A casting method applicable to brake caliper bodies of various passenger vehicles

By combining the design of the mold base and the product forming insert with a standardized gating system, and by combining spheroidizing and inoculation treatment, the problems of high mold development cost, long R&D cycle, low production efficiency and poor quality consistency caused by structural differences in multiple passenger vehicle brake caliper bodies have been solved, and efficient and stable casting of multiple brake caliper bodies has been achieved.

CN123102941APending Publication Date: 2026-11-17SHAOGUAN JINBAO FOUNDRY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611036909.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing technology for brake calipers for various passenger vehicles suffers from high mold development costs, long R&D cycles, low production efficiency, and poor quality consistency due to significant structural differences.

Method used

By adopting a mold base and multiple sets of product molding inserts, and through a standardized gating system and split insert design, combined with spheroidizing and inoculation treatments, it is possible to achieve rapid switching and quality stability of multiple brake caliper bodies on the same production platform.

Benefits of technology

This significantly reduced mold development costs, shortened the R&D cycle, improved production efficiency, and ensured the consistency of casting quality and the stability of metallographic structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102941A_ABST
    Figure CN123102941A_ABST
Patent Text Reader

Abstract

This invention discloses a casting method applicable to brake caliper bodies of various passenger vehicles, including providing a mold base and a molding insert assembly. The mold base is equipped with a standardized gating system and mounting positions. The molding insert assembly includes multiple sets of product molding inserts, each set of which has an external shape adapted to the mounting position and an internal cavity matching the external shape of different brake caliper bodies. The method involves selecting the corresponding product molding insert based on the desired brake caliper model and installing it on the mold base to form a casting cavity; performing spheroidizing treatment on molten iron; after the spheroidizing reaction, adding a first inoculant to the molten iron for in-lamb inoculation treatment; pouring the spheroidized and in-lamb inoculated molten iron into the casting cavity, and adding a second inoculant to the molten iron flow during the pouring process for in-flow inoculation treatment; cooling the casting in a sand mold after pouring, removing the casting blank after cooling; and cleaning, shot blasting, and removing the gate and flash from the casting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of automotive parts casting technology, and in particular to a casting method applicable to brake caliper bodies of various passenger vehicles. Background Technology

[0002] Brake caliper bodies are the core safety components of automotive disc brake systems. During braking, they withstand enormous impact loads and alternating stresses, placing extremely stringent requirements on the strength, toughness, and fatigue resistance of the castings. Currently, ductile iron, due to its excellent comprehensive mechanical properties and good casting processability, has become the primary casting material for brake caliper bodies.

[0003] With the rapid development of the new energy vehicle industry and the continuous upgrading and iteration of traditional fuel passenger vehicles, passenger vehicle production and sales have steadily increased, leading to a continuous rise in market demand for brake caliper bodies. At the same time, brake caliper bodies from different brands and models exhibit significant structural differences. Floating calipers and fixed calipers have distinct structures, with key dimensions such as cylinder wall thickness, flange angle, and mounting hole positions varying depending on the vehicle model. This structural difference presents technical challenges to the casting production of brake calipers, including high mold development costs, long development cycles, low production efficiency, high changeover costs, and difficulty in ensuring consistent casting quality.

[0004] To address the aforementioned issues, some improvements have been proposed in the existing technology. For example, Chinese patent CN105745042B discloses a casting method for manufacturing brake calipers. This method constructs flange faces with different angles by setting independent removable molding parts in the mold, thereby enabling the manufacture of brake calipers with different flange face configurations using the same mold. However, this solution only addresses the differentiation of local flange face structures; it still cannot achieve universal manufacturing for differences in the overall caliper body structure. Similarly, Chinese patent CN114458707A discloses an automotive disc brake caliper body and its design method, achieving rapid matching of caliper body structures through a modular design approach. However, its technical solution focuses on the product design stage and does not address universal solutions at the casting process level. Furthermore, Chinese patent CN117428168B discloses a casting mold for an automotive brake caliper body bracket and its processing method. However, its mold structure is complex, primarily addressing demolding efficiency rather than the issue of universality across multiple product types. Summary of the Invention

[0005] This invention provides a casting method applicable to brake caliper bodies of various passenger vehicles, which can solve the technical problems in the prior art that lead to high mold development costs, long R&D cycles, low production efficiency, and poor quality consistency due to large structural differences in brake caliper bodies of various passenger vehicles.

[0006] A casting method applicable to brake caliper bodies of multiple passenger vehicles includes the following steps: S1, providing a mold base and a forming insert assembly. The mold base is equipped with a standardized gating system and mounting positions. The forming insert assembly includes multiple sets of product forming inserts, the shape of each set of product forming inserts being adapted to the mounting positions, and the inner cavity matching the shape of different brake caliper bodies; S2, selecting the corresponding product forming insert according to the required brake caliper body model and installing it on the mold base to form a casting cavity; S3, balling the molten iron. S4. After the spheroidizing reaction is completed, the first inoculant is added to the molten iron for in-lamb inoculation treatment; S5. The molten iron after spheroidizing and in-lamb inoculation treatment is poured into the casting cavity, and the second inoculant is added to the molten iron flow during the pouring process for in-flow inoculation treatment; S6. After pouring, the casting is cooled in the sand mold, and after cooling, the mold is opened and the sand is removed to take out the casting blank; S7. The casting is cleaned, shot blasted, the gate and flash are removed, and the metallographic structure and mechanical properties of the casting are tested.

[0007] The present invention provides a casting method for brake caliper bodies applicable to various passenger vehicles, which, compared with the prior art, has, but is not limited to, the following beneficial effects: This casting method, applicable to brake calipers for various passenger vehicles, utilizes a mold base and multiple sets of product forming inserts. This allows different brake caliper structures to share the same mold base and standardized gating system simply by replacing the forming inserts that are compatible with the mounting position and whose inner cavities match the corresponding caliper shape. This significantly reduces mold development costs and shortens the R&D cycle. By installing the corresponding product forming inserts onto the mold base according to the required production model, a casting cavity is formed, enabling rapid switching between multiple caliper models on the same production platform. This effectively reduces mold changeover time and production line downtime losses, significantly improving production efficiency. Through the synergistic combination of spheroidizing treatment and in-lamb inoculation treatment, the molten iron achieves a good graphite spheroidization foundation before pouring. Furthermore, by adding a second inoculant during the pouring process for in-flow inoculation treatment, inoculation decline is effectively prevented. This systematically solves the technical problems of high mold development costs, long R&D cycles, low production efficiency, and poor quality consistency caused by significant structural differences in brake calipers for various passenger vehicles in existing technologies.

[0008] Furthermore, in step S1, the product forming insert is a split insert, including multiple sub-inserts corresponding to the hydraulic cylinder part, the bridge part, and the mounting ear part of the clamp body, respectively. Each sub-insert is detachably installed on the mounting position, and the corresponding sub-inserts of different clamp body models can be interchanged and combined.

[0009] Furthermore, in step S1, a positioning pin and a locking mechanism are provided between the mold base and the product molding insert to achieve rapid positioning and locking of the product molding insert. The mold base is provided with a coding mark to record the installation position and process parameters corresponding to different product molding inserts.

[0010] Further, in step S1, the standardized gating system includes a gating cup, a sprue, a runner, and multiple risers disposed above the cavity of each product molding insert; the runner and each riser are connected by an ingate, and the cross-sectional area of ​​the ingate is determined proportionally according to the cavity volume of each product molding insert.

[0011] Furthermore, prior to step S3, low-sulfur scrap steel, stamping offcuts, and recycled materials are selected as furnace charge, and are batched and smelted with low-sulfur carbon raiser and silicon carbide to adjust the chemical composition of the molten iron so that the carbon content is 3.5%–4.0%, the silicon content is 2.0%–3.2%, the manganese content is ≤0.45%, the phosphorus content is ≤0.07%, the sulfur content is ≤0.035%, the rare earth residue is ≤0.03%, and the magnesium content is 0.025%–0.060%.

[0012] Further, in step S3, the spheroidizing treatment adopts the sludge-filling method or the pouring method, the amount of spheroidizing agent added is 1.0% to 1.6% of the mass of molten iron, the spheroidizing treatment temperature is controlled at 1480℃ to 1520℃, and the spheroidizing agent is a low rare earth magnesium silicon iron alloy.

[0013] Further, in step S4, the first inoculant is a barium silicon inoculant containing 1% to 4% Ba, with a particle size of 3 to 8 mm, and the amount added is 0.3% to 0.5% of the mass of molten iron.

[0014] Further, in step S5, the second inoculant is a silicon-strontium inoculant containing 0.5% to 1.5% Sr, with a particle size of 0.2 to 0.8 mm, and the amount added is 0.1% to 0.2% of the mass of molten iron.

[0015] Furthermore, in step S5, the pouring temperature is controlled at 1360℃~1420℃. Before pouring, casting simulation software is used to numerically simulate the filling and solidification process of molten iron. Based on the simulation results, the combination of process parameters such as pouring temperature, pouring speed and cooling time is optimized.

[0016] Furthermore, in step S6, the cooling time is determined based on the casting wall thickness. The relationship between the cooling time t and the maximum casting wall thickness δ is: t = k × δ, where k is the cooling coefficient, and the value of k ranges from 1.0 to 1.5 min / mm. Attached Figure Description

[0017] Figure 1 A flowchart illustrating a method for casting brake caliper bodies applicable to various passenger vehicles according to one embodiment of the present invention. Detailed Implementation

[0018] To make the objectives, technical solutions, and advantages of this application clearer, specific embodiments of this application are described clearly and completely below with reference to the accompanying drawings. It should be understood that the described embodiments are only a part of the embodiments of this application, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments described in this application without creative effort will fall within the scope of protection of this application.

[0019] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used in the specification of this application is for the purpose of describing specific embodiments only and is not intended to limit this application; the terms "comprising," "including," "having," "containing," "comprise," etc., in the specification, claims, and accompanying drawings of this application are open-ended terms, indicating that a method comprises one or more steps, or an apparatus comprises one or more elements, but do not exclude the inclusion of other steps or elements. The terms "first," "second," etc., in the specification, claims, or accompanying drawings of this application are used to distinguish different objects, not to describe a specific order or primary / secondary relationship. Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined with "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this application, unless otherwise stated, "a plurality of" means two or more.

[0020] In the description of this application, it should be understood that the terms "upper," "lower," "left," "right," "front," "rear," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation on this application. It should also be noted that...

[0021] In the description of this application, it should be noted that, unless otherwise expressly specified and limited, the terms "installation," "connection," "linking," and "attachment" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal communication between two components. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.

[0022] In this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. Additionally, in this application, the character " / " generally indicates that the preceding and following related objects have an "or" relationship.

[0023] like Figure 1 As shown in the figure, an embodiment of the present invention provides a casting method applicable to brake caliper bodies of various passenger vehicles, including the following steps: S1, providing a mold base and a molding insert assembly, the mold base being provided with a standardized gating system and mounting positions, the molding insert assembly including multiple sets of product molding inserts, the shape of each set of product molding inserts being adapted to the mounting positions, and the inner cavity matching the shape of different brake caliper bodies; S2, selecting the corresponding product molding insert according to the required brake caliper body model and installing it on the mold base to form a casting cavity; S3, S4. After the spheroidization reaction, the first inoculant is added to the molten iron for in-lamb inoculation treatment; S5. The molten iron after spheroidization and in-lamb inoculation treatment is poured into the casting cavity, and a second inoculant is added to the molten iron flow during the pouring process for in-flow inoculation treatment; S6. After pouring, the casting is cooled in the sand mold, and after cooling, the mold is opened and the sand is removed to take out the casting blank; S7. The casting is cleaned, shot blasted, and the gate and flash are removed. The metallographic structure and mechanical properties of the casting are then tested.

[0024] In this embodiment, by setting up a mold base and multiple sets of product forming inserts, different brake caliper bodies only need to have their forming inserts adapted to the mounting position and whose inner cavities match the corresponding caliper body shape to share the same mold base and standardized gating system, significantly reducing mold development costs and shortening the R&D cycle; by installing the corresponding product forming inserts on the mold base according to the required production model, a casting cavity is formed, realizing rapid switching of multiple caliper bodies on the same production platform, effectively reducing mold change time and production line downtime losses, and significantly improving production efficiency; through the synergistic combination of spheroidizing treatment and ladle inoculation treatment, the molten iron obtains good conditions before pouring. Based on the graphite spheroidization foundation, a second inoculant is added during the pouring process for in-flow inoculation treatment, which effectively prevents inoculation decline and ensures that different clamp bodies can obtain a consistent spheroidization effect under their respective solidification conditions. This avoids fluctuations in metallographic structure and mechanical properties caused by differences in wall thickness. Cooling, unpacking, cleaning, shot blasting, removal of gates and flash, and metallographic and mechanical property testing further ensure the quality stability of each clamp body casting. This systematically solves the technical problems of high mold development costs, long R&D cycles, low production efficiency, and poor quality consistency caused by large structural differences in multiple passenger car brake clamp bodies in the existing technology.

[0025] Furthermore, in step S1, the product forming insert is a split insert, including multiple sub-inserts corresponding to the hydraulic cylinder part, the bridge part, and the mounting ear part of the clamp body, respectively. Each sub-insert is detachably installed on the mounting position, and the corresponding sub-inserts of different clamp body models can be interchanged and combined.

[0026] In this embodiment, the product molding insert is set as a split insert, which is composed of multiple sub-inserts corresponding to the clamp body cylinder part, clamp body bridge part, and clamp body mounting ear part. Each sub-insert is detachably installed on the mounting position of the mold base. This allows for rapid transformation between different models of clamp bodies by interchangeably combining the corresponding sub-inserts. Since each sub-insert only needs to be processed independently for a local structure of the clamp body, the volume and processing difficulty of a single sub-insert are much smaller than those of an integral insert, which greatly reduces the mold processing cost and manufacturing cycle. At the same time, when the structure of a certain part changes, only the corresponding sub-insert needs to be replaced without scrapping the entire set of inserts, which effectively reduces the mold rework and repair costs and material waste. Furthermore, by arranging and combining different sub-inserts, a variety of clamp body cavities with different structures can be derived on the same mold base, further shortening the mold preparation time and product development cycle of new clamp bodies, and significantly improving the mold change efficiency and equipment utilization rate under the production conditions of multiple types of brake clamp bodies.

[0027] Furthermore, in step S1, a positioning pin and a locking mechanism are provided between the mold base and the product molding insert to achieve rapid positioning and locking of the product molding insert. The mold base is provided with a coding mark to record the installation position and process parameters corresponding to different product molding inserts.

[0028] In this embodiment, by setting positioning pins and locking mechanisms between the mold base and the product forming inserts, when different models of product forming inserts are replaced, the positioning pins ensure that each sub-insert is quickly and accurately aligned in its installation position, avoiding cavity misalignment or dimensional deviations caused by installation deviations. The locking mechanism firmly fixes the inserts to the mold base, effectively preventing the inserts from shifting or loosening due to the impact of molten iron during the pouring process. This ensures both the rapid switching between multiple product types and the dimensional accuracy and cavity integrity of the castings. At the same time, the coded markings on the mold base record the installation positions and process parameters corresponding to different product forming inserts. This allows operators to directly retrieve key parameters such as pouring temperature and cooling time based on the coded markings when replacing inserts, eliminating the need for repeated adjustments and trial and error. This significantly shortens the process parameter setting time after mold change, reduces the risk of process deviations caused by human memory errors, improves the process repeatability and quality consistency during the alternating production of multiple product types, further shortens the product development cycle, and reduces rework and maintenance costs.

[0029] Furthermore, in step S1, the standardized gating system includes a gating cup, a sprue, a runner, and multiple risers disposed above the cavities of each product molding insert; the runner and each riser are connected by an ingate, and the cross-sectional area of ​​the ingate is determined proportionally according to the cavity volume of each product molding insert.

[0030] In this embodiment, by setting the standardized gating system to include a pouring cup, sprue, runner, and multiple risers located above the cavities of each product's molding insert, different models of brake caliper castings can share the same set of pouring cup, sprue, and runner. During pouring, molten iron enters the sprue through the pouring cup and then flows to the runner, before entering the cavities of each product's molding insert and the risers above them through the ingates. Because different product molding inserts share the same standardized gating system, the redundant development costs and long design cycles caused by designing a separate gating system for each caliper body are avoided, significantly reducing mold development costs and shortening the product lifecycle. The development cycle is shortened. Meanwhile, the horizontal runner and each riser are connected by an ingate, and the cross-sectional area of ​​the ingate is determined proportionally according to the cavity volume of each product's molding insert. This ensures that when switching between different models of clamps, the molten iron can be filled smoothly at the corresponding flow rate and speed according to the actual feeding requirements of each cavity. This ensures that each cavity achieves a balanced filling effect and sequential solidification under the same pouring conditions, effectively avoiding casting defects such as local shrinkage cavities, shrinkage porosity, cold shuts, and insufficient pouring caused by differences in the structure of different clamps. Thus, while enabling multiple clamps to share the same pouring system for integrated production, the stability and consistency of the internal quality of each clamp casting are guaranteed.

[0031] Furthermore, prior to step S3, low-sulfur scrap steel, stamping offcuts, and recycled materials are selected as furnace charge, and are batched and smelted with low-sulfur carbon raiser and silicon carbide to adjust the chemical composition of the molten iron so that the carbon content is 3.5%–4.0%, the silicon content is 2.0%–3.2%, the manganese content is ≤0.45%, the phosphorus content is ≤0.07%, the sulfur content is ≤0.035%, the rare earth residue is ≤0.03%, and the magnesium content is 0.025%–0.060%.

[0032] In this embodiment, low-sulfur scrap steel, stamping offcuts, and recycled materials are selected as furnace charge, and low-sulfur recarburizing agent and silicon carbide are used for batching and smelting. The low-sulfur scrap steel and low-sulfur recarburizing agent control the amount of sulfur introduced from the source, providing low-sulfur mother liquor conditions for subsequent spheroidizing treatment. This effectively reduces the consumption of magnesium in the spheroidizing agent by reacting with sulfur to form magnesium sulfide slag, keeping the magnesium content stably controlled within the range of 0.025% to 0.060%, ensuring the full progress of the spheroidizing reaction and the stable achievement of the spheroidization rate. The addition of silicon carbide not only increases silicon and carbon content, but also forms a large number of dispersed fine silicon carbide particles during smelting, which serve as core particles for graphite crystallization, significantly increasing the heterogeneous nucleation ability of molten iron and improving the number and roundness of graphite spheres. The carbon content is controlled at 3.5%. With a carbon content of 2.0% to 4.0% and a silicon content of 2.0% to 3.2%, the carbon equivalent of the molten iron is kept near the eutectic point, ensuring good fluidity and feeding ability. This effectively reduces the risk of cold shuts at thin-walled sections and the tendency for shrinkage porosity at thick sections. A manganese content of ≤0.45% avoids the segregation and aggregation of manganese elements at grain boundaries. A phosphorus content of ≤0.07% reduces the formation of brittle phosphorus eutectic. A sulfur content of ≤0.035% reduces the burden of spheroidizing treatment. A rare earth residue of ≤0.03% ensures the amount of rare earth required to neutralize anti-spheroidizing elements and avoids excessive rare earth increasing the tendency of molten iron to overcool, which could lead to white iron at thin-walled sections. Thus, by controlling the chemical composition from the source, it is possible to comprehensively ensure that brake caliper castings with different structures can obtain stable and uniform metallographic structure and mechanical properties under the same casting process conditions.

[0033] Furthermore, in step S3, the spheroidizing treatment adopts the sludge-filling method or the pouring method, the amount of spheroidizing agent added is 1.0% to 1.6% of the mass of molten iron, the spheroidizing treatment temperature is controlled at 1480℃ to 1520℃, and the spheroidizing agent is a low rare earth magnesium silicon iron alloy.

[0034] In this embodiment, the covered ladle method reduces the volatilization and burn-off of magnesium vapor during the spheroidizing reaction by adding a sealed device over the ladle. The flushing method uses the impact force of the molten iron flow to press the spheroidizing agent into the bottom of the ladle for a full reaction. Both methods can effectively improve the absorption rate of magnesium, allowing the magnesium and rare earth elements in the low rare earth magnesium-silicon ferroalloy to fully act on the molten iron and achieve a good spheroidizing effect. The spheroidizing agent is a low rare earth magnesium-silicon ferroalloy with a moderate rare earth content. It can effectively neutralize the interference of anti-spheroidizing elements such as titanium, lead, and antimony in the molten iron on graphite spheroidization and avoid graphite distortion. It will not increase the tendency of the molten iron to overcool due to excessive rare earth, and prevent the appearance of white iron or excessive cementite content in the thin-walled brake caliper body.

[0035] Specifically, the amount of spheroidizing agent added is controlled at 1.0% to 1.6% of the molten iron mass. This range fully considers the fluctuation of sulfur content in the molten iron and the loss of magnesium during the spheroidizing reaction, ensuring that the residual magnesium content in the molten iron after spheroidizing treatment is stable within the effective range of 0.025% to 0.060%. This ensures that the graphite is fully spheroidized, while avoiding the increase of graphite spheroid irregularities or shrinkage defects due to excessive residual magnesium.

[0036] The spheroidizing treatment temperature is controlled between 1480℃ and 1520℃. Within this temperature range, the magnesium alloy spheroidizing agent can melt rapidly and react fully. If the temperature is below 1480℃, the spheroidizing agent will not melt sufficiently, which will easily lead to poor spheroidization. If the temperature is above 1520℃, the magnesium vapor loss will be aggravated and the molten iron will be severely oxidized. Precisely controlling the temperature within this range ensures the stable progress of the spheroidizing reaction and the consistency of the spheroidizing effect. This allows brake calipers with different structural wall thicknesses to obtain excellent graphite morphology with a spheroidization rate of more than 80% and a spheroidization level of 1 to 4 after subsequent casting. This provides a key guarantee for achieving stable and reliable metallographic structure and mechanical properties for multiple caliper bodies under the same casting process conditions.

[0037] Further, in step S4, the first inoculant is a barium silicon inoculant containing 1% to 4% Ba, with a particle size of 3 to 8 mm, and the amount added is 0.3% to 0.5% of the mass of molten iron.

[0038] In this embodiment, a barium silicate inoculant containing 1% to 4% Ba is used as the first inoculant for inoculation treatment in the ladle. The barium element has the effect of significantly extending the effective inoculation time. It forms a stable high-melting-point compound in the molten iron, which can serve as a persistent nucleation substrate for graphite crystals. This makes the graphite nuclei generated by inoculation less prone to decay during the heat preservation and transportation of molten iron. It effectively suppresses the inoculation decay phenomenon caused by long pouring waiting time or differences in the treatment time of different batches of molten iron, ensuring that the molten iron from the first ladle to the last ladle has sufficient graphite nucleation capacity during pouring.

[0039] Specifically, the inoculant particle size is controlled between 3 and 8 mm. This particle size range ensures that the inoculant can slowly and uniformly dissolve in the molten iron after being added to the ladle, preventing premature depletion of the inoculant due to excessively fine particles, thus avoiding loss of inoculation effect. It also prevents insufficient dissolution and inclusion defects caused by excessively coarse particles. The amount of inoculant added is controlled between 0.3% and 0.5% of the molten iron mass. This amount provides sufficient silicon to promote graphitization and also provides a sufficient quantity of inoculant. The core is composed of fine graphite spheres. At the same time, due to the moderate amount added, the shrinkage porosity or graphite distortion caused by excessive inoculation is avoided. This ensures that the molten iron after inoculation in the ladle has a good graphite nucleation foundation before entering the casting process. This ensures that the brake caliper bodies with different wall thicknesses that are subsequently cast can obtain a dense and uniform distribution of graphite spheres. This provides an inoculation guarantee for the final casting to have a spheroidization rate of more than 80%, a graphite size of 5 to 7, and a pearlite content of no more than 75%.

[0040] Further, in step S5, the second inoculant is a silicon-strontium inoculant containing 0.5% to 1.5% Sr, with a particle size of 0.2 to 0.8 mm, and the amount added is 0.1% to 0.2% of the mass of molten iron.

[0041] In this embodiment, a silicon-strontium inoculant containing 0.5% to 1.5% Sr is used as the second inoculant for in-flow inoculation treatment. Strontium has a strong effect on refining graphite and significantly inhibiting the tendency of white iron. During the solidification process of molten iron, it can provide a large number of highly active nucleation particles, promote the precipitation and growth of graphite on uniform and fine cores, and effectively inhibit the tendency of thin-walled parts to generate carbides or cementite due to rapid cooling. In-flow inoculation is added simultaneously when molten iron is poured from the ladle into the casting cavity. At this time, the molten iron enters the cavity and begins to solidify almost immediately after contacting the inoculant. The inoculant particle size is as fine as 0.2 to 0.8 mm. It can quickly and completely melt and release a large number of nucleation cores in the molten iron flow, so that the inoculation treatment is completed at the last moment before the molten iron is about to solidify. This effectively avoids the problem of inoculation decline caused by long-term placement or transportation of molten iron after traditional ladle inoculation, and ensures that each batch of molten iron maintains the best nucleation activity state at the moment of entering the cavity.

[0042] Specifically, the amount of inoculant added is controlled at 0.1% to 0.2% of the molten iron mass. This proportion can provide sufficient nucleation cores to refine graphite spheres and optimize the matrix structure. At the same time, the small amount of inoculant avoids the negative effects of graphite floating or grain boundary segregation caused by excessive strontium in the inoculant. In addition, it is combined with the 0.3% to 0.5% inoculation amount in step S4 to form a total secondary inoculation amount of 0.4% to 0.7%. This fully leverages the synergistic advantages of the long-term anti-fading effect of barium silicon inoculant and the instantaneous strong refining effect of strontium silicon inoculant. It also enables brake caliper bodies with different wall thicknesses to obtain a fine, round, and uniformly distributed microstructure of graphite spheres under their respective solidification conditions.

[0043] Furthermore, in step S5, the pouring temperature is controlled at 1360℃~1420℃. Before pouring, casting simulation software is used to numerically simulate the filling and solidification process of molten iron. Based on the simulation results, the combination of process parameters such as pouring temperature, pouring speed and cooling time is optimized.

[0044] In this embodiment, by controlling the pouring temperature between 1360℃ and 1420℃, the molten iron has suitable fluidity and filling capacity within this temperature range. When the temperature is below 1360℃, the molten iron has insufficient fluidity, which can easily lead to cold shuts or incomplete pouring defects in the thin-walled brake caliper body. When the temperature is above 1420℃, the molten iron is overheated, which not only aggravates the burning loss and inoculation degradation of magnesium, but also increases the solidification shrinkage and porosity of the casting. By precisely limiting the pouring temperature within this range, it is ensured that brake caliper bodies with different wall thicknesses can obtain a complete and continuous cavity filling effect during the filling process. At the same time, it reduces the quality variation caused by temperature fluctuations and realizes stable production of multiple caliper bodies under the same pouring temperature window.

[0045] Specifically, before casting, casting simulation software is used to numerically simulate the filling and solidification process of molten iron. The simulation software can predict the flow front morphology, filling sequence, temperature field distribution, and solidification shrinkage law of molten iron in the cavity in advance based on the three-dimensional model of the cavity corresponding to the specific product molding insert selected in step S1. Based on the simulation results, the operator can optimize the combination configuration of process parameters such as pouring temperature, pouring speed, and cooling time in a differentiated manner according to the differences in wall thickness and heat distribution characteristics of different clamp bodies. When switching between different clamp body models, there is no need to explore the process conditions through repeated trial and error and physical trial casting. Instead, the parameters can be adjusted directly based on the simulation data, which greatly reduces the number of trial productions and material waste in the new product development process and shortens the product development cycle.

[0046] Among these methods, high-risk areas for potential defects such as shrinkage cavities, porosity, and air entrapment are identified in advance through numerical simulation. These areas are then eliminated during the simulation phase by adjusting the combination of process parameters. This ensures that the molten iron flows smoothly and without turbulence or air entrapment during the filling process. During solidification, the solidification proceeds sequentially from thin-walled areas to thick-walled areas or from areas far from the riser to areas close to the riser. This allows for the mass production of multiple brake caliper bodies with different structures using the same gating system, while also preventing casting defects such as shrinkage cavities, porosity, cold shuts, and air holes from the source, significantly reducing the scrap rate.

[0047] Furthermore, in step S6, the cooling time is determined based on the casting wall thickness. The relationship between the cooling time t and the maximum casting wall thickness δ is: t = k × δ, where k is the cooling coefficient, and the value of k ranges from 1.0 to 1.5 min / mm.

[0048] In this embodiment, the maximum wall thickness δ varies for different brake caliper bodies corresponding to different product molding inserts. Using this relationship, the differentiated cooling time applicable to each caliper body structure can be quantitatively calculated. For those with larger wall thicknesses, the heat preservation time in the cavity is longer to avoid coarse grains and graphite spheroidization due to slow cooling. For those with smaller wall thicknesses, the cooling time is correspondingly shortened to prevent the formation of white iron or cementite due to excessive cooling. This ensures that caliper bodies of any structure can obtain a fine and uniform metallographic structure under their respective optimized cooling conditions. Since the calculation of cooling time only depends on the maximum wall thickness δ of the casting, which can be directly obtained from the cavity size of the product molding insert, when switching between different models of product molding inserts in step S2, the operator only needs to measure or read the maximum wall thickness value corresponding to that model and substitute it into the relationship to quickly determine the cooling time. There is no need to conduct a large number of cooling process experiments for each new caliper body to explore the optimal cooling parameters, which greatly shortens the process debugging cycle when introducing new products and reduces the consumption of test materials and labor costs.

[0049] The above-disclosed embodiments are merely a few specific examples of the present invention. However, the embodiments of the present invention are not limited thereto, and any variations that can be conceived by those skilled in the art should fall within the protection scope of the present invention.

Claims

1. A casting method applicable to brake caliper bodies of various passenger vehicles, characterized in that, Includes the following steps: S1. Provide a mold base and molding insert assembly. The mold base is equipped with a standardized gating system and mounting positions. The molding insert assembly includes multiple sets of product molding inserts. The shape of each set of product molding inserts is adapted to the mounting position, and the inner cavity is matched with the shape of different brake caliper bodies. S2. Select the corresponding product molding insert according to the required brake caliper model and install it on the mold base to form a casting cavity; S3. Spheroidizing treatment of molten iron; S4. After the spheroidizing reaction is completed, the first inoculant is added to the molten iron for in-lamb inoculation treatment; S5. Pour the molten iron that has undergone spheroidizing treatment and in-lamb inoculation treatment into the casting cavity, and add a second inoculant to the molten iron flow during the pouring process for in-flow inoculation treatment. S6. After pouring, the casting is cooled in the sand mold. After cooling, the mold is opened, the sand is removed, and the casting blank is taken out. S7. Clean the casting, shot blast it, remove the gate and flash, and test the metallographic structure and mechanical properties of the casting.

2. The casting method for brake caliper bodies of various passenger vehicles as described in claim 1, characterized in that, In step S1, the product forming insert is a split insert, including multiple sub-inserts corresponding to the hydraulic cylinder part, the bridge part, and the mounting ear part of the clamp body, respectively. Each sub-insert is detachably installed on the mounting position, and the corresponding sub-inserts of different clamp body models can be interchanged and combined.

3. The casting method for brake caliper bodies applicable to various passenger vehicles as described in claim 1, characterized in that, In step S1, a positioning pin and a locking mechanism are provided between the mold base and the product molding insert to achieve rapid positioning and locking of the product molding insert. The mold base is provided with a coding mark to record the installation position and process parameters corresponding to different product molding inserts.

4. The casting method for brake caliper bodies of various passenger vehicles as described in claim 1, characterized in that, In step S1, the standardized gating system includes a gating cup, a sprue, a runner, and multiple risers disposed above the cavities of each product molding insert; the runner and each riser are connected by an ingate, and the cross-sectional area of ​​the ingate is determined proportionally according to the cavity volume of each product molding insert.

5. The casting method for brake caliper bodies of various passenger vehicles as described in claim 1, characterized in that, Before step S3, low-sulfur scrap steel, stamping offcuts, and recycled materials are selected as furnace charge, and are batched and smelted with low-sulfur carbon raiser and silicon carbide. The chemical composition of the molten iron is adjusted so that the carbon content is 3.5% to 4.0%, the silicon content is 2.0% to 3.2%, the manganese content is ≤0.45%, the phosphorus content is ≤0.07%, the sulfur content is ≤0.035%, the rare earth residue is ≤0.03%, and the magnesium content is 0.025% to 0.060%.

6. The casting method for brake caliper bodies of various passenger vehicles as described in claim 1, characterized in that, In step S3, the spheroidizing treatment is performed using the slough method or the pouring method. The amount of spheroidizing agent added is 1.0% to 1.6% of the mass of molten iron. The spheroidizing treatment temperature is controlled at 1480℃ to 1520℃. The spheroidizing agent is a low rare earth magnesium silicon iron alloy.

7. The casting method for brake caliper bodies of various passenger vehicles as described in claim 1, characterized in that, In step S4, the first inoculant is a barium silicon inoculant containing 1% to 4% Ba, with a particle size of 3 to 8 mm, and the amount added is 0.3% to 0.5% of the mass of molten iron.

8. The casting method for brake caliper bodies of various passenger vehicles as described in claim 1, characterized in that, In step S5, the second inoculant is a silicon-strontium inoculant containing 0.5% to 1.5% Sr, with a particle size of 0.2 to 0.8 mm, and the amount added is 0.1% to 0.2% of the mass of molten iron.

9. The casting method for brake caliper bodies of various passenger vehicles as described in claim 1, characterized in that, In step S5, the pouring temperature is controlled between 1360℃ and 1420℃. Before pouring, casting simulation software is used to numerically simulate the filling and solidification process of molten iron. Based on the simulation results, the combination of process parameters such as pouring temperature, pouring speed and cooling time is optimized.

10. The casting method for brake caliper bodies of various passenger vehicles as described in claim 1, characterized in that, In step S6, the cooling time is determined based on the casting wall thickness. The relationship between the cooling time t and the maximum casting wall thickness δ is: t = k × δ, where k is the cooling coefficient and the value of k ranges from 1.0 to 1.5 min / mm.

Citation Information

Patent Citations

  • Casting method and mold for manufacturing brake caliper

    CN105745042B

  • Automobile disc brake caliper body and design method thereof

    CN114458707A

  • A casting mold for automobile brake caliper bracket and a processing method thereof

    CN117428168B