. The present invention employs a green auxiliary agent system (i.e., soluble inorganic salt solution) to improve solution permeability, effectively reducing process temperature and overall energy consumption; the added value of material recycled through this process is significantly increased. Carbon accounting analysis verifies that this process possesses excellent carbon emission reduction potential and low-carbon application value.
[0020] According to some embodiments of the present invention, the anion includes a mixture of chloride ions and sulfate ions; or, the cation includes a mixture of magnesium, calcium, aluminum ions and sodium ions.
[0021] According to some embodiments of the present invention, the magnesium-calcium-aluminum ions include Mg 2+ Ca 2+ Or Al 3+ At least one of them.
[0022] According to some embodiments of the present invention, the soluble inorganic salt includes at least one of sodium chloride, potassium chloride, sodium sulfate, or sodium bicarbonate.
[0023] According to some embodiments of the present invention, the soluble inorganic salt includes at least one selected from NaCl, KCl, MgCl2, CaCl2, and AlCl3.
[0024] According to some embodiments of the present invention, the soluble inorganic salt includes a mixture of sodium chloride and sodium sulfate, a mixture of potassium chloride and potassium sulfate, a mixture of sodium chloride and magnesium chloride, and a mixture of sodium chloride and calcium chloride.
[0025] According to some embodiments of the present invention, the soaking temperature is 70~90°C, such as 80°C.
[0026] According to some embodiments of the present invention, the total molar concentration of soluble inorganic salts in the soaking solution is 0.5~2 mol / L, such as 1 mol / L.
[0027] According to some embodiments of the present invention, the soaking treatment time is 1 to 4 hours. Pre-soaking for a predetermined period under medium to low temperature conditions effectively weakens the guide surface.
[0028] According to some embodiments of the present invention, the soaking treatment time is 1.5 to 3 hours, such as 2 hours.
[0029] According to some embodiments of the present invention, during the immersion treatment, the solid-liquid ratio of the photovoltaic module to the immersion solution is 1 kg: 4 L to 6 L.
[0030] According to some embodiments of the present invention, the soaking treatment is carried out under stirring conditions, wherein the stirring speed is 200-600 rpm.
[0031] According to some embodiments of the present invention, in step S2, the photovoltaic module after soaking is placed at 80~100℃ and kept at that temperature for 10~20 minutes before being thermally cut.
[0032] According to some embodiments of the present invention, the photovoltaic module is pre-crushed before being immersed, and the characteristic size of the pre-treated photovoltaic module is between 3cm and 10cm.
[0033] According to some embodiments of the present invention, the pre-crushing process includes at least one of impact crushing, rolling crushing, or shear crushing.
[0034] According to some embodiments of the present invention, the working parameters of the thermal cutting include at least one of the following parameters: 1) temperature of 150~180℃; 2) cutting speed of 3~6cm / s.
[0035] According to some embodiments of the present invention, the operating parameters of the thermal cutting also include a downward blade pressure of 20~50N.
[0036] According to some embodiments of the present invention, the blade material used in the thermal cutting is a nickel-chromium alloy or a silicon carbide coating.
[0037] According to some embodiments of the present invention, the apparatus used for thermal cutting includes a hot knife system. Thermal cutting is performed using a continuous hot knife system with a heating function.
[0038] According to some embodiments of the present invention, the hot knife system includes a hot knife assembly, a conveying assembly, and a control module. The control module is controlled and connected to the hot knife assembly and the conveying assembly respectively. The hot knife assembly includes a blade, a hot wire, and a heating plate disposed on the blade. The conveying assembly includes a drive motor and a hot roller that is driven and connected to the drive motor.
[0039] According to some embodiments of the present invention, the thermal cutting apparatus includes a thermal knife system or an infrared cutting apparatus.
[0040] According to some embodiments of the present invention, other parts of the photovoltaic module include silicon wafers and glass.
[0041] According to some embodiments of the present invention, the method further includes sieving and separating the photovoltaic module after the above separation treatment, and collecting the glass, solar cells and backsheet materials respectively. The materials are then recycled after deionization cleaning and drying.
[0042] The glass, solar cells, and backsheet materials obtained after separation by this invention have the following advantages: 1) The glass maintains good transparency and is free from fogging; 2) The silicon wafers are free from cracks and missing corners and can be used for silver extraction processes; 3) The EVA residue is extremely low and does not affect the metal leaching step, which is beneficial to subsequent green silver extraction, silicon wafer regeneration, glass recycling and other industrial chain operations.
[0043] According to another aspect of the present invention, a system for implementing the above-described separation method is also proposed, comprising, in sequence, an immersion module, a preheating module, and a hot knife cutting unit.
[0044] According to some embodiments of the present invention, the immersion module includes a heating component and an immersion tank, the heating component being connected to the immersion tank. The immersion tank is used to contain a soluble inorganic salt immersion solution and to immerse the photovoltaic module to be recycled.
[0045] According to some embodiments of the present invention, the heating assembly includes a circulating heating element. The circulating heating element maintains a constant solution temperature and promotes ion penetration into the material's internal interface.
[0046] According to some embodiments of the present invention, the soaking module further includes a stirring element for stirring the material in the soaking tank.
[0047] According to some embodiments of the present invention, the soaking tank is further provided with a closed-loop circulation filtration and purification device. The closed-loop circulation filtration and purification device is used to achieve the recycling and reuse of the salt solution.
[0048] According to some embodiments of the present invention, the preheating module includes a hot air device or an infrared preheating device. The preheating device is used to preheat the soaked material online with hot air or infrared light to soften its encapsulation.
[0049] According to some embodiments of the present invention, the hot knife cutting unit is disposed at the rear end of the preheating device and is used for continuous hot cutting and peeling along the material interface.
[0050] According to some embodiments of the present invention, the hot knife cutting unit includes an automatic guide rail and a cutting speed control closed-loop module. The entire separation production line equipped with the automatic guide rail and cutting speed control closed-loop module has a continuous processing capacity of 300~500 kg / h.
[0051] According to some embodiments of the present invention, the system further includes a crushing module. A crushing device may also be provided for mechanized pre-crushing of the photovoltaic modules to form material with fragments of a specific size.
[0052] According to some embodiments of the present invention, the system further includes a material sorting and collection unit. The material sorting and collection unit is configured to classify and recycle the cut and separated glass, EVA film, and silicon wafers.
[0053] According to another aspect of the present invention, the application of the above-mentioned method or system in photovoltaic module recycling is also proposed. The separation method of the present invention is green and low-energy-consumption, and can be used for the separation of EVA film layers in decommissioned crystalline silicon photovoltaic modules. Specifically, it can be applied to the photovoltaic module dismantling industry, the management of decommissioned photovoltaic power plants, the recycling of renewable materials and related equipment manufacturing fields, and has good application prospects in the high-value recycling of decommissioned crystalline silicon photovoltaic modules, the high-purity sorting of encapsulation materials, and the renewable resource recycling industry chain.
[0054] Compared with the prior art, the present invention has the following significant advantages, as detailed below: (1) Mild and low-energy chemically induced interface weakening: This invention proposes for the first time that immersion in a simple inorganic salt solution at medium and low temperatures can significantly reduce the adhesion between EVA and the glass interface. Its core lies in utilizing the dual mechanism of "ion penetration + interface polarity adjustment" to achieve efficient stripping of EVA from decommissioned photovoltaic modules. This invention is the first to discover and utilize the aforementioned interface weakening mechanism, successfully overcoming the technical bottleneck of existing technologies that rely on high temperatures, organic solvents, or highly corrosive media for EVA stripping. By cleverly using salt solution-induced interface weakening, the adhesion between EVA and glass is significantly reduced (≥70%, original stripping force: 1500-2000 N, stripping force after treatment: 300-500 N). Photovoltaic modules treated with weakened interfaces directly enter the "strippable range," greatly simplifying the process and making it more environmentally friendly.
[0055] (2) Low energy consumption: Separation can be achieved at medium and low temperatures. Traditional methods require 500-600°C, while the present invention only requires medium and low temperatures to achieve separation, reducing energy consumption by 70-85%. There is no smoke, no toxic solvent, and no residual adhesive cleaning steps during the separation process.
[0056] (3) Significantly improved material integrity: Experimental results show that the glass separation rate using the method of the present invention is ≥99%, the glass integrity is well maintained, the Ag in the wires is not significantly corroded, and the EVA residue is extremely low. Compared with the pyrolysis method (silicon wafer integrity rate of 30-60%), the present invention has an overwhelming advantage.
[0057] (4) More suitable for industrialization (continuous production): Due to the low processing temperature and non-toxicity, there is no need for complex exhaust gas purification equipment, high-temperature furnaces, or organic solvent circulation systems. It is suitable for establishing modular separation production lines that can operate continuously.
[0058] (5) The salt solution is cheap, safe, non-toxic and recyclable: The preferred soluble inorganic salt of this invention has a highly competitive industrial cost and excellent environmental protection, and the solution can be used in a closed loop.
[0059] (6) Significant carbon reduction benefits: Based on the total carbon emissions of the entire process of recycling retired photovoltaic modules, the carbon accounting results show that the carbon emissions of the heating process account for as high as 48.9%, which is the main source of carbon emissions; the green soaking process adopted in this invention accounts for only 21.5% of carbon emissions, which significantly reduces the energy consumption and carbon emissions of the process; the reuse of recycled materials can achieve a carbon reduction of 14.9%, and the overall process has excellent low-carbon application value and carbon reduction potential.
[0060] Additional aspects and advantages of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description
[0061] Figure 1 This is a schematic diagram of the separation method process in Embodiments 1-4 of the present invention.
[0062] Figure 2 This is a schematic diagram of the micro-swelling and ion permeation that occur at the EVA-glass interface after treatment in NaCl solution at 80°C in Example 1 of the present invention.
[0063] Figure 3 This is a schematic diagram of the appearance of microbubbles and reduced interfacial energy near the Ag wire in Embodiment 1 of the present invention: the right figure is a partial enlarged view of the part selected in the left figure.
[0064] Figure 4 This is an experimental curve showing the decrease in adhesion force with salt solution treatment time in Example 1 of the present invention.
[0065] Figure 5 This is a schematic diagram of the EVA separation system for decommissioned photovoltaic modules in Embodiment 5 of the present invention.
[0066] Figure 6 This is a schematic diagram of the main functional unit component module structure of the EVA separation system for decommissioned photovoltaic modules in Embodiment 5 of the present invention. Detailed Implementation
[0067] The following will clearly and completely describe the concept and technical effects of the present invention in conjunction with embodiments, so as to fully understand the purpose, features and effects of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are all within the scope of protection of the present invention. Unless otherwise specified, the experimental methods used in the embodiments are conventional methods; the materials and reagents used, unless otherwise specified, are commercially available. Unless otherwise specified, the same parameter value is the same in all embodiments. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0068] In the description of this invention, references to terms such as "some embodiments" indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0069] Unless otherwise specified, "%" in this invention represents mass percentage.
[0070] Salt spray is a highly corrosive atmospheric environment. Chloride ions easily penetrate along the surface and interfacial pores of photovoltaic modules, causing metal corrosion, aging of encapsulation materials, and debonding of interlayer interfaces, resulting in deterioration of module structure and electrical performance, ultimately leading to service failure. This technology reverses this by utilizing the interface weakening and encapsulation layer aging debonding effect induced by salt spray as an auxiliary dissociation method, applied to the green recycling and layer separation of retired photovoltaic modules. In existing technologies, no patents or literature have reported that the adhesion between EVA and glass can be significantly reduced by using salt solutions, nor have they revealed a technical solution for efficiently promoting EVA removal using ion penetration and interfacial polarity regulation. Through extensive experimental research, this invention has found that: 1) the encapsulation material EVA undergoes slight swelling in a specific inorganic salt aqueous solution, providing initial conditions for interfacial separation; 2) a unique "ion-induced microbubble" phenomenon appears near the Ag conductor, which can effectively disrupt the interfacial bond between EVA and the substrate. Under the synergistic effect of the above, the interfacial adhesion between EVA and glass can be reduced by more than 70%. Based on this, the EVA layer can be completely peeled off under set medium-temperature conditions without damaging the glass. The above experimental results show that the inorganic salt solution-assisted medium-temperature stripping technology proposed in this invention can achieve efficient and non-destructive separation of EVA under conditions of low temperature, non-toxicity, and low energy consumption, which is something that previous separation technologies could not achieve.
[0071] To address the problems of EVA film removal in existing decommissioned photovoltaic modules under low-to-medium temperature conditions, high energy consumption of traditional processes, significant environmental risks from toxic solvents, easy damage to glass and silicon wafers, and difficulties in subsequent precious metal extraction from silicon wafers, the core objective of this invention is to provide a green, efficient, and industrially scalable EVA layer separation technology that does not require high-temperature pyrolysis (500-600°C), does not require the use of toxic organic solvents, does not require strong acid or alkali corrosion, can separate EVA with low damage within a medium temperature range, maintains the integrity of silicon wafers, and creates conditions for subsequent silver extraction.
[0072] This invention provides a highly efficient separation process based on salt solution-induced EVA softening and interface weakening, specifically including the following steps: Step 1: Pre-crushing treatment Retired photovoltaic modules are broken down to create 3-10 cm cracks or fragments in the glass layers, thereby increasing the contact area at the interface. The purpose of breaking down is not to pulverize, but to enhance immersion permeability while preserving the integrity of the glass structure. Breaking methods can include impact breaking, rolling breaking, or shear breaking.
[0073] Step 2: Salt solution induces interfacial weakening The crushed components are placed in an immersion solution containing soluble inorganic salts and immersed for a preset immersion period at a preset medium temperature. The soluble inorganic salts include at least one of sodium, potassium, magnesium, calcium, and aluminum salts.
[0074] Step 3: Medium-temperature heat softening and hot knife cutting After processing, the component is heated, transitioning from a highly elastic state to a viscous flow state with extremely low interfacial bonding energy. Using a hot knife at 150-180℃ and a cutting speed of 3-6 cm / s, rapid separation of glass, EVA, and silicon wafers can be achieved.
[0075] The hot knife parameters are set as follows: Temperature: 150-180°C; Cutting speed: 3-6 cm / s; Blade pressure: 20-50 N; Blade material: nickel-chromium alloy or silicon carbide coating. This step does not require strong mechanical separation and protects both the glass and the silicon wafer.
[0076] Step 4: Material Recycling The crushed components after the above treatment are screened and separated, and the glass, battery cells and backsheet materials are collected separately. After being washed with deionized water and dried, the recycling is completed.
[0077] The novel technical approach of "salt solution-induced interface weakening + medium-temperature hot knife cutting" proposed in this invention effectively solves several common technical problems in the industry, including at least the following: 1) How to significantly reduce the interfacial adhesion between EVA and glass / silicon wafers? 2) How to achieve peeling with low energy consumption? 3) How to improve the purity of recycled glass? 4) How to construct a continuous separation process suitable for industrialization? Example 1
[0078] This example provides a method for EVA separation in photovoltaic modules based on salt solution-induced separation, such as... Figure 1 As shown, the specific operation is as follows: Step 1: Pre-crushing treatment After removing the frames and junction boxes, retired crystalline silicon photovoltaic modules are sent to a crushing equipment for crushing. An impact crushing method is used to break the tempered glass at the front end into 3-10 cm fragments without damaging the overall structure of the silicon wafer.
[0079] Step 2: Salt solution induces interfacial weakening The broken photovoltaic modules were placed in an immersion solution containing soluble inorganic salts and immersed at a preset temperature of 80°C for 2 hours. The total molar concentration of inorganic salts in the immersion solution was 1 mol / L. After the salt solution was prepared, it was preheated to 80°C. The broken photovoltaic modules were then completely immersed in the constant-temperature salt solution at a solid-liquid ratio of 1 kg: 5 L. Under sealed conditions, the modules were continuously stirred at 400 rpm for 2 hours. The stirring throughout the process accelerated the heat transfer in the liquid phase and the bidirectional penetration of anions and cations. The microscopic adhesion between the EVA and glass substrate was weakened through ion wetting and micro-electrochemical effects.
[0080] A schematic diagram illustrating the micro-swelling and ion permeation mechanism of the EVA-glass interface after immersion in inorganic salt solution is shown below. Figure 2 As shown in the figure (NaCl is used as an example in the figure; other salts have similar effects). It can be seen from the figure that sodium chloride first penetrates through the glass crack, then EVA undergoes hydrolysis, generating acidic substances (acetic acid, hydrogen ions, etc.). These acidic substances reduce the adhesion at the glass-EVA interface. During the implementation process, microbubbles were observed near the Ag wire, and the interfacial energy decreased. Specific phenomena are shown in the figure. Figure 3 As shown, the right image in the figure is an enlarged view of the selected area in the left image.
[0081] The diagram illustrating the relationship between adhesion force (peeling force) and soaking time during the NaCl soaking process is shown below. Figure 4 As shown.
[0082] The interface weakening mechanism in the embodiments of this invention is speculated as follows: 1) Ion penetration enhances the destruction of the hydration layer: Anions preferentially interact with the polar functional groups of the EVA interface, reducing hydrogen bonds and van der Waals forces. 2) EVA micro-swelling promotes chain segment loosening: improving thermal softening efficiency. 3) Microbubbles at the wire indicate a decrease in interfacial energy: Electrochemical perturbations in the Ag electrode region lead to gas evolution. 4) The combined effect reduces interfacial adhesion by ≥70%: making separation possible under intermediate temperature conditions.
[0083] Step 3: Medium-temperature heat softening and hot knife cutting After treatment, the component was heated to 90°C and held for 15 minutes. At this temperature, EVA transitioned from a highly elastic state to a viscous flow state, and the interfacial bonding energy decreased significantly. Using a hot blade at 160°C (blade pressure: 40N; blade material: nickel-chromium alloy) at a cutting speed of 5cm / s, rapid separation of glass, EVA, and silicon wafer was achieved. During cutting, it was observed that the EVA layer was cut continuously and stably without molten droplet splashing; no stress cracks were generated in the glass; and the blade was subjected to uniform force, requiring minimal mechanical force.
[0084] Step 4: Material Recycling The crushed components after the above treatment are screened and separated, and the glass, battery cells and backsheet materials are collected separately. After being washed with deionized water and dried, the recycling is completed.
[0085] In this example, to compare the effects of different salt systems, four types of salt solutions were prepared: System 1 (single salt system) consists of NaCl, KCl, MgCl2, CaCl2, or AlCl3; System 2 (single salt system) consists of Na2SO4, K2SO4, MgSO4, Al2(SO4)3, Na2CO3, K2CO3, or MgCO3; System 3 (chloride-sulfate complex system) is ①80%NaCl+20%Na2SO4 or ②80%KCl+20%K2SO4; System 4 (sodium salt-magnesium calcium aluminum salt complex system) is one of the following: ①80% NaCl+20% MgCl2; ②80% NaCl+20% CaCl2; ③80% NaCl+20% AlCl3; ④80% Na2SO4+20% MgSO4.
[0086] The phenomena observed after soaking in the above four salt systems are shown in Table 2 below: Table 2
[0087] *The EVA swelling rate test in the table above is the result of three parallel tests, so the result is a range value.
[0088] The method for testing the swelling rate is as follows: Take pure EVA film (after removing impurities) and cut it into samples of uniform size. Vacuum dry the samples at 60 °C to constant weight and record the weight as W0. Immerse the samples in a sufficient amount of solvent at a constant temperature for a set time. After removal, gently wipe the surface of free solvent with filter paper and quickly weigh to obtain the swollen wet weight W1. Then, vacuum dry the samples again to constant weight and weigh W2. Calculate the mass swelling rate. Calculate the dissolution loss rate, set up 3 parallel samples for each group, take the average value, and label the experimental conditions such as solvent, temperature, soaking time, etc.
[0089] The peel force test data after soaking are shown in Table 3 below.
[0090] Table 3
[0091] *For simplification, the peel force test results were rounded to the nearest hundred. Since the test results were obtained from three parallel measurements, range values are shown for parts with slightly larger differences.
[0092] The peel force test method is as follows: Photovoltaic glass-EVA composite sheets were cut into standard narrow strips and subjected to 180° peel tests using a Guangdong Jitian Electronics universal tensile testing machine. A constant tensile rate of 50 mm / min was set on the crossbeam to peel the glass from the EVA interface. The peel strength was calculated by taking the maximum peel force during the steady-state peeling phase. Multiple sets of parallel samples were used for each group to reduce errors. Lower peel force allows for lower operating conditions in the subsequent hot-blade cutting process, such as lower temperatures and lower energy consumption.
[0093] The analytical results of the separated material that entered the peelable zone and completed the peeling process are shown in Table 4 below: Table 4
[0094] Example 2
[0095] This example provides a salt solution-induced EVA separation method for photovoltaic modules, which differs from Example 1 in that the immersion temperature is different (60°C, 80°C, or 100°C). Different chloride solutions were tested at each temperature, with the immersion solution being either a 1 mol / L NaCl solution or a 1 mol / L KCl solution.
[0096] The changes in appearance, interfacial phenomena, and peel strength test results of EVA after soaking in different types of chloride solutions are summarized in Tables 5 and 6 below.
[0097] Table 5
[0098] Among them, the size is almost unchanged to the naked eye, the hardness and appearance are unchanged, and the swelling rate is 1~10% which is slight swelling; the thickness increases slightly, the color turns slightly white, and the feel is not sticky, with a swelling rate of 10~30% which is moderate swelling; the thickness increases significantly and curls up, and the rebound is slower, with a swelling rate of 30~40% which is moderate to strong swelling.
[0099] Table 6
[0100] *For simplification, the peel force test results were rounded to the nearest hundred. Since the test results were obtained from three parallel measurements, range values are shown for parts with slightly larger differences.
[0101] As can be seen from Tables 5 and 6, the optimal immersion temperature is 80℃. At this temperature, both sufficient ion penetration and good preservation of clear glass without fogging can be ensured.
[0102] Example 3
[0103] This example provides a method for EVA separation in photovoltaic modules based on salt solution induction. The difference between this method and Example 1 is that the concentration of soluble inorganic salt in the soaking solution is 0.5 mol / L, 1 mol / L or 2 mol / L, and the soluble inorganic salt used is sodium chloride.
[0104] The peel strength test results of the EVA after soaking are shown in Table 7 below.
[0105] Table 7
[0106] As can be seen from the table above, the NaCl concentration of the present invention is optimal in terms of both economy and effectiveness when it is 1 mol / L.
[0107] Example 4
[0108] This example provides a method for separating EVA from photovoltaic modules based on salt solution induction. The difference between this method and Example 1 is that the soaking time is 0.5h, 1h or 2h, and the soluble inorganic salt used is sodium chloride.
[0109] The peel strength test results of the EVA after soaking are shown in Table 8 below.
[0110] Table 8
[0111] As can be seen from the table above, a soaking time of 2 hours provides the best economic benefits.
[0112] Example 5
[0113] This example provides a salt solution-induced EVA separation system for decommissioned photovoltaic modules, such as... Figure 5 and 6 As shown, it includes, in sequence, a crushing unit, a salt solution soaking unit, a preheating unit, a hot knife cutting unit, and a sorting and collection unit.
[0114] The crushing unit includes a pretreatment module and a crushing module. The crushing module includes an automatic crushing and conveying module, which includes a feed inlet, a crushing roller assembly (including crushing roller A and crushing roller B), and a conveying device. After manual pretreatment, the photovoltaic module is conveyed to the feed inlet and enters the crushing roller assembly for crushing. After processing, it is conveyed to the salt solution soaking unit.
[0115] The salt solution immersion unit includes a salt solution heating module and an immersion conveyor chain. The salt solution heating module specifically includes a heating element and an immersion tank. The heating element is used to heat the immersion solution, and the immersion tank is used to hold the immersion solution. After immersion for 30~120 minutes, the photovoltaic modules are transported to the preheating unit via the conveyor chain.
[0116] The preheating unit includes a hot air preheating module, specifically including a hot air preheating zone located at the front end of the hot knife cutting unit.
[0117] The hot knife cutting unit includes a track-mounted hot knife cutting module, which comprises a conveyor track, a hot knife assembly, and a control module. The control module is used to control the operating signals of the conveyor track and the hot knife assembly.
[0118] The sorting and collection unit includes a material conveying module and a product temporary storage module. The product temporary storage module includes glass, silicon wafer, and EVA recycling devices. The material conveying module conveys the separated materials for easy sorting, and the sorted products are temporarily stored in the glass, silicon wafer, and EVA recycling devices, respectively.
[0119] A solution circulation and purification unit can also be set up in the system. The solution circulation and purification unit is connected to the salt solution soaking unit and is used to circulate and purify the soaking solution.
[0120] The statistical results of the data after 2 hours of industrial trial operation of the system are shown in Table 9 below.
[0121] Table 9
[0122] The statistical process in this table uses an immersion temperature of 80℃, an immersion time of 30~120min for the immersion conveyor chain (the statistical data in the table above is calculated based on a 120min immersion time), a hot air preheating zone temperature of 80~100℃, and a hot knife working temperature of 150~180℃ for the track-type hot knife cutting system.
[0123] As can be seen from the table above, the solution of this invention is fully capable of large-scale industrial application.
[0124] Comparative Example 1 This example provides a method for separating EVA in photovoltaic modules, which differs from Example 1 in that the soaking solution is replaced with pure water. The same stirring and temperature control as in Example 1 are used throughout the process to eliminate the interference of the swelling effect of high-temperature pure water alone on the EVA / glass interface adhesion performance.
[0125] The results of the immersion test are as follows: After immersion in pure water, the swelling rate of the EVA film is less than 3%, with only a small amount of water absorption and swelling; no microbubbles are generated on the surface of the silver grid lines; pure water is difficult to penetrate into the micro-gap between EVA and glass, and the EVA-glass interface bonding structure basically remains in its original state with no signs of micro-debonding; the cover glass is completely transparent without fogging, and the silicon solar cells have no cracks or local detachment; the test interface peel force is 1450~1800 N, and the attenuation of interface bonding strength is negligible.
[0126] This method involves immersing pre-crushed photovoltaic modules in a solution containing soluble inorganic salts at a predetermined medium temperature for a set time. Active anions are then directed to penetrate the glass-EVA interface, promoting a directional weakening of interfacial adhesion. After treatment, the interfacial peel force is reduced to 300-500N, entering the peelable range. Subsequently, under specific medium-temperature heating conditions, a hot knife is used to cut along the interface at a set speed, achieving rapid and low-energy separation of the glass-EVA-silicon wafer structure. The soluble inorganic salts used in this invention include at least one of sodium, potassium, magnesium, calcium, and aluminum salts. The synergistic effect of multi-component compounding further enhances the interfacial modification effect. Compared with traditional high-temperature pyrolysis methods, this method significantly reduces energy consumption and carbon emissions while maintaining the transparency of the glass and the integrity of the silicon wafer, achieving a glass separation rate of over 99%, demonstrating extremely high economic value and industrialization potential.
[0127] The embodiments of the present invention have been described in detail above, but the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention.
Claims
1. A method for EVA separation in photovoltaic modules based on salt solution-induced separation, characterized in that: Includes the following steps: S1. Salt solution-induced interface weakening: The photovoltaic module is immersed in a solution containing soluble inorganic salts at 60~100℃; the soluble inorganic salts include cations and anions, the cations include at least one of alkali metal ions, alkaline earth metal ions or aluminum ions; the anions include chloride ions; S2. Medium-temperature heat softening and hot knife cutting: After immersion treatment, the temperature of the photovoltaic module is controlled at 80~100℃. Hot cutting can be used to separate the EVA layer from other parts of the photovoltaic module.
2. The method for EVA separation in photovoltaic modules based on salt solution induction according to claim 1, characterized in that: The cation includes Na. + K + Mg 2+ Ca 2+ Or Al 3+ At least one of the following; and / or, the anion further includes at least one of sulfate ion or carbonate ion.
3. The method for EVA separation in photovoltaic modules based on salt solution induction according to claim 1, characterized in that: The soluble inorganic salt contains at least two anions or at least two cations; and / or, the mass of the chloride salt in the soluble inorganic salt accounts for 50-100% of the mass of the soluble inorganic salt.
4. The method for EVA separation in photovoltaic modules based on salt solution induction according to claim 1, characterized in that: The anions include a mixture of chloride and sulfate ions; or, the cations include a mixture of magnesium, calcium, aluminum ions and sodium ions.
5. The method for EVA separation in photovoltaic modules based on salt solution induction according to claim 1, characterized in that: The soluble inorganic salts include mixtures of sodium chloride and sodium sulfate, mixtures of potassium chloride and potassium sulfate, mixtures of sodium chloride and magnesium chloride, and mixtures of sodium chloride and calcium chloride.
6. The method for EVA separation in photovoltaic modules based on salt solution induction according to claim 1, characterized in that: The soaking treatment in step S1 includes at least one of the following conditions: 1) the total molar concentration of soluble inorganic salts in the soaking solution is 0.5~2 mol / L; 2) the soaking treatment time is 1~4 h; 3) during the soaking treatment, the solid-liquid ratio of the photovoltaic module to the soaking solution is 1 kg: 4 L~6 L.
7. The method for EVA separation in photovoltaic modules based on salt solution induction according to claim 1, characterized in that: The photovoltaic module is pre-crushed before being immersed, and the characteristic size of the pre-treated photovoltaic module is between 3cm and 10cm; and / or, the working parameters of the thermal cutting include at least one of the following parameters: 1) temperature of 150~180℃; 2) cutting speed of 3~6cm / s.
8. A system for implementing the separation method as described in any one of claims 1 to 7, characterized in that: It includes, in sequence, an immersion module, a preheating module, and a hot knife cutting unit.
9. The system according to claim 8, characterized in that: The system also includes a crushing module.
10. The application of the method according to any one of claims 1 to 7 or the system according to claim 8 or 9 in the recycling of photovoltaic modules.