Disassembly methods for power battery packs, disassembly systems for power battery packs, and battery cells.

By subjecting the power battery pack to alternating temperature cycling and monitoring the interface damage index, the problems of long disassembly time and high energy consumption of power battery packs have been solved, achieving more efficient and less damaged separation of cells from the casing, improving disassembly efficiency and the cascade utilization value of cells.

CN123102718APending Publication Date: 2026-11-17BEIJING CHEHEJIA AUTOMOBILE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611356268.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing power battery pack disassembly processes are time-consuming and energy-intensive, and the reduction in interface adhesion is limited, resulting in a high cell disassembly damage rate and a lack of quantitative judgment standards.

Method used

By subjecting the power battery pack to at least three alternating temperature cycles, monitoring the interface damage index of the bonding interface, and performing a final cooling process when the preset threshold or number of cycles is reached, the separation of the battery cell from the housing is achieved by combining the temperature control module, monitoring module, and separation operation module.

Benefits of technology

It shortens disassembly time, reduces energy consumption, improves disassembly efficiency and cell integrity, quantifies interface damage assessment, and reduces mechanical force damage to the cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102718A_ABST
    Figure CN123102718A_ABST
Patent Text Reader

Abstract

This application provides a method for disassembling a power battery pack, a system for disassembling a power battery pack, and battery cells, relating to the field of battery pack disassembly technology. The disassembly method includes: subjecting the power battery pack to at least three alternating temperature cycles. The power battery pack includes battery cells and a casing, with the battery cells and casing bonded together using structural adhesive. During the alternating temperature cycles, the interface damage index at the bonding interface between the battery cells and the casing is monitored. If the interface damage index is greater than or equal to a preset threshold, or if the total number of alternating temperature cycles reaches a preset number of cycles, a final cooling treatment is performed on the power battery pack. After the final cooling treatment, a separation operation is applied to the battery cells to separate them from the casing. The embodiments of this application can shorten the disassembly time of the power battery pack, reduce the energy consumption during disassembly, and improve the disassembly efficiency and yield of the power battery pack.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of battery pack disassembly technology, and in particular to a method for disassembling a power battery pack, a system for disassembling a power battery pack, and battery cells. Background Technology

[0002] After the power battery pack is retired, the non-destructive dismantling of the battery cells is a prerequisite for the secondary use of the battery cells and the recycling of materials.

[0003] In related technologies, the disassembly process of power battery packs usually involves placing the entire battery pack in a temperature chamber and refrigerating it at low temperatures for about 12 hours. This causes the structural adhesive used to bond the battery cells to the housing to become brittle at low temperatures. Then, tools are used to tap the interface gap between the battery cells and the housing, causing the battery cells to detach from the housing and be removed.

[0004] However, the above dismantling process has the problems of long processing time and high energy consumption. Summary of the Invention

[0005] The technical problem to be solved by this application is to provide a method for disassembling a power battery pack, a system for disassembling a power battery pack, and battery cells, so as to solve the problems of long processing time and high energy consumption in the disassembly process of power battery packs in related technologies.

[0006] To solve the above problems, this application provides the following technical solution: This application proposes a method for disassembling a power battery pack, the method comprising: The power battery pack is subjected to at least three alternating temperature cycles. Each alternating temperature cycle includes a low temperature holding stage and a high temperature holding stage, and the temperature difference between the high temperature holding stage and the low temperature holding stage is ≥40℃. The power battery pack includes cells and a housing, and the cells and the housing are bonded together with structural adhesive. During the alternating temperature cycling process, the interface damage index of the bonding interface between the battery cell and the housing is monitored. When the interface damage index is greater than or equal to a preset threshold, or when the total number of alternating temperature cycles reaches a preset number of cycles, the power battery pack is subjected to a final cooling treatment. After the final cooling process, a separation operation is performed on the battery cell to separate the battery cell from the housing.

[0007] Furthermore, the process of subjecting the power battery pack to at least three alternating temperature cycles includes: For a single alternating temperature cycle treatment, the temperature of the power battery pack is reduced to a first temperature and maintained at the first temperature for a first duration, where the first temperature is the temperature of the low temperature holding stage and the first duration is the duration of the low temperature holding stage; The temperature of the power battery pack is raised from the first temperature to the second temperature and maintained at the second temperature for a second duration. The second temperature is the temperature of the high-temperature holding stage, the second duration is the duration of the high-temperature holding stage, and the difference between the second temperature and the first temperature is ≥40℃.

[0008] Furthermore, the cooling rate for reducing the temperature of the power battery pack to the first temperature is ≥2℃ / min; and / or, The heating rate of the power battery pack from the first temperature to the second temperature is ≥3℃ / min.

[0009] Furthermore, the first temperature is -35℃ to -20℃, and the second temperature is 50℃ to 60℃.

[0010] Furthermore, the first duration and / or the second duration is 30 min to 60 min.

[0011] Furthermore, the power battery pack undergoes alternating temperature cycling treatment a total of 4 to 6 times.

[0012] Furthermore, the total cumulative time for alternating temperature cycling treatment of the power battery pack is ≤6 hours.

[0013] Furthermore, the temperature difference between the high-temperature holding stage and the low-temperature holding stage is 70℃~95℃.

[0014] Furthermore, an acoustic emission sensor is provided on the housing near the bonding interface; During the alternating temperature cycling process, monitoring the interface damage index at the bonding interface between the battery cell and the housing includes: During the alternating temperature cycling process, the acoustic emission signal of the bonding interface is collected by the acoustic emission sensor; The interface damage index is calculated based on the cumulative count of the acoustic emission signals.

[0015] Furthermore, the final cooling treatment of the power battery pack includes: The temperature of the power battery pack is reduced to the temperature of the final cooling treatment and maintained for a third duration; The final cooling process is performed at a temperature of -35℃ to -20℃, and the third cooling period is 20 min to 30 min.

[0016] Further, the step of applying a separation operation to the battery cell after the final cooling treatment to separate the battery cell from the housing includes: After the final cooling process, a wedge tool is inserted along the bonding interface and a force is applied to separate the battery cell from the housing.

[0017] Furthermore, before subjecting the power battery pack to at least three alternating temperature cycles, the disassembly method further includes: Based on the material type of the structural adhesive, process parameters for alternating temperature cycling treatment that match the material type are retrieved from a preset parameter library; wherein, the preset parameter library includes process parameters corresponding to at least two material types, and the process parameters include the temperature and duration of the low-temperature holding stage, the temperature and duration of the high-temperature holding stage, and the total number of alternating temperature cycling treatments performed on the power battery pack; The process of subjecting the power battery pack to at least three alternating temperature cycles includes: The power battery pack is subjected to at least three alternating temperature cycles according to the process parameters.

[0018] This application also proposes a disassembly system for a power battery pack, the disassembly system comprising a temperature control module, a monitoring module, and a separation operation module; wherein: The temperature control module is used to perform at least three alternating temperature cycles on the power battery pack. Each alternating temperature cycle includes a low temperature holding stage and a high temperature holding stage, and the temperature difference between the high temperature holding stage and the low temperature holding stage is ≥40℃. The power battery pack includes battery cells and a housing, and the battery cells and the housing are bonded together with structural adhesive. The monitoring module is used to monitor the interface damage index of the bonding interface between the battery cell and the housing during the alternating temperature cycle treatment. The temperature control module is also used to perform a final cooling treatment on the power battery pack when the interface damage index is greater than or equal to a preset threshold, or when the total number of alternating temperature cycles reaches a preset number of cycles. The separation operation module is used to apply a separation operation to the battery cell after the final cooling process to separate the battery cell from the housing.

[0019] This application also proposes a battery cell, which is obtained by disassembling the power battery pack using the disassembly method described above.

[0020] Compared with related technologies, the embodiments of this application have the following advantages: The disassembly method for the power battery pack provided in this application embodiment, by subjecting the power battery pack to at least three alternating temperature cycles and controlling the temperature difference between the high-temperature holding stage and the low-temperature holding stage during a single alternating temperature cycle to ≥40℃, can induce periodic shear fatigue stress at the bonding interface between the battery cell and the casing, accumulating interface fatigue damage. This weakens the adhesion force at the bonding interface in a shorter time and with lower energy consumption, shortening the disassembly time of the power battery pack, reducing the disassembly energy consumption of the power battery pack, and improving the disassembly efficiency and yield of the power battery pack. During the alternating temperature cycling process, the interface damage index of the bonding interface is monitored. When the interface damage index is greater than or equal to a preset threshold, or when the total number of alternating temperature cycles reaches a preset number of cycles, it indicates that the adhesion force of the bonding interface has decreased to a separable state. The power battery pack can then undergo a final cooling treatment to maintain the fatigued bonding interface in a low-temperature embrittlement state. This, combined with the interface fatigue damage caused by the alternating temperature cycling process, can significantly reduce the peeling force of the bonding interface, reduce the mechanical force required to separate the battery cell from the casing, reduce the damage to the battery cell during disassembly, and improve the integrity rate and cascade utilization value of the battery cell after disassembly.

[0021] It should be understood that the above general description and the following detailed description are exemplary and explanatory only, and do not limit this application. Attached Figure Description

[0022] Figure 1 This application provides a step-by-step flowchart of a method for disassembling a power battery pack. Figure 1 ; Figure 2 This is a logic block diagram of a power battery pack disassembly system provided in an embodiment of this application; Figure 3 This is a schematic diagram illustrating the principle of interfacial shear stress generated at an adhesive interface during the low-temperature holding stage, as provided in an embodiment of this application. Figure 4 This is a schematic diagram illustrating the principle of interfacial shear stress generated at an adhesive interface during the high-temperature holding stage, as provided in an embodiment of this application. Figure 5 This is a schematic diagram of a temperature control curve for alternating temperature cycle processing provided in an embodiment of this application; Figure 6 This is a schematic diagram illustrating the cumulative law of interface damage index with the number of cycles of alternating temperature provided in an embodiment of this application; Figure 7 This application provides a step-by-step flowchart of a method for disassembling a power battery pack. Figure 2 . Detailed Implementation

[0023] To make the above-mentioned objectives, features and advantages of this application more apparent and understandable, the application will be further described in detail below with reference to the accompanying drawings and specific embodiments.

[0024] Method Implementation Examples After a power battery pack is decommissioned, the non-destructive disassembly of the battery cells is a crucial preliminary step for the secondary use of the cells and the recycling of materials. In the manufacturing process of a power battery pack, the cells are bonded to the bottom surface of the casing (water-cooled plate) with structural adhesive, forming a high-strength adhesive interface. In related technologies, the disassembly process typically involves placing the entire battery pack in a temperature chamber and refrigerating it at low temperatures for approximately 12 hours. This allows the structural adhesive to become brittle at low temperatures, after which tools are used to tap the interface gap between the cells and the casing, causing the cells to detach from the casing. The above technical solutions have the following shortcomings: First, the processing time is too long: 12 hours of refrigeration causes the temperature box to be occupied for a long time. At the same time, due to the long processing time, the number of battery packs that can be disassembled per day is severely limited.

[0025] Second, it has extremely high energy consumption: cooling the entire battery pack (including the casing, water cooling plate, battery cells, etc.) to a low temperature and maintaining it for 12 hours consumes a great deal of energy.

[0026] Third, the mechanism of action is simple: relying solely on low temperature to embrittle the adhesive layer, the reduction in interfacial adhesion is limited. This results in a large mechanical force required to remove the battery cell from the casing by tapping the interface gap between the battery cell and the casing with tools, leading to a high rate of damage during battery cell disassembly.

[0027] Fourth, the process parameters rely on engineering experience and lack quantitative judgment standards: the temperature under low-temperature conditions (e.g., -30℃) and the refrigeration time under low-temperature conditions are both empirical values. The disassembly effect varies greatly under different structural adhesive formulations and different working conditions, and there is no quantitative judgment basis for interface damage.

[0028] To address the aforementioned problems, this application provides a method for disassembling a power battery pack, referring to... Figure 1 The disassembly method may specifically include the following steps: Step S101: Perform at least three alternating temperature cycles on the power battery pack. The power battery pack includes cells and a housing, and the cells and housing are bonded together with structural adhesive.

[0029] Step S102: During the alternating temperature cycling process, monitor the interface damage index of the bonding interface between the battery cell and the housing.

[0030] Step S103: Determine whether the following conditions are met: the interface damage index is greater than or equal to the preset threshold, or the total number of alternating temperature cycles reaches the preset number of cycles.

[0031] Step S104: When the interface damage index is greater than or equal to a preset threshold, or when the total number of alternating temperature cycles reaches a preset number of cycles, perform the final cooling treatment on the power battery pack.

[0032] Step S105: After the final cooling process, a separation operation is performed on the battery cell to separate the battery cell from the housing.

[0033] The disassembly method for the power battery pack provided in this application embodiment can be applied to, for example, Figure 2 The power battery pack disassembly system shown includes a temperature control module 21, a monitoring module 22, a separation operation module 23, and a control module 24. The control module 24 establishes communication connections with the temperature control module 21, the monitoring module 22, and the separation operation module 23, and acts as the core control unit to control the temperature control module 21, the monitoring module 22, and the separation operation module 23 to work together to realize the disassembly method of the power battery pack.

[0034] The temperature control module 21 is a programmable module, used to receive control instructions from the control module 24 and perform the operation of step S101 to perform at least three alternating temperature cycles on the power battery pack. It is also used to receive control instructions from the control module 24 and perform the operation of step S104 to perform the final cooling process on the power battery pack.

[0035] The monitoring module 22 is used to receive control commands from the control module 24 and execute the operation of step S102. During the alternating temperature cycle processing, it monitors the interface damage index of the bonding interface between the cell and the housing in real time and feeds back the monitored interface damage index to the control module 24 in real time.

[0036] The separation operation module 23 is used to receive the control command from the control module 24 and execute the operation in step S105 after the final cooling process to apply a separation operation to the battery cell to separate the battery cell from the housing.

[0037] The disassembly method for the power battery pack provided in this application embodiment can be used to disassemble a power battery pack in which the battery cells and the casing are fixed together by structural adhesive, thereby achieving the separation of the battery cells and the casing.

[0038] Before step S101, electrical components other than the cells in the power battery pack can be removed, leaving the cells and the housing assembly intact. This ensures that there is no electrolyte leakage from the cells, thereby reducing the ineffective heat load during the alternating temperature cycle process, reducing temperature control energy consumption, avoiding damage to electrical components from alternating high and low temperatures, and facilitating the subsequent classification and recycling of electrical components. At the same time, it eliminates the interference of external electrical components on the cell separation process and improves the efficiency of the dismantling operation.

[0039] In some embodiments, electrical components other than the battery cell may include, but are not limited to, internal wiring harnesses, battery disconnect units (BDUs), copper busbars, and battery strips.

[0040] In step S101, the control module can perform at least three alternating temperature cycles on the power battery pack through the temperature control module.

[0041] The single alternating temperature cycle treatment includes a low temperature holding stage and a high temperature holding stage. The temperature of the low temperature holding stage is lower than that of the high temperature holding stage, and the temperature difference between the high temperature holding stage and the low temperature holding stage is ≥40℃. This temperature difference can cause the materials on both sides of the bonding interface to generate periodic differential thermal strain due to the difference in the coefficient of thermal expansion, forming periodic shear stress at the bonding interface. After multiple cycles, the interface fatigue damage is accumulated, reducing the adhesion of the bonding interface to a separable state, thereby achieving the weakening of the adhesion of the bonding interface in a shorter time and with lower energy consumption.

[0042] The insulation duration of the low-temperature holding stage can be the same as or different from that of the high-temperature holding stage. The specific duration can be determined according to the actual working conditions. This application does not impose any specific limitations on this.

[0043] Structural adhesives are polymeric adhesives, including but not limited to polyurethane structural adhesives and epoxy resin structural adhesives.

[0044] The enclosure includes a water-cooled plate; specifically, the battery cells are bonded to the water-cooled plate in the enclosure using structural adhesive.

[0045] The casing of the battery cell and the water-cooling plate are usually made of metal. For example, the casing of the battery cell and the water-cooling plate are both made of aluminum. Referring to Table 1, taking the bonding structure composed of polyurethane structural adhesive, aluminum casing of the battery cell and aluminum substrate water-cooling plate as an example, the linear thermal expansion coefficient of polyurethane structural adhesive is 100μm / (m·℃)~150μm / (m·℃), which is significantly higher than the linear thermal expansion coefficient of aluminum material of 23μm / (m·℃). The difference between the two is about 4.3 times to 6.5 times. During the alternating temperature change process, under the action of temperature difference ΔT, differential thermal strain will be generated between the structural adhesive and the aluminum casing of the battery cell, and between the structural adhesive and the water-cooling plate, which will then be converted into interfacial shear stress τ.

[0046] Table 1

[0047] The bonding interface between the battery cell and the housing includes a first interface between the battery cell housing and the structural adhesive, and a second interface between the structural adhesive and the water-cooling plate of the housing.

[0048] For example, refer to Figure 3 and Figure 4The battery cell casing is made of aluminum, and the structural adhesive is polyurethane. The water-cooling plate inside the housing is made of aluminum, and the aluminum casing of the battery cell is bonded to the water-cooling plate using polyurethane structural adhesive. (Refer to...) Figure 3 During the low-temperature holding stage, because the linear thermal expansion coefficient of polyurethane structural adhesive is significantly higher than that of aluminum, the shrinkage of the polyurethane structural adhesive layer as the intermediate layer is significantly greater than that of the aluminum shell of the battery cell and the water-cooling plate, generating inward shear stress at the first and second interfaces. (Refer to...) Figure 4 During the high-temperature holding stage, because the linear thermal expansion coefficient of polyurethane structural adhesive is significantly higher than that of aluminum, the expansion of the polyurethane structural adhesive layer as the intermediate layer is significantly greater than that of the aluminum shell of the battery cell and the water-cooling plate, resulting in outward shear stress at the first interface and the second interface.

[0049] In some embodiments, the inward shear stress generated at the adhesive interface during the low-temperature holding phase is greater than the outward shear stress generated at the adhesive interface during the high-temperature holding phase.

[0050] Although the amplitude of interfacial shear stress generated by a single alternating temperature cycle is limited, cumulative fatigue damage will occur at the bonding interface after N cycles, and the interfacial adhesion will continuously decrease according to the fatigue law with the number of cycles. Here, N represents the preset number of cycles, and N is an integer greater than or equal to 3.

[0051] In some embodiments, in step S101, the control module can record in real time the total number of alternating temperature cycles performed on the power battery pack.

[0052] In some embodiments, the temperature difference between the high-temperature holding stage and the low-temperature holding stage can be a range of one or any two of 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, and 100°C.

[0053] During the alternating temperature cycle process, the control module can execute step S102 through the monitoring module to monitor the interface damage index of the bonding interface between the cell and the housing in real time, and feed back the monitored interface damage index to the control module in real time so that the control module can compare the current interface damage index with the preset threshold in real time.

[0054] In some embodiments, the monitoring module includes an acoustic emission sensor and a signal processing unit. The acoustic emission sensor can be positioned on the housing near the bonding interface to collect acoustic emission signals generated by the initiation and propagation of microcracks at the bonding interface in real time. The signal processing unit analyzes and processes the collected acoustic emission signals, calculates the interface damage index based on the cumulative count of the acoustic emission signals, and feeds back the interface damage index to the control module in real time.

[0055] In step S103, the control module can determine whether the interface damage index is greater than or equal to a preset threshold based on the interface damage index; and determine whether the total number of alternating temperature cycles has reached a preset number of cycles based on the total number of alternating temperature cycles. If either of these two conditions is met, the alternating temperature cycle process can be terminated, and the process can proceed to the final cooling step in step S104.

[0056] The preset threshold is the critical damage threshold at which the adhesion force of the bonding interface decreases to a state where it can be easily separated. As an example, the preset threshold can be a normalized value of 0.85.

[0057] The preset number of cycles refers to the maximum number of times the alternating temperature cycle processing is executed in advance. It serves as the termination condition for the alternating temperature cycle processing and is used to prevent the alternating temperature cycle processing from running indefinitely due to abnormal monitoring modules, special working conditions of the bonding interface, etc., thus ensuring the controllability of the disassembly process and production efficiency.

[0058] When the interface damage index is greater than or equal to the preset threshold, it indicates that the adhesion force of the bonding interface has been reduced to a separable state. The control module can execute step S104 to perform the final cooling treatment on the power battery pack through the temperature control module, so that the fatigued bonding interface is kept in a low-temperature embrittlement state, further reducing the interface peeling force.

[0059] The interface damage index is a normalized parameter used to characterize the degree of fatigue damage at the adhesive interface. (Refer to...) Figure 5 and Figure 6 As the number of alternating temperature cycles increases, the interface damage index gradually increases: when there is no fatigue damage at the bonding interface in the initial state, the interface damage index is 0; as the number of alternating temperature cycles increases, microcracks at the interface continuously initiate and expand, and the interface damage index gradually increases accordingly; when the interface damage index is 1, it means that the bonding performance of the bonding interface has completely failed; and after the fourth alternating temperature cycle, the interface damage index reaches 0.85, which is the same as the preset threshold, thus meeting the termination condition of the alternating temperature cycle.

[0060] If the interface damage index is less than the preset threshold, but the total number of alternating temperature cycles on the power battery pack reaches the preset number of cycles, it indicates that although the current bonding interface has not reached the theoretical critical damage state, it has completed the preset maximum number of cycles, and the bonding interface has accumulated enough fatigue damage. In this scenario, the control module can still execute step S104 to perform the final cooling treatment on the power battery pack through the temperature control module, so that the bonding interface that has developed fatigue can be kept in a low-temperature embrittlement state.

[0061] If the interface damage index is less than the preset threshold and the total number of alternating temperature cycles on the power battery pack has not reached the preset number of cycles, it indicates that the fatigue damage accumulation of the current bonding interface is not sufficient and the interface adhesion has not been weakened to a separable state. In this scenario, the control module can execute step S101 again until the interface damage index is greater than or equal to the preset threshold, or the total number of alternating temperature cycles reaches the preset number of cycles.

[0062] In step S104, the control module can reduce the temperature of the power battery pack to the final cooling temperature through the temperature control module and keep it warm, so that the fatigued bonding interface can reach a sufficient low-temperature embrittlement state.

[0063] In some embodiments, the temperature of the final cooling treatment can be the same as the temperature of the low-temperature holding stage, and the holding time of the final cooling treatment can be flexibly adjusted according to the low-temperature embrittlement state of the bonding interface. This application embodiment does not specifically limit this.

[0064] In step S105, after the final cooling process, the control module can apply a separation operation to the battery cell through the separation operation module to separate the battery cell from the housing. The separation operation may include, but is not limited to, wedge tool insertion and peeling, suction cup lifting and separation, and lifting mechanism lifting and separation.

[0065] After step S105, the battery cell can be subjected to visual inspection and basic electrical performance testing to determine whether it can be used for secondary applications. The basic electrical performance may include, but is not limited to, open circuit voltage (OCV) and direct current internal resistance (DCIR).

[0066] The disassembly method for the power battery pack provided in this application embodiment, by subjecting the power battery pack to at least three alternating temperature cycles and controlling the temperature difference between the high-temperature holding stage and the low-temperature holding stage during a single alternating temperature cycle to ≥40℃, can induce periodic shear fatigue stress at the bonding interface between the battery cell and the casing, accumulating interface fatigue damage. This weakens the adhesion force at the bonding interface with shorter duration and lower energy consumption, shortening the disassembly time of the power battery pack, reducing the disassembly energy consumption of the power battery pack, and improving the disassembly efficiency and yield of the power battery pack. For example, if the total number of alternating temperature cycles is 5, and the holding time of the low-temperature holding stage and the high-temperature holding stage is 30 minutes, then the total time for alternating temperature cycle treatment of the power battery pack in step S101 is approximately 4h~6h, which is shortened by approximately 50%~65% compared to the 12h of related technologies. In addition, the temperature of the low-temperature holding stage can be appropriately higher than -30℃ in related technologies (for example, -20℃), which can not only further shorten the alternating temperature cycle treatment time, but also reduce the overall energy consumption by approximately 40%.

[0067] Meanwhile, during the alternating temperature cycling process, the interface damage index of the bonding interface is monitored. When the interface damage index is greater than or equal to a preset threshold, or when the total number of alternating temperature cycles reaches a preset number of cycles, it indicates that the adhesion force of the bonding interface has decreased to a separable state. The power battery pack can then undergo a final cooling treatment to maintain the fatigued bonding interface in a low-temperature embrittlement state. This, combined with the interface fatigue damage caused by the alternating temperature cycling process, can significantly reduce the peeling force of the bonding interface, reduce the mechanical force required to separate the battery cell from the casing, reduce the damage to the battery cell during disassembly, and improve the integrity rate and cascade utilization value of the battery cell after disassembly.

[0068] Moreover, the process parameters in the embodiments of this application can be quantified, and the interface damage index provides a real-time assessment of the weakening degree of adhesion at the bonding interface, so that the timing of the end of the alternating temperature cycle treatment changes from relying on experience to data judgment, and the consistency between different batches is significantly improved.

[0069] Optionally, step S101, which involves subjecting the power battery pack to at least three alternating temperature cycles, includes: Step S1011: For a single alternating temperature cycle treatment, the temperature of the power battery pack is reduced to a first temperature and maintained at the first temperature for a first duration.

[0070] Step S1012: Raise the temperature of the power battery pack from the first temperature to the second temperature, and maintain it at the second temperature for a second duration.

[0071] In this embodiment, during the alternating temperature cycle treatment of the power battery pack, the control module can first lower the temperature of the power battery pack to a first temperature in step S1011 and maintain it at the first temperature for a first duration. Then, in step S1012, the temperature of the power battery pack is raised from the first temperature to a second temperature and maintained at the second temperature for a second duration. This stepwise temperature control method is beneficial to fully utilize the difference in thermal expansion coefficients between the structural adhesive and the metal substrates on both sides, causing the bonding interface to undergo two deformation stages of contraction and expansion. This generates shear stresses in opposite directions at the first interface between the cell and the structural adhesive, and at the second interface between the structural adhesive and the housing, constituting a complete alternating shear loading cycle. The bidirectional alternating shear stress can effectively drive the initiation and propagation of interfacial microcracks, improve the cumulative efficiency of interfacial fatigue damage, and accelerate the weakening speed of the bonding interface adhesion. This reduces the number of cycles required to weaken the interfacial adhesion to a separable state, further shortening the processing time for separating the cell from the housing and reducing the overall energy consumption of the disassembly process.

[0072] In each round of alternating temperature cycle processing, the control module can complete one alternating temperature cycle processing through the operations of steps S1011 to S1012.

[0073] The first temperature is the temperature of the low-temperature holding phase, and the first duration is the duration of the low-temperature holding phase.

[0074] The second temperature is the temperature during the high-temperature holding phase, the second duration is the duration of the high-temperature holding phase, and the difference between the second temperature and the first temperature is ≥40℃.

[0075] Optionally, in step S1011, the cooling rate of the power battery pack to the first temperature is ≥2℃ / min. For example, the cooling rate of the power battery pack to the first temperature can be one of 2℃ / min, 3℃ / min, 4℃ / min, 5℃ / min, 6℃ / min, 7℃ / min, and 8℃ / min, or a range between any two.

[0076] Optionally, in step S1012, the heating rate of the power battery pack from the first temperature to the second temperature is ≥3℃ / min. For example, the heating rate of the power battery pack from the first temperature to the second temperature can be one of 3℃ / min, 4℃ / min, 5℃ / min, 6℃ / min, 7℃ / min, 8℃ / min, 9℃ / min, and 10℃ / min, or a range between any two.

[0077] In the process of alternating temperature cycling treatment of the power battery pack, the embodiments of this application control the cooling rate of the power battery pack to a first temperature to be ≥2℃ / min, and / or control the heating rate of the power battery pack to be ≥3℃ / min. During the rapid temperature change, due to the dual differences in thermal response speed and thermal expansion coefficient, a more significant transient temperature difference stress is formed at the bonding interface between the structural adhesive and the metal substrates on both sides. This amplifies the amplitude of the interface shear stress in a single alternating temperature cycle treatment, improves the efficiency of interface damage accumulation in a single alternating temperature cycle treatment, and thus reduces the number of cycles required to weaken the interface adhesion to a separable state. This shortens the disassembly time for separating the battery cell from the casing and reduces the overall energy consumption of the disassembly process.

[0078] In some embodiments, both cooling rate and heating rate refer to the average temperature change rate of the temperature-controlled environment in which the power battery pack is located.

[0079] Optionally, the first temperature is -35℃ to -20℃, and the second temperature is 50℃ to 60℃. By controlling the first temperature of the low-temperature holding stage within the range of -35℃ to -20℃ and the second temperature of the high-temperature holding stage within the range of 50℃ to 60℃, this embodiment of the application can create a sufficient temperature difference between the low-temperature holding stage and the high-temperature holding stage, fully satisfying the conditions for the generation of interfacial shear stress. This allows the adhesive interface to generate stable and sufficiently large periodic shear stress during each round of alternating temperature cycles, improving the cumulative efficiency of interfacial fatigue damage.

[0080] Furthermore, the first temperature range can induce a certain degree of low-temperature embrittlement effect in the structural adhesive, which helps to weaken the adhesion force at the bonding interface and avoids the problems of increased cooling energy consumption and prolonged heating and cooling cycles caused by excessively low temperatures. The second temperature range can ensure that the structural adhesive undergoes sufficient thermal expansion deformation and that the temperature is within the safe tolerance range of the battery cell, further reducing the damage to the battery cell during the disassembly process. While improving disassembly efficiency and reducing energy consumption costs, it also takes into account the integrity rate and cascade utilization value of the battery cell after disassembly.

[0081] For example, the first temperature can be one of -35°C, -32°C, -30°C, -29°C, -26°C, -23°C, and -20°C, or a range between any two of them.

[0082] The second temperature can be one of 50℃, 52℃, 54℃, 55℃, 56℃, 58℃ and 60℃ or a range between any two.

[0083] Optionally, the first duration is 30 min to 60 min. Within this range, it is beneficial to promote the uniform reduction of the overall temperature of the power battery pack to the first temperature, allowing the structural adhesive and the metal substrates on both sides to fully complete the low-temperature shrinkage deformation, promoting the full establishment and stabilization of the inward shear stress at the first and second interfaces, and simultaneously assisting the structural adhesive to produce a moderate low-temperature embrittlement effect, thus enhancing the interface damage effect. Furthermore, this duration range can not only reduce the problems of uneven temperature field and insufficient interface stress loading caused by excessively short heat preservation time, but also reduce the problems of increased ineffective energy consumption and decreased efficiency of alternating temperature cycle treatment caused by excessively long heat preservation time. This helps to improve the single-cycle damage effect while taking into account the efficiency and energy consumption cost of dismantling and processing.

[0084] For example, the first duration can be one of 30 min, 35 min, 40 min, 45 min, 50 min, 55 min and 60 min or a range between any two.

[0085] Optionally, the second duration is 30 min to 60 min. Within this range, it is beneficial to promote the uniform increase of the overall temperature of the power battery pack to the second temperature, allowing the structural adhesive and the metal substrates on both sides to fully complete the high-temperature expansion deformation, and promoting the full loading of the outward shear stress at the first and second interfaces. Together with the shear stress in the low-temperature holding stage, it forms a complete alternating shear cycle, driving the full propagation of interface microcracks and improving the fatigue damage accumulation effect of a single alternating temperature cycle treatment. Furthermore, this duration range can not only alleviate the problems of insufficient thermal deformation and weakened alternating loading effect caused by insufficient heat preservation time, but also reduce the possibility of cell performance degradation caused by excessive heat preservation time, thus balancing cell quality and dismantling efficiency.

[0086] For example, the second duration can be a range of one or any two of 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, and 60 min.

[0087] It should be noted that the first duration and the second duration can be the same or different, and this application embodiment does not specifically limit this.

[0088] Optionally, in step S101, the total number of alternating temperature cycles N for the power battery pack is 4 to 6 times. Within this range, not only can sufficient fatigue damage be accumulated at the bonding interface, but the risk of the alternating temperature cycle process being executed indefinitely due to abnormal monitoring modules or special working conditions at the bonding interface can also be reduced, thereby improving the controllability and production efficiency of the disassembly process.

[0089] For example, the total number of alternating temperature cycles N for the power battery pack can be any one of 4, 5, and 6.

[0090] Optionally, the total cumulative duration of alternating temperature cycling treatment of the power battery pack is ≤6 hours.

[0091] In this embodiment of the application, the total cumulative duration of alternating temperature cycling of the power battery pack can be controlled to be less than or equal to 6 hours by adjusting the cooling rate, heating rate, and holding time during the alternating temperature cycling process, as well as adjusting the total number of alternating temperature cycles of the power battery pack.

[0092] This application embodiment controls the cumulative total time of alternating temperature cycling treatment of the power battery pack to be ≤6 hours, which can shorten the disassembly time of the power battery pack and reduce the energy consumption level of the disassembly process, thereby simultaneously improving the disassembly efficiency and reducing the disassembly cost of the power battery pack.

[0093] For example, the total cumulative duration of alternating temperature cycling treatment of the power battery pack can be one of 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours and 6 hours or any value between two of them.

[0094] Optionally, the temperature difference between the high-temperature holding stage and the low-temperature holding stage is 70℃~95℃. Within this range, the periodic differential thermal strain caused by the difference in thermal expansion coefficients of the materials on both sides of the bonding interface can be amplified, forming a periodic shear stress with a higher amplitude at the bonding interface. After multiple alternating temperature cycles, the accumulation rate of interface fatigue damage is accelerated, and the adhesion of the bonding interface is gradually weakened to a separable state. This is beneficial to further shorten the disassembly and processing time of the power battery pack and reduce the energy consumption level of the disassembly process.

[0095] For example, the temperature difference between the high-temperature holding stage and the low-temperature holding stage can be a range of 70°C, 75°C, 80°C, 85°C, 90°C and 95°C or any two of them.

[0096] Optionally, an acoustic emission sensor is installed on the housing near the bonding interface. Step S102, which involves monitoring the interface damage index of the bonding interface between the cell and the housing during alternating temperature cycling, includes: Step S1021: During the alternating temperature cycle process, the acoustic emission signal of the bonding interface is collected by an acoustic emission sensor.

[0097] Step S1022: Calculate the interface damage index based on the cumulative count of acoustic emission signals.

[0098] In this embodiment, during the monitoring of the interface damage index of the bonding interface between the battery cell and the housing, the control module can collect the acoustic emission signal of the bonding interface through the acoustic emission sensor in the monitoring module, and calculate the interface damage index based on the cumulative count of the acoustic emission signal by the signal processing unit in the monitoring module. This monitoring method does not require intrusion into the bonding interface and can dynamically reflect the degree of fatigue damage of the bonding interface without interfering with the normal operation of the alternating temperature cycle treatment. It provides quantitative data for determining the timing of termination of the alternating temperature cycle treatment and helps to improve the consistency and controllability of the disassembly process of different batches.

[0099] In some embodiments, a water-cooled plate is provided at the bottom of the enclosure, and the battery cell is bonded to the water-cooled plate at the bottom of the enclosure with structural adhesive. In this scenario, the acoustic emission sensor can be placed on the bottom surface of the enclosure, and the acoustic emission signal generated at the bonding interface can be conducted to the sensor through the solid medium between the water-cooled plate and the enclosure, ensuring the effectiveness of signal acquisition.

[0100] In step S1021, the control module can acquire acoustic emission signals from the bonding interface via the acoustic emission sensor in the monitoring module. Specifically, during the alternating temperature cycling process, when the bonding interface is subjected to periodic shear stress, microcracks initiate and propagate, releasing strain energy in the form of elastic waves. The acoustic emission sensor can continuously acquire the acoustic emission signals corresponding to these elastic waves throughout the entire alternating temperature cycling cycle and transmit the acquired acoustic emission signals to the signal processing unit.

[0101] In step S1022, the control module can calculate the interface damage index based on the cumulative count of acoustic emission signals through the signal processing unit in the monitoring module. Specifically, the signal processing unit uses the initial undamaged state of the bonding interface as the calculation benchmark, performs cumulative statistics on the collected valid acoustic emission events, and normalizes the real-time cumulative count value with the benchmark count value corresponding to the completely failed state of the bonding interface to obtain the interface damage index with a value range of 0 to 1.

[0102] Among them, the higher the value of the interface damage index, the higher the degree of fatigue damage at the bonding interface and the weaker the interface adhesion.

[0103] Optionally, the final cooling treatment of the power battery pack described in step S104 includes: Step S1041: Reduce the temperature of the power battery pack to the temperature of the final cooling process and maintain it for a third duration.

[0104] In this embodiment, during the final cooling process of the power battery pack, the control module can reduce the temperature of the power battery pack to the final cooling temperature and maintain it for a third duration. The final cooling temperature is -35℃ to -20℃, and the third duration is 20min to 30min. This embodiment can further induce a sufficient low-temperature embrittlement effect in the structural adhesive based on the interface fatigue damage accumulated during the previous alternating temperature cycle treatment, reducing the cohesive strength and interfacial adhesion strength of the structural adhesive layer, and providing a more favorable interface state for the subsequent separation operation of the battery cell and the casing. At the same time, controlling the final cooling temperature and the third duration within the above range is beneficial to improving the overall temperature uniformity and stability of the power battery pack during the final cooling process, making the degree of embrittlement of the bonding interface more consistent, reducing the risk of cell casing deformation and uneven structural adhesive layer residue during subsequent disassembly, and balancing disassembly efficiency and disassembly yield.

[0105] In step S1041, the temperature control module can reduce the temperature of the power battery pack to the final cooling treatment temperature at a cooling rate of ≥2℃ / min, and maintain it at the final cooling treatment temperature for a third time, so that the power battery pack can quickly reach the final cooling treatment temperature. During the cooling process, the thermal strain difference promotes the further expansion of the existing microcracks at the bonding interface. Combined with the continuous low temperature effect in the subsequent heat preservation stage, the structural adhesive is effectively embrittled in a short period of time, balancing the processing efficiency and embrittlement effect.

[0106] For example, the final cooling temperature can be one of -35°C, -32°C, -30°C, -29°C, -26°C, -23°C, and -20°C, or a range between any two.

[0107] In some embodiments, the final cooling temperature may be the same as or different from the temperature of the cryogenic holding phase.

[0108] For example, the third duration can be a range of 20 min, 22 min, 24 min, 26 min, 28 min, and 30 min, or any two of them.

[0109] Optionally, step S105, which involves performing a separation operation on the battery cell after the final cooling process to separate the battery cell from the casing, includes: Step S1051: After the final cooling process, wedge tool is inserted along the bonding interface and force is applied to separate the battery cell from the housing.

[0110] In this embodiment, the control module applies a separation operation to the battery cell to separate it from the casing. After the final cooling process, a wedge tool is inserted along the bonding interface and applied force to separate the battery cell from the casing. This separation method is suitable for the interface state after the final cooling, where the structural adhesive has become brittle at low temperatures and fatigue microcracks have accumulated at the bonding interface. The force applied by the wedge tool can be continuously transmitted and extended along the existing microcracks at the bonding interface, driving the interface cracks to penetrate the entire bonding interface, reducing the mechanical force required to separate the battery cell from the casing. At the same time, the wedge-type force application method can gradually advance along the bonding interface, making the force distribution at the bonding interface more uniform. This helps to reduce the possibility of deformation of the battery cell casing and damage to the internal electrode assembly during the separation process. Combined with the brittle fracture characteristics of the structural adhesive after low-temperature embrittlement, it can reduce the risk of large-area residue of structural adhesive on the surface of the battery cell, improve the appearance integrity of the battery cell after separation, and improve the disassembly and separation efficiency while increasing the integrity rate and cascade utilization value of the battery cell.

[0111] In some embodiments, step S1051 can be performed immediately after the final cooling process in step S104, making full use of the structural adhesive in its optimal low-temperature embrittlement state and avoiding the increase in separation difficulty caused by the recovery of the structural adhesive's toughness after the temperature rises.

[0112] A wedge tool can be inserted at the assembly gap between the cell and the housing and gradually advanced along the extension direction of the bonding interface, so that the force distribution at the bonding interface is more uniform, which helps to further reduce the possibility of cell housing deformation and internal electrode assembly damage during the separation process.

[0113] In some embodiments, the wedge tool has a blunt working surface design at the wedge insertion end, which helps to reduce the risk of scratching the battery cell housing or water-cooling plate surface during the wedge insertion process; the separation operation module can control the wedge insertion speed and the applied force of the wedge tool, and can also combine the real-time signal feedback of the acoustic emission sensor to determine the separation status; when the effective acoustic emission event count is significantly reduced, it can be determined that the bonding interface has been basically separated and the wedge insertion force application operation is terminated.

[0114] Optionally, before performing at least three alternating temperature cycles on the power battery pack as described in step S101, the disassembly method for the power battery pack provided in this application embodiment may further include the following steps: Step S106: Based on the material type of the structural adhesive, retrieve the process parameters for alternating temperature cycling treatment that match the material type from the preset parameter library.

[0115] Step S101, which involves subjecting the power battery pack to at least three alternating temperature cycles, includes: Step S1013: Perform at least three alternating temperature cycles on the power battery pack according to the process parameters.

[0116] The preset parameter library includes process parameters corresponding to at least two material types. Each set of process parameters includes the temperature and duration of the low-temperature holding stage, the temperature and duration of the high-temperature holding stage, and the preset number of cycles for alternating temperature cycling of the power battery pack.

[0117] The types of structural adhesives can include, but are not limited to, polyurethane, epoxy resin, and modified acrylate.

[0118] The preset parameter library refers to a set of parameters that have been pre-calibrated through material performance testing and actual disassembly, and are stored in the control module or the upper-level system of the production line. Each set of process parameters in the preset parameter library corresponds to the optimal value that balances interface damage effect, disassembly efficiency and energy consumption level under a specific material type. It can be directly called and executed, reducing the workload of repeated on-site debugging.

[0119] In some embodiments, the process parameters can be expressed as {T} 低 ,T 高 ,t 保温 ,N}. Where, T 低 Indicates the temperature during the low-temperature holding phase; T 高 The temperature indicated during the high-temperature holding phase; t 保温 This represents the baseline value for insulation duration. The insulation duration for the low-temperature holding phase and the high-temperature holding phase can use the same t value. 保温 The value can also be set independently based on the material properties; N represents the preset number of cycles for alternating temperature cycling treatment.

[0120] In this embodiment, before performing at least three alternating temperature cycles on the power battery pack, the control module can first obtain the material type of the structural adhesive in the power battery pack. Then, based on the material type of the structural adhesive, it retrieves the process parameters for alternating temperature cycling that match the material type from a preset parameter library. In step S1013, the power battery pack is then subjected to at least three alternating temperature cycles according to the process parameters. This solution can adapt to different types of structural adhesives used in different models of power battery packs. Different types of structural adhesives differ in their thermophysical properties, such as coefficient of thermal expansion, glass transition temperature, and low-temperature embrittlement characteristics. By pre-calibrating and storing the process parameters corresponding to different types of structural adhesives, the temperature control range, holding time, and total number of cycles for alternating temperature cycling can be precisely matched to the characteristics of the structural adhesive. This ensures a sufficient accumulation of interface fatigue damage for different types of structural adhesives, reducing the risks of insufficient interface damage and increased disassembly difficulty due to mismatch between process parameters and the material type of the structural adhesive, or excessive temperature control leading to redundant energy consumption and increased processing time.

[0121] Meanwhile, the preset parameter library settings can improve the compatibility of the power battery pack disassembly method with different models of power battery packs, reduce the workload of on-site process debugging when changing products, improve the consistency of disassembly effect of different batches and different types of power battery packs, and take into account disassembly efficiency, disassembly yield and production line adaptability.

[0122] In step S106, the control module can obtain the material type of the structural adhesive used in the power battery pack by reading the product identification code of the power battery pack and matching the material configuration information of the power battery pack, or by manual input. Then, the control module can match the obtained material type with the material type entries in the preset parameter library one by one; after a successful match, it retrieves the process parameters corresponding to that material type.

[0123] In step S1013, the control module can send the process parameters obtained in step S106 to the temperature control module, so that the temperature control module can complete the temperature control logic configuration for a single alternating temperature cycle based on the process parameters. Then, the temperature control module executes the single alternating temperature cycle sequentially according to the configured program: "cooling down to the low-temperature holding temperature, low-temperature holding, heating up to the high-temperature holding temperature, and high-temperature holding." After each alternating temperature cycle is completed, the control module automatically accumulates the number of cycles, and simultaneously monitors the interface damage index through the monitoring module.

[0124] It should be noted that combinations of the different embodiments described above are also within the scope of protection of this application.

[0125] As an example, refer to Figure 7 The flowchart illustrates the steps of a disassembly method for a power battery pack provided in an embodiment of this application. Figure 2 The disassembly method may specifically include the following steps: Step S201: Pre-disassembly processing.

[0126] Specifically, electrical components such as wiring harnesses, BDUs, copper busbars, and battery packs can be removed from the power battery pack, leaving the battery cells and housing assembly intact, and confirming that there is no electrolyte leakage from the battery cells.

[0127] Step S202: Determine the process parameters for alternating temperature cycling treatment.

[0128] Specifically, the control module can, in the same manner as step S106, retrieve the alternating temperature cycling process parameters {T} from the preset parameter library that match the material type of the structural adhesive. 低 ,T 高 ,t 保温 ,N}.

[0129] As an example, the temperature T during the cryogenic holding phase 低T is the temperature during the high-temperature holding phase at -30℃. 高 The temperature is 55℃; the insulation time for each stage is t. 保温 The duration is 30-60 minutes; the preset number of cycles N for alternating temperature cycling is 4-6 times, and the temperature difference between the high-temperature holding stage and the low-temperature holding stage is ΔT=T. 高 -T 低 =85℃.

[0130] Step S203: Perform alternating temperature cycling treatment on the power battery pack and monitor the interface damage index of the bonding interface between the cell and the housing.

[0131] Specifically, for the single alternating temperature cycle processing: First, the control module reduces the temperature of the power battery pack to a first temperature at a cooling rate of not less than 2℃ / min, following the same method as in step S1011, and maintains the temperature at the first temperature for a first duration. Then, the control module increases the temperature of the power battery pack from the first temperature to a second temperature at a heating rate of not less than 3℃ / min, following the same method as in step S1012, and maintains the temperature at the second temperature for a second duration. During this period, the control module monitors the interface damage index of the bonding interface between the battery cell and the casing, following the same method as in step S102.

[0132] Step S204: Determine whether the interface damage index is greater than or equal to the preset threshold.

[0133] Specifically, if the interface damage index is greater than or equal to a preset threshold, the control module executes step S206. If the interface damage index is less than the preset threshold, the control module executes step S205.

[0134] Step S205: Determine whether N alternating temperature cycles have been completed.

[0135] In the case where N alternating temperature cycles have been completed, indicating that the total number of alternating temperature cycles has reached the preset number of cycles, the control module executes step S206. In the case where N alternating temperature cycles have not been completed, indicating that the interface damage index is less than the preset threshold and the total number of alternating temperature cycles performed on the power battery pack has not reached the preset number of cycles, the control module executes step S203 again.

[0136] Step S206: Perform final cooling treatment on the power battery pack.

[0137] Specifically, the control module can reduce the temperature of the power battery pack to the final cooling temperature and maintain it for a third duration; wherein the final cooling temperature is -30℃ and the third duration is 20min~30min, so that the fatigued bonding interface is maintained in a low-temperature embrittlement state, which facilitates subsequent mechanical separation.

[0138] Step S207: Separate the battery cell using a wedge tool.

[0139] Specifically, the control module can follow the same method as in step S1051, after the final cooling process, align the wedge tool with the gap between adjacent cells, tap and wedge it in, so as to separate the cells from the housing and remove them from the housing.

[0140] Step S208: Cell status detection.

[0141] Specifically, the control module can perform visual inspections and basic electrical performance tests on the battery cells to determine whether they are suitable for reuse. These basic electrical performance tests may include, but are not limited to, open-circuit voltage and internal resistance.

[0142] In summary, the disassembly method for the power battery pack provided in this application embodiment, by subjecting the power battery pack to at least three alternating temperature cycles and controlling the temperature difference between the high-temperature holding stage and the low-temperature holding stage during a single alternating temperature cycle to ≥40℃, can induce periodic shear fatigue stress at the bonding interface between the battery cell and the casing, accumulating interface fatigue damage. This weakens the adhesion force at the bonding interface in a shorter time and with lower energy consumption, shortening the disassembly time of the power battery pack, reducing the disassembly energy consumption of the power battery pack, and improving the disassembly efficiency and yield of the power battery pack. During the alternating temperature cycling process, the interface damage index of the bonding interface is monitored. When the interface damage index is greater than or equal to a preset threshold, or when the total number of alternating temperature cycles reaches a preset number of cycles, it indicates that the adhesion force of the bonding interface has decreased to a separable state. The power battery pack can then undergo a final cooling treatment to maintain the fatigued bonding interface in a low-temperature embrittlement state. This, combined with the interface fatigue damage caused by the alternating temperature cycling process, can significantly reduce the peeling force of the bonding interface, reduce the mechanical force required to separate the battery cell from the casing, reduce the damage to the battery cell during disassembly, and improve the integrity rate and cascade utilization value of the battery cell after disassembly.

[0143] Device Examples Reference Figure 2 This application also provides a power battery pack disassembly system 20, which includes a temperature control module 21, a monitoring module 22, and a separation operation module 23; wherein: The temperature control module 21 is used to perform at least three alternating temperature cycles on the power battery pack. Each alternating temperature cycle includes a low temperature holding stage and a high temperature holding stage, and the temperature difference between the high temperature holding stage and the low temperature holding stage is ≥40℃. The power battery pack includes battery cells and a housing, and the battery cells and the housing are bonded together with structural adhesive. The monitoring module 22 is used to monitor the interface damage index of the bonding interface between the battery cell and the housing during the alternating temperature cycle treatment. The temperature control module 21 is also used to perform a final cooling treatment on the power battery pack when the interface damage index is greater than or equal to a preset threshold, or when the total number of alternating temperature cycle treatments reaches a preset number of cycles. The separation operation module 23 is used to apply a separation operation to the battery cell after the final cooling process to separate the battery cell from the housing.

[0144] Optionally, the temperature control module includes: The first temperature control submodule is used to reduce the temperature of the power battery pack to a first temperature for a single alternating temperature cycle and maintain it at the first temperature for a first duration. The first temperature is the temperature of the low temperature holding stage, and the first duration is the duration of the low temperature holding stage. The second temperature control submodule is used to raise the temperature of the power battery pack from the first temperature to the second temperature and maintain it at the second temperature for a second duration. The second temperature is the temperature of the high-temperature holding stage, the second duration is the duration of the high-temperature holding stage, and the difference between the second temperature and the first temperature is ≥40℃.

[0145] Optionally, the cooling rate of the power battery pack to a first temperature is ≥2℃ / min; and / or, The heating rate of the power battery pack from the first temperature to the second temperature is ≥3℃ / min.

[0146] Optionally, the first temperature is -35℃ to -20℃, and the second temperature is 50℃ to 60℃.

[0147] Optionally, the first duration and / or the second duration is 30 min to 60 min.

[0148] Optionally, the power battery pack is subjected to alternating temperature cycling treatment for a total of 4 to 6 times.

[0149] Optionally, the total cumulative duration of alternating temperature cycling treatment on the power battery pack is ≤6 hours.

[0150] Optionally, the temperature difference between the high-temperature holding stage and the low-temperature holding stage is 70°C to 95°C.

[0151] Optionally, an acoustic emission sensor is disposed on the housing near the bonding interface; the monitoring module includes: An acoustic emission sensor is used to collect acoustic emission signals from the adhesive interface during the alternating temperature cycling process. The signal processing unit is used to calculate the interface damage index based on the cumulative count of the acoustic emission signal.

[0152] Optionally, the temperature control module further includes: The third temperature control submodule is used to reduce the temperature of the power battery pack to the temperature of the final cooling process and maintain it for a third duration. The final cooling process is performed at a temperature of -35℃ to -20℃, and the third cooling period is 20 min to 30 min.

[0153] Optionally, the separation operation module includes: The separation operation submodule is used to wedge a wedge tool along the bonding interface and apply force after the final cooling treatment to separate the battery cell from the housing.

[0154] Optionally, the disassembly system for the power battery pack further includes: The control module is used to retrieve process parameters for alternating temperature cycling treatment that match the material type of the structural adhesive from a preset parameter library. The preset parameter library includes process parameters corresponding to at least two material types. The process parameters include the temperature and duration of the low-temperature holding stage, the temperature and duration of the high-temperature holding stage, and the total number of alternating temperature cycling treatments performed on the power battery pack. The temperature control module is also used to perform at least three alternating temperature cycles on the power battery pack according to the process parameters.

[0155] As the apparatus embodiment is basically similar to the method embodiment, it is described in a relatively simple manner. For relevant details, please refer to the description of the method embodiment.

[0156] This application also provides a battery cell that is obtained by disassembling the power battery pack using the disassembly method described in any of the above embodiments.

[0157] The battery cells obtained from the power battery pack disassembly using the above-mentioned disassembly method can achieve complete separation from the casing under relatively low mechanical force during the separation process, thanks to the synergistic effect of fatigue damage accumulation at the bonding interface and low-temperature embrittlement of the structural adhesive. This effectively reduces the probability of appearance defects such as dents, scratches, and deformation on the battery cell casing, and the amount of residual structural adhesive on the battery cell surface is relatively lower, making subsequent surface cleaning processes easier. At the same time, the temperature range throughout the disassembly process is within the safe tolerance range of the battery cell, and will not cause additional thermal shock or cold damage to the core components such as the internal electrode assembly and electrolyte. The electrical performance of the battery cell is not significantly reduced compared to before disassembly, and the residual value of the battery cell is well preserved.

[0158] The battery cells obtained from the power battery pack dismantling method described above can be used in energy storage, low-speed vehicles and other tiered utilization scenarios after performance sorting, or they can be directly entered into the material recycling process for resource utilization. This can adapt to different levels of recycling needs and help improve the resource utilization efficiency of the power battery pack throughout its entire life cycle.

[0159] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to each other.

[0160] Although preferred embodiments of the present application have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments as well as all changes and modifications falling within the scope of the embodiments of the present application.

[0161] Finally, it should be noted that in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or terminal device that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or terminal device.

[0162] The above provides a detailed description of the disassembly method, disassembly system, and battery cells of a power battery pack provided in this application. Specific examples have been used to illustrate the principles and implementation methods of this application. The descriptions of the above embodiments are only for the purpose of helping to understand the method and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.

Claims

1. A method for disassembling a power battery pack, characterized in that, The disassembly method includes: The power battery pack is subjected to at least three alternating temperature cycles. Each alternating temperature cycle includes a low temperature holding stage and a high temperature holding stage, and the temperature difference between the high temperature holding stage and the low temperature holding stage is ≥40℃. The power battery pack includes cells and a housing, and the cells and the housing are bonded together with structural adhesive. During the alternating temperature cycling process, the interface damage index of the bonding interface between the battery cell and the housing is monitored. When the interface damage index is greater than or equal to a preset threshold, or when the total number of alternating temperature cycles reaches a preset number of cycles, the power battery pack is subjected to a final cooling treatment. After the final cooling process, a separation operation is performed on the battery cell to separate the battery cell from the housing.

2. The disassembly method according to claim 1, characterized in that, The process of subjecting the power battery pack to at least three alternating temperature cycles includes: For a single alternating temperature cycle treatment, the temperature of the power battery pack is reduced to a first temperature and maintained at the first temperature for a first duration, where the first temperature is the temperature of the low temperature holding stage and the first duration is the duration of the low temperature holding stage; The temperature of the power battery pack is raised from the first temperature to the second temperature and maintained at the second temperature for a second duration. The second temperature is the temperature of the high-temperature holding stage, the second duration is the duration of the high-temperature holding stage, and the difference between the second temperature and the first temperature is ≥40℃.

3. The disassembly method according to claim 2, characterized in that, The cooling rate of the power battery pack to a first temperature is ≥2℃ / min; and / or, The heating rate of the power battery pack from the first temperature to the second temperature is ≥3℃ / min.

4. The disassembly method according to claim 2 or 3, characterized in that, The first temperature is -35℃ to -20℃, and the second temperature is 50℃ to 60℃.

5. The disassembly method according to any one of claims 2 to 4, characterized in that, The first duration and / or the second duration is 30 min to 60 min.

6. The disassembly method according to any one of claims 1 to 5, characterized in that, The power battery pack is subjected to alternating temperature cycling treatment for a total of 4 to 6 times.

7. The disassembly method according to any one of claims 1 to 6, characterized in that, The total cumulative time for alternating temperature cycling treatment of the power battery pack is ≤6 hours.

8. The disassembly method according to any one of claims 1 to 7, characterized in that, The temperature difference between the high-temperature holding stage and the low-temperature holding stage is 70℃~95℃.

9. The disassembly method according to any one of claims 1 to 8, characterized in that, An acoustic emission sensor is provided on the housing near the bonding interface; During the alternating temperature cycling process, monitoring the interface damage index at the bonding interface between the battery cell and the housing includes: During the alternating temperature cycling process, the acoustic emission signal of the bonding interface is collected by the acoustic emission sensor; The interface damage index is calculated based on the cumulative count of the acoustic emission signals.

10. The disassembly method according to any one of claims 1 to 9, characterized in that, The final cooling process for the power battery pack includes: The temperature of the power battery pack is reduced to the temperature of the final cooling treatment and maintained for a third duration; The final cooling process is performed at a temperature of -35℃ to -20℃, and the third cooling period is 20 min to 30 min.

11. The disassembly method according to any one of claims 1 to 10, characterized in that, The step of performing a separation operation on the battery cell after the final cooling treatment to separate the battery cell from the housing includes: After the final cooling process, a wedge tool is inserted along the bonding interface and a force is applied to separate the battery cell from the housing.

12. The disassembly method according to any one of claims 1 to 11, characterized in that, Before subjecting the power battery pack to at least three alternating temperature cycles, the disassembly method further includes: Based on the material type of the structural adhesive, process parameters for alternating temperature cycling treatment that match the material type are retrieved from a preset parameter library; wherein, the preset parameter library includes process parameters corresponding to at least two material types, and the process parameters include the temperature and duration of the low-temperature holding stage, the temperature and duration of the high-temperature holding stage, and the total number of alternating temperature cycling treatments performed on the power battery pack; The process of subjecting the power battery pack to at least three alternating temperature cycles includes: The power battery pack is subjected to at least three alternating temperature cycles according to the process parameters.

13. A disassembly system for a power battery pack, characterized in that, The disassembly system includes a temperature control module, a monitoring module, and a separation operation module; wherein: The temperature control module is used to perform at least three alternating temperature cycles on the power battery pack. Each alternating temperature cycle includes a low temperature holding stage and a high temperature holding stage, and the temperature difference between the high temperature holding stage and the low temperature holding stage is ≥40℃. The power battery pack includes battery cells and a housing, and the battery cells and the housing are bonded together with structural adhesive. The monitoring module is used to monitor the interface damage index of the bonding interface between the battery cell and the housing during the alternating temperature cycle treatment. The temperature control module is also used to perform a final cooling treatment on the power battery pack when the interface damage index is greater than or equal to a preset threshold, or when the total number of alternating temperature cycles reaches a preset number of cycles. The separation operation module is used to apply a separation operation to the battery cell after the final cooling process to separate the battery cell from the housing.

14. A battery cell, characterized in that, It is obtained by disassembling the power battery pack using the disassembly method described in any one of claims 1 to 12.