A method for surface quality control of tempered high-strength hydroelectric steel billets
By adjusting the inverted taper of the crystallizer and the position of the chamfering roller, modifying the structure of the secondary cooling system, and controlling the secondary cooling water volume in different zones, the risk of corner and surface cracks in the billet during the continuous casting of hydroelectric steel was solved, and stable control of the surface quality of the billet was achieved.
Patent Information
- Application Number
- CN202611559003.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-09
- Publication Date
- 2026-11-17
AI Technical Summary
In the current technology for continuous casting of steel for hydropower, the mismatch between the chamfering roll and the corner of the billet, and the insufficient adjustment capacity of the secondary cooling edge circuit, lead to an increased risk of cracks at the corners and surface of the billet, especially under unsteady conditions and uneven cooling.
By adjusting the inverted taper and chamfer angle of the crystallizer, optimizing the relative position of the chamfering roller and the foot roller, modifying the structure of the secondary cooling system, setting independent adjustment and detection elements, and controlling the secondary cooling water volume in zones, the nozzles can be made to work stably under low casting speed conditions, and the water volume can be gradually restored after the billet passes through the straightening section.
It effectively reduced the incidence of corner and surface cracks in the billet, improved the surface quality of the billet, reduced the sudden change in cooling intensity when switching between low casting speed and normal conditions, and enhanced the system's adaptability to unsteady conditions.
Smart Images

Figure CN123102952A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of continuous casting production technology, specifically to a method for controlling the surface quality of tempered high-strength hydroelectric steel billets. Background Technology
[0002] High-strength steel for hydropower is mainly used in key load-bearing components such as turbine runners and frames in large hydropower stations. These components operate in complex environments, demanding high strength, low-temperature toughness, weldability, and surface quality from the steel. As the raw material for subsequent rolling and heat treatment, continuously cast billets are prone to defects such as cracks, especially at the corners, which can easily propagate during subsequent processing. Therefore, the surface quality of the cast billets is a crucial factor affecting the quality of finished hydropower steel products.
[0003] Compared to conventional slab steel grades, quenched and tempered high-strength hydroelectric steel exhibits more significant solidification shrinkage during solidification. If the same inverted taper of the crystallizer as conventional steel grades is used, a mismatch can easily occur between the changes in the crystallizer's internal dimensions and the solidification shrinkage of the initial billet shell, thus affecting the adhesion, heat transfer, and uniform growth of the billet shell to the crystallizer copper plate. Therefore, it is necessary to adaptively adjust the inverted taper and chamfer angle of the chamfered crystallizer according to the solidification shrinkage characteristics of quenched and tempered high-strength hydroelectric steel. In addition, after the billet leaves the crystallizer, the relative position between the chamfering rolls and foot rolls and the chamfered narrow-face copper plate directly affects the support state of the narrow-face and corner billet shell; insufficient support can easily cause additional deformation of the billet shell, increasing the risk of corner cracks.
[0004] During secondary cooling and subsequent straightening, the edge secondary cooling circuit, the number of nozzles, and the nozzle arrangement all affect the cooling intensity of the billet's edges and corners. For quenched and tempered high-strength hydroelectric steel, if the corner cooling intensity is too high, the billet corner temperature drops too quickly. When the corner temperature before the billet enters the straightening zone is lower than the upper limit temperature of the second brittle zone, the risk of corner cracking increases. Therefore, it is necessary to optimize the edge secondary cooling circuit and nozzle design to reduce the corner cooling intensity and increase the corner temperature, ensuring that the corner temperature before the billet enters the straightening zone avoids the second brittle zone.
[0005] Furthermore, continuous casting production involves various operating conditions, including initial casting speed increase, normal casting, and final casting speed reduction. Under low casting speed conditions such as initial casting and final casting, the residence time of the billet in the secondary cooling zone increases, necessitating a corresponding reduction in the secondary cooling water flow to prevent over-cooling. However, as the casting speed decreases, the target water flow rate for some secondary cooling circuits calculated based on the casting speed may drop to a lower level. When the water supply is lower than the minimum water flow rate required for normal nozzle operation, the nozzle spray and atomization state is prone to deterioration, and the cooling water may change from a uniform spray state to an unstable spray or even a dripping state. When dripping cooling water concentrates on a local surface of the billet, it can easily lead to excessive local cooling intensity, causing abnormal temperature drops in the local area of the billet and increasing the risk of surface cracks. Therefore, under low casting speed conditions, it is necessary not only to reduce the secondary cooling water flow rate according to the billet casting speed but also to consider the minimum water flow rate required for stable nozzle operation, ensuring that the secondary cooling system maintains a stable and uniform cooling state even under weak cooling conditions.
[0006] Existing technologies have studied the production of hydropower steel and the secondary cooling of continuous casting. For example, Chinese invention patent CN115141969A discloses a production method for 800MPa grade hydropower steel, but it does not optimize the geometric parameters of the chamfering roller and their relationship with the quality of the billet corner. Chinese invention patent CN103611903B discloses a continuous casting production process for extra-thick slabs for hydropower station pressure vessel steel. The published document involves a secondary cooling system for extra-thick slabs of hydropower steel, but there is still room for optimization in terms of independent control of the edge loop and adjustment of the cooling range. Overall, existing technologies do not adequately consider the synergistic effect between measures such as adjusting the chamfering taper of the chamfering crystallizer based on the solidification shrinkage characteristics of hydropower steel, optimizing the relative positions of the chamfering roller and foot roller with the chamfering narrow face crystallizer, controlling the billet corner temperature through secondary cooling nozzle design, and setting the minimum water volume of the nozzle under low casting speed conditions. It is necessary to implement systematic control of the above-mentioned aspects to reduce the risk of corner and surface cracks in hydropower steel billets. Summary of the Invention
[0007] This invention provides a method for controlling the surface quality of tempered high-strength hydroelectric steel billets, in order to solve the problems of unreasonable matching between the chamfering roller and the corner of the billet, insufficient adjustment capability of the secondary cooling edge circuit, and uneven cooling of the billet under non-steady-state conditions such as start-up speed increase, speed decrease and tail pulling in the existing hydroelectric steel continuous casting process.
[0008] The present invention provides a method for controlling the surface quality of tempered high-strength hydroelectric steel billets, which adopts the following technical solution: A method for controlling the surface quality of tempered high-strength hydroelectric steel billets includes the following steps.
[0009] S1 uses a chamfered crystallizer for slab continuous casting. The chamfered taper and chamfered angle of the crystallizer are adjusted according to the solidification shrinkage characteristics of the tempered high-strength hydroelectric steel so that the dimensional change of the inner cavity of the chamfered crystallizer perpendicular to the casting direction is adapted to the solidification shrinkage of the initial slab shell. Taking the lower working surface of the chamfered narrow copper plate of the crystallizer as the reference, the relative position of the chamfered roller and foot roller with the chamfered narrow copper plate is adjusted so that the narrow face and corner of the slab after exiting the crystallizer can obtain continuous and sufficient support. S2 optimizes the secondary cooling circuit and nozzle arrangement at the edge of the arc-shaped fan-shaped section, reducing the number of edge circuits and adjusting the number and arrangement of nozzles. Independent adjustment and detection elements are installed in each edge control circuit. The edge water pipes are independently led out from the main water supply pipe to achieve independent adjustment of each circuit. A slitting function is also set to adjust the edge cooling range according to the billet width. By reducing the secondary cooling intensity at the edges and corners of the billet, the corner temperature of the billet is increased, ensuring that the corner temperature before the billet enters the straightening zone is higher than the upper limit temperature of the second brittle zone. The nozzle configuration is adjusted accordingly in the straightening section, and independent control elements are added. S3, for low casting speed conditions during the initial casting speed increase and the final casting speed decrease, the cooling water volume of each secondary cooling circuit is adjusted according to the casting speed, and the minimum water volume corresponding to each secondary cooling circuit is set in the secondary cooling control program; when the target water volume calculated according to the casting speed is lower than the minimum water volume of the corresponding secondary cooling circuit, water is supplied according to the minimum water volume to keep the nozzle in a stable spray state, and to avoid local overcooling caused by the secondary cooling water dripping onto the casting surface due to the low water supply. S4. When the low casting speed condition ends and the billet corresponding to the low casting speed stage passes through the straightening section, the cooling water volume of each secondary cooling circuit is gradually restored from the controlled water volume under the low casting speed condition to the normal casting water volume according to the preset progressive method, so as to reduce the sudden change in cooling intensity during the switching between the low casting speed condition and the normal casting condition.
[0010] Furthermore, in S1, the inverted taper of the crystallizer is adjusted to 1.20%–1.30%; the flat portion of the first chamfering roller is 0.2–0.3 mm lower than the working surface of the lower end of the copper plate; the surface of the fourth foot roller is 1.5–2.0 mm lower than the reference; the second and third foot rollers are adjusted based on the reference formed by the first chamfering roller and the fourth foot roller, so that the gap between the second and third foot rollers and the reference is 0.
[0011] Furthermore, before S1, there are also pre-smelting process controls: converter endpoint control C≤0.05%, P≤0.008%, S≤0.035%; RH vacuum degree≤133Pa, vacuum treatment time≥15min, and calcium wire 80~200m is fed in after vacuum treatment.
[0012] Furthermore, when using a chamfered crystallizer for slab continuous casting in S1, continuous casting adopts full-process protective pouring, and the depth of the crystallizer immersion nozzle inserted into the molten steel surface is 150-180mm; the crystallizer adopts sinusoidal vibration with an amplitude of 2-3mm and a vibration frequency of 180-20V; the cooling water flow rate of the narrow face is 530-550L / min, and the cooling water flow rate of the wide face is 3900-4100L / min.
[0013] Furthermore, the structural modifications to the secondary cooling circuit at the edge of the arc-shaped fan-shaped section in S2 include: optimizing the original three-way width adjustment to two-way, reducing the number of nozzles per row from 6 to 4, and adjusting the nozzle arrangement and spray frame structure accordingly; maintaining the original spray frame structure in the straightening section and replacing the nozzles with models compatible with the weak cooling process; and adding filters to each modified circuit to reduce the impact of nozzle blockage on the secondary cooling water volume and spray state.
[0014] Furthermore, the low casting speed condition described in S3, i.e., the unsteady casting condition, includes two stages: the initial casting speed-up stage, which is the process from the start of casting until the casting speed increases to 0.8 m / min, and the entire process of the billet produced from the crystallizer before passing through the straightening section during this stage; and the final casting stage, which is the process of reducing the casting speed to 0.2 m / min at the end of casting for pouring the remaining steel in the tundish and pulling out the tail billet, and the entire process of the tail billet produced during this stage before passing through the straightening section. Under the above unsteady casting condition, based on the normal casting foundation water meter, the adjustment coefficients of the secondary cooling water volume in zones 1-3, 4-8, and 9-10 are set to 0.4-0.6, 0.7-0.9, and 0.9-1.1, respectively.
[0015] Furthermore, shutting off the wide-side cooling water means shutting off the wide-side cooling water from the lower part of the curved section to the fan-shaped section 8, while retaining the compressed air in the corresponding wide-side circuit.
[0016] Furthermore, the secondary cooling water volume in S4 is gradually restored to the normal casting water volume in a preset progressive manner: it is gradually restored in a progressive manner according to a fixed time interval, with each interval increasing to a preset multiple of the previous stage water volume, until the normal casting water volume is reached.
[0017] Furthermore, the fixed time interval is 25 to 35 seconds, and the preset multiple is 1.03 to 1.08 times. The method also sets the minimum water volume limit for each loop in the secondary cooling control program. When the target water volume calculated based on the pulling speed and adjustment coefficient is lower than the minimum water volume of the corresponding loop, water is supplied according to the minimum water volume set for that loop to ensure that the nozzle is in a stable working state. The minimum water volume of each loop is set according to the number of nozzles, the nozzle model, and the secondary cooling area where it is located.
[0018] Furthermore, after the billet is removed from the mold, it is placed in a heat preservation pit for slow cooling. The temperature in the pit is 780-820℃, and the slow cooling time is ≥46-50h. Then, surface inspection and necessary grinding are carried out.
[0019] The beneficial effects of this invention are as follows: The method for controlling the surface quality of high-strength hydroelectric steel billets using this invention effectively reduces the incidence of corner cracks by employing a chamfered crystallizer and adjusting its taper and chamfer angle. Through structural modifications to the secondary cooling circuits at the edges of the arc-shaped fan-shaped section, reducing the number of edge circuits, adjusting the nozzle arrangement, and setting independent adjustment and detection elements, each circuit can be independently adjusted. Combined with the width-cutting function, the edge cooling range is adjusted according to the billet width, reducing the edge strength of the billet and thus lowering the incidence of transverse cracks on the billet surface. By implementing zoned water reduction control with decreasing coefficients for different secondary cooling zones under unsteady casting conditions, and gradually restoring water volume according to a preset progressive method after the billet passes through the straightening section, the risk of overcooling of the billet under low casting speed conditions is reduced. Furthermore, by setting the minimum water volume of the nozzles under low casting speed conditions, the atomization effect of the nozzles is ensured, thereby reducing the sudden change in cooling intensity during the transition between low casting speed conditions and normal casting conditions.
[0020] Furthermore, by optimizing the inverted taper of the crystallizer to 1.20%–1.30% and precisely setting the geometric parameters of the chamfering roll and the foot roll, the mechanical support and deformation conditions of the billet corners were further improved; through strict control of the pre-smelting process, the quality of the molten steel entering the continuous casting process was ensured; through precise control of the entire process of protective pouring and the cooling water volume of the crystallizer, the stability of the continuous casting process was ensured; through specific modification schemes of the secondary cooling system, the existing equipment foundation was fully utilized, reducing the need for large-scale equipment replacement; through specific setting of the zonal dewatering coefficient under unsteady conditions, selective closure of the wide-side cooling water, and precise control of gradual recovery, the adaptability of the original control system to low casting speed conditions was improved; through the setting of minimum water volume limits, normal water output and atomization of the nozzles under weak cooling conditions were ensured; and through slow cooling treatment of the billet, the internal stress of the billet and the risk of hydrogen-induced cracking were further reduced. Attached Figure Description
[0021] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0022] Figure 1 A flowchart of a method for controlling the surface quality of tempered high-strength hydroelectric steel billets provided in an embodiment of the present invention; Figure 2 A comparison diagram of the arrangement of nozzles 1-6 in the fan-shaped section before and after the modification; Figure 3 This is a comparison diagram of the arrangement of nozzles 7-8 in the straightening section before and after the modification. Detailed Implementation
[0023] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0024] The component designations used in this document, such as "first" and "second," are merely for distinguishing the described objects and do not have any sequential or technical meaning. The terms "connection" and "linkage" used in this invention, unless otherwise specified, include both direct and indirect connections (linkages). It should be understood that the terms "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," and "counterclockwise," indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings and are used only for the convenience of describing the invention and simplifying the description. They do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as limiting the invention.
[0025] In this invention, unless otherwise explicitly specified and limited, "above" or "below" the second feature can mean that the first and second features are in direct contact, or that they are in indirect contact through an intermediate medium. Furthermore, "above," "over," and "on top" of the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply indicates that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply indicates that the first feature is at a lower horizontal level than the second feature.
[0026] This embodiment uses the continuous casting production of quenched and tempered high-strength hydroelectric steel (e.g., SX780CF steel) as an example to illustrate a method for controlling the surface quality of quenched and tempered high-strength hydroelectric steel billets according to the present invention. The production process of this embodiment is: molten iron – converter – LF refining – RH vacuum treatment – continuous casting – billet slow cooling and finishing. The smelting and refining processes are used to ensure that the composition, cleanliness, and temperature of the molten steel entering the continuous casting process meet the requirements for stable casting. The main improvements of the present invention are reflected in three aspects: optimization of the crystallizer taper and chamfer angle, optimization of the geometric parameters of the chamfering roller and foot roller, improvement of the secondary cooling system structure and nozzle arrangement, and zoned control of the secondary cooling water volume under unsteady conditions such as start-up speed increase and tail-end speed decrease. These three aspects work together to achieve full-process control of the billet surface quality. It should be noted that the implementation of the present invention is not limited to this; those skilled in the art can adjust the specific parameters according to the method given by the present invention.
[0027] like Figures 1 to 3 As shown in the figure, the present invention provides a method for controlling the surface quality of tempered high-strength hydroelectric steel billets, which specifically includes the following steps.
[0028] S1 employs a chamfered crystallizer for slab continuous casting. The crystallizer's taper and chamfer angle are adjusted based on the solidification shrinkage characteristics of quenched and tempered high-strength hydroelectric steel, ensuring that the dimensional changes of the crystallizer's inner cavity perpendicular to the casting direction match the solidification shrinkage of the initial slab shell. Using the lower working surface of the chamfered narrow-face copper plate of the crystallizer as a reference, the relative positions of the chamfering rollers and foot rollers with the chamfered narrow-face copper plate are adjusted to provide continuous and sufficient support for the narrow face and corners of the slab after exiting the crystallizer. Specifically, in slab continuous casting using a chamfered crystallizer, the crystallizer's taper is optimized from the default 1.15% to 1.25% based on the solidification shrinkage characteristics of quenched and tempered high-strength hydroelectric steel, and the chamfer angle is adjusted accordingly to improve the contact and heat transfer uniformity between the initial slab shell at the corner of the slab and the crystallizer, ensuring continuous and stable support for the corners of the slab after exiting the crystallizer. Then, the installation reference of the chamfering roll and the foot roll is determined according to the working surface of the lower end of the copper plate of the crystallizer, so that the corner of the billet can continuously obtain reasonable mechanical support after leaving the crystallizer, and reduce the additional strain at the corner caused by the mismatch of the roll gap.
[0029] S2 optimizes the secondary cooling circuit and nozzle arrangement at the edges of the arc-shaped fan-shaped section, reducing the number of edge circuits and adjusting the number and arrangement of nozzles. Independent adjustment and detection elements are installed in each edge control circuit. The edge water pipes are independently led out from the main water supply pipe to achieve independent adjustment of each circuit. A slitting function is set to adjust the edge cooling range according to the billet width. By reducing the secondary cooling intensity at the edges and corners of the billet, the corner temperature is increased, ensuring that the corner temperature before the billet enters the straightening zone is higher than the upper limit temperature of the second brittle zone. The nozzle configuration is adjusted accordingly in the straightening section, and independent control elements are added. Specifically, for arc-shaped fan-shaped sections 1 to... The secondary cooling circuit at the edge of section 6 underwent structural modification, optimizing the original three-way width adjustment into two-way adjustments. The number of nozzles per row was reduced from six to four, and the nozzle arrangement and spray frame structure were adjusted accordingly. Regulating valves and water flow meters were installed in each edge control circuit, while the original shut-off valves were retained. The edge water pipes were independently led out from the main water supply pipes, enabling each secondary cooling control circuit to be adjusted independently. At the same time, a slitting function was installed in the arc-shaped fan sections 1 to 6 to adjust the edge cooling range according to the width of the billet. The straightening sections 7 to 8 maintained the original spray frame structure, but the nozzle models were replaced with those adapted to the weak cooling process of hydroelectric steel, and independent control components were added.
[0030] S3, for low casting speed conditions during the initial casting speed increase and the final casting speed decrease, adjust the cooling water volume of each secondary cooling circuit according to the billet casting speed, and set the minimum water volume corresponding to each secondary cooling circuit in the secondary cooling control program; when the target water volume calculated according to the billet casting speed is lower than the minimum water volume of the corresponding secondary cooling circuit, water is supplied according to the minimum water volume to keep the nozzle in a stable spray state, and avoid local overcooling caused by the cooling water dripping onto the billet surface due to the low water supply.
[0031] S4. When the low casting speed condition ends and the billet corresponding to the low casting speed stage passes through the straightening section, the cooling water volume of each secondary cooling circuit is gradually restored from the controlled water volume under the low casting speed condition to the normal casting water volume according to the preset progressive method, so as to reduce the sudden change in cooling intensity during the switching between the low casting speed condition and the normal casting condition.
[0032] Specifically, for non-steady-state working conditions such as the initial acceleration of casting and the deceleration and tail pulling at the end of casting, the water volume adjustment coefficient of different secondary cooling zones is set to implement zoned water reduction control based on the normal casting foundation water meter. At the same time, the wide-side cooling water is turned off while the compressed air is retained. After the billet passes through the straightening section, the water volume is gradually restored to the normal casting volume according to the preset progressive method.
[0033] Through the synergistic effect of optimizing the crystallizer taper and roller system parameters, modifying the secondary cooling system structure, and controlling the water volume in unsteady conditions, the corner support and surface cooling processes of the billet are matched, effectively reducing the incidence of corner and surface cracks.
[0034] Furthermore, by adopting a chamfered crystallizer and adjusting the crystallizer's taper to a preset range, combined with the installation reference of the chamfered roller and foot roller determined according to the working surface of the lower end of the copper plate, the corner support of the billet after exiting the crystallizer is made more continuous, effectively reducing additional corner deformation. By modifying the structure of the secondary cooling circuit at the edge of the arc-shaped fan-shaped section, reducing the number of edge circuits, adjusting the nozzle arrangement, and setting independent adjustment and detection elements, each circuit can be adjusted independently. Combined with the width-cutting function, the edge cooling range is adjusted according to the billet width, reducing repeated edge cooling and mutual influence between different circuits. By implementing zoned water reduction control with decreasing coefficients for different secondary cooling areas under unsteady casting conditions, and gradually restoring water volume according to a preset progressive method after the billet passes through the straightening section, the risk of overcooling of the billet under low casting speed conditions is reduced, and the sudden change in cooling intensity during the switching between low-speed conditions and normal casting conditions is reduced.
[0035] In one embodiment, the inverted taper of the crystallizer in S1 is adjusted to 1.20% to 1.30%; the flat portion of the first chamfering roller is 0.2 to 0.3 mm lower than the working surface of the lower end of the copper plate; the surface of the fourth foot roller is 1.5 to 2.0 mm lower than the reference; the second and third foot rollers are adjusted based on the reference formed by the first chamfering roller and the fourth foot roller, so that the gap between the second and third foot rollers and the reference is 0.
[0036] Specifically, in this embodiment, the taper of the crystallizer is adjusted from 1.15% to 1.25%. The crystallizer adopts a chamfered structure, and its chamfered surface can be of type G30 or G32. The installation reference of the chamfering roller and foot roller is determined with the working surface of the lower end of the copper plate of the crystallizer as the reference: the flat part of the first chamfering roller is 0.2-0.3 mm lower than the working surface of the lower end of the copper plate, preferably 0.2 mm in this embodiment; the surface of the fourth foot roller is 1.5-2.0 mm lower than the above reference, 1.8 mm in this embodiment; the second and third foot rollers are adjusted with the reference formed by the first chamfering roller and the fourth foot roller, so that the gap between the second and third foot rollers and the above reference is 0. As a result, after the billet exits the crystallizer, its corners transition smoothly under the continuous support of the chamfering roller and foot roller, reducing the additional deformation of the corner billet shell.
[0037] In one embodiment, a pre-smelting process control is included before S1 to ensure that the composition, cleanliness, and temperature of the molten steel entering the continuous casting process meet the requirements for stable casting. Specifically, the converter endpoint is controlled with C ≤ 0.05%, P ≤ 0.008%, and S ≤ 0.035%, preferably controlled in this embodiment with C ≤ 0.04%, P ≤ 0.006%, and S ≤ 0.035%; during RH vacuum treatment, the vacuum degree is controlled to ≤ 133 Pa, and the vacuum treatment time is ≥ 15 min; after vacuum treatment, 80–200 m of calcium wire is fed in, and in this embodiment, 150–180 m of seamless calcium wire is fed in. In addition, the superheat of the molten steel in the tundish can be controlled within the range of 10–20°C to ensure the stability of the continuous casting process.
[0038] In one embodiment, in S1, continuous casting employs full-process protective casting, with the immersion nozzle of the crystallizer inserted to a depth of 150–180 mm into the molten steel. The crystallizer uses sinusoidal vibration with an amplitude of 2–3 mm (2.5 mm in this embodiment) and a vibration frequency of 180–20 V. The mold flux can be ZT-01-2 type mold flux. When using a chamfered crystallizer, the cooling water flow rate on the narrow side is 530–550 L / min (540 ± 10 L / min in this embodiment); the cooling water flow rate on the wide side is 3900–4100 L / min (4000 ± 100 L / min in this embodiment), to ensure uniform growth of the billet shell and stable solidification at the corners within the crystallizer. The control of the insertion depth of the immersion nozzle in the molded crystallizer during the entire pouring process effectively prevents secondary oxidation and slag entrapment of molten steel; the optimization of the protective slag and the vibration parameters of the molded crystallizer ensures uniform growth of the billet shell and good surface quality; the precise control of the cooling water volume in the molded crystallizer enables the billet to obtain a suitable cooling intensity in the molded crystallizer, providing stable initial conditions for the cooling control of the subsequent secondary cooling zone.
[0039] In one embodiment, in S2, the secondary cooling circuit at the edge of the arc-shaped sector segment is structurally modified, specifically including: as follows Figure 2 As shown, the original three-way width adjustment of the arc-shaped fan-shaped segments 1-6 has been optimized to two-way, the number of nozzles in each row has been adjusted from 6 to 4, and the nozzle arrangement and spray frame structure have been adjusted accordingly; as shown Figure 3As shown, the straightening sections 7-8 retain the original spray frame structure, only replacing the nozzles with models compatible with the weak cooling process of the hydroelectric steel. In each edge control loop of the arc-shaped fan sections 1-6 and the straightening sections 7-8, regulating valves (as independent regulating elements) and water flow meters (as detection elements) are installed, while the original shut-off valves are retained. The edge water pipes are independently led out from the main water supply pipe, allowing each secondary cooling control loop to be independently adjustable. Arc-shaped fan sections 1-6 are equipped with a sizing function to adjust the edge cooling range according to the billet width. Simultaneously, filters are added to each secondary cooling modification loop; in this embodiment, a Y-type filter is added to reduce the impact of nozzle blockage on the secondary cooling water volume and spray pattern. Through the above modifications, the existing equipment foundation is fully utilized, eliminating the need for large-scale replacement of continuous casting equipment. Simultaneously, each edge loop can independently adjust the water volume and independently detect the flow rate. Combined with the sizing function, precise control of the edge cooling range is achieved, effectively reducing repeated edge cooling and mutual interference between different loops, and lowering the risk of localized overcooling at the edges.
[0040] In one embodiment, the low-speed casting condition in S3, i.e., the unsteady-state casting condition, includes two stages: the initial casting speed-up stage, which is the process from the start of casting until the casting speed increases to 0.8 m / min, and the entire process of the billet produced from the crystallizer before passing through the straightening section; and the final casting stage, which is the process of reducing the casting speed to 0.2 m / min at the end of casting for pouring the remaining steel in the tundish and pulling out the tail billet, and the entire process of the tail billet produced in this stage before passing through the straightening section. Under the above unsteady-state casting condition, based on the normal casting foundation water meter, the adjustment coefficients of the secondary cooling water volume in zones 1-3, 4-8, and 9-10 are set to 0.4-0.6, 0.7-0.9, and 0.9-1.1, respectively.
[0041] Specifically, this includes the period from the start of casting to the increase in casting speed to 0.8 m / min, and the stage before the cast billet passes through the straightening section; it also includes the stage at the end of casting when the casting speed decreases to 0.2 m / min for the pouring of the remaining steel in the tundish and the removal of the tail billet. Under the above-mentioned unsteady casting conditions, based on the water meter of the normal casting foundation, a decreasing water volume adjustment coefficient is set for different secondary cooling zones to achieve zoned water reduction control. Specifically: the secondary cooling water volume adjustment coefficient for zones 1 to 3 is set to 0.4 to 0.6, and in this embodiment, it is 0.5; the secondary cooling water volume adjustment coefficient for zones 4 to 8 is set to 0.7 to 0.9, and in this embodiment, it is 0.8; the secondary cooling water volume adjustment coefficient for zones 9 to 10 is set to 0.9 to 1.1, and in this embodiment, it is 1.0. Because the residence time of the cast billet in the secondary cooling zone increases and the cooling time per unit length is prolonged under low casting speed conditions, the above-mentioned zoned water reduction control can avoid local overcooling of the cast billet. To put it simply, the above-mentioned zoned cooling control strategy effectively avoids undercooling in different areas of the billet under low casting speed conditions: the cooling effect is greatest in the near-crystallizer area (zones 1-3) because the billet temperature is highest in this area and the residence time increases most significantly at low casting speeds; moderate cooling is applied to the middle area (zones 4-8); and the water level is maintained close to normal in the far-end area (zones 9-10). Closing the wide-edge cooling water while retaining compressed air further reduces undercooling at the edges and uneven cooling.
[0042] In one embodiment, in S3, shutting off the wide-edge cooling water specifically involves shutting off the wide-edge cooling water from the lower part of the curved section to the fan-shaped section 8, while retaining the compressed air in the corresponding wide-edge loop to keep the nozzle atomization channel unobstructed and prevent nozzle blockage during water outages. This area corresponds to the transition zone between the billet and the arc-shaped fan-shaped section after the billet exits the curved section. During this stage, the temperature gradient of the billet is large, and excessive edge cooling can easily lead to a sudden drop in corner temperature, increasing crack sensitivity. Retaining the compressed air in the corresponding wide-edge loop keeps the pipeline unobstructed even without water supply, avoiding problems such as water pressure shock and unstable nozzle atomization when water supply is restored. By selectively shutting off the wide-edge cooling water in specific areas, the risk of edge overcooling is reduced while ensuring normal narrow-face cooling and the uniformity of the overall temperature distribution of the billet.
[0043] In one embodiment, in S4, after the billet corresponding to the low casting speed stage in S3 passes through the straightening section, the secondary cooling water volume is gradually restored in a progressive manner according to a fixed time interval, increasing to a preset multiple of the water volume of the previous stage at each interval. That is, from the beginning of the restoration, after each fixed time interval, the secondary cooling water volume of each circuit is increased to a preset multiple of the water volume at the beginning of that interval. This is done step by step until the normal casting water volume is reached, thereby reducing the sudden change in cooling intensity during the switching between low casting speed conditions and normal casting conditions, making the surface temperature of the billet transition smoothly, and effectively reducing thermal stress cracks caused by sudden temperature changes.
[0044] In one embodiment, the fixed time interval in S4 is 25-35 seconds, and in this embodiment it is 30 seconds; the preset multiple is 1.03-1.08 times, and in this embodiment it is 1.05 times. Furthermore, to address the issue of low calculated water volume in some secondary cooling circuits under weak cooling conditions in hydroelectric steel systems, and the potential for unstable water output or poor atomization from the nozzles, minimum water volume limits are set for each circuit in the secondary cooling control program: when the target water volume calculated based on the pulling speed and adjustment coefficient is higher than the minimum water volume of the corresponding circuit, water is supplied according to the calculated target water volume; when the target water volume is lower than the minimum water volume of the corresponding circuit, water is supplied according to the minimum water volume set for that circuit, ensuring that the nozzles are in a stable working state and avoiding unstable water output or poor atomization due to insufficient water volume, thus ensuring the stable operation of the secondary cooling system. The minimum water volume for each circuit is set according to the number of nozzles, nozzle model, and the secondary cooling area. The minimum water volume for each circuit in this embodiment is shown in Table 1.
[0045] Table 1 Minimum water volume for each loop In one embodiment, after the billet is removed from the heat treatment pit, it is slowly cooled. The temperature inside the pit is 780–820°C, and in this embodiment, the temperature inside the pit is controlled to be ≥800°C. The slow cooling time is 46–50 hours, and in this embodiment, the slow cooling time is controlled to be ≥48 hours. Slow cooling in the heat treatment pit further reduces the internal stress of the billet and the risk of hydrogen-induced cracking. After slow cooling, the surface of the billet is inspected, and necessary grinding is performed based on the inspection results to obtain a billet with acceptable surface quality. Furthermore, through the slow cooling treatment in the heat treatment pit, the internal temperature of the billet decreases slowly and uniformly, effectively releasing the thermal stress accumulated during continuous casting and solidification, while promoting the escape of diffusible hydrogen in the billet, reducing the risk of hydrogen-induced cracking, and further ensuring the surface and internal quality of the hydropower steel billet.
[0046] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method of controlling the surface quality of a quenched high-strength hydroelectric steel cast slab, characterized in that, Includes the following steps: S1 uses a chamfered crystallizer for slab continuous casting. The chamfered taper and chamfered angle of the crystallizer are adjusted according to the solidification shrinkage characteristics of the tempered high-strength hydroelectric steel so that the dimensional change of the inner cavity of the chamfered crystallizer perpendicular to the casting direction is adapted to the solidification shrinkage of the initial slab shell. Taking the lower working surface of the chamfered narrow copper plate of the crystallizer as the reference, the relative position of the chamfered roller and foot roller with the chamfered narrow copper plate is adjusted so that the narrow face and corner of the slab after exiting the crystallizer can obtain continuous and sufficient support. S2 optimizes the secondary cooling circuit and nozzle arrangement at the edge of the arc-shaped fan-shaped section, reducing the number of edge circuits and adjusting the number and arrangement of nozzles. Independent adjustment and detection elements are installed in each edge control circuit. The edge water pipes are independently led out from the main water supply pipe to achieve independent adjustment of each circuit. A slitting function is also set to adjust the edge cooling range according to the billet width. By reducing the secondary cooling intensity at the edges and corners of the billet, the corner temperature of the billet is increased, ensuring that the corner temperature before the billet enters the straightening zone is higher than the upper limit temperature of the second brittle zone. The nozzle configuration is adjusted accordingly in the straightening section, and independent control elements are added. S3, for low casting speed conditions during the initial casting speed increase and the final casting speed decrease, the cooling water volume of each secondary cooling circuit is adjusted according to the casting speed, and the minimum water volume corresponding to each secondary cooling circuit is set in the secondary cooling control program; when the target water volume calculated according to the casting speed is lower than the minimum water volume of the corresponding secondary cooling circuit, water is supplied according to the minimum water volume to keep the nozzle in a stable spray state, and to avoid local overcooling caused by the secondary cooling water dripping onto the casting surface due to the low water supply. S4. When the low casting speed condition ends and the billet corresponding to the low casting speed stage passes through the straightening section, the cooling water volume of each secondary cooling circuit is gradually restored from the controlled water volume under the low casting speed condition to the normal casting water volume according to the preset progressive method, so as to reduce the sudden change in cooling intensity during the switching between the low casting speed condition and the normal casting condition.
2. The surface quality control method of a quenched and tempered high-strength steel for a water power plant according to claim 1, characterized by: In S1, the taper of the crystallizer is adjusted to 1.20%–1.30%; the flat part of the first chamfering roller is 0.2–0.3 mm lower than the working surface of the lower end of the copper plate; the surface of the fourth foot roller is 1.5–2.0 mm lower than the reference; the second and third foot rollers are adjusted based on the reference formed by the first chamfering roller and the fourth foot roller, so that the gap between the second and third foot rollers and the reference is 0.
3. The surface quality control method of a quenched and tempered high-strength steel for a water power plant according to claim 1, characterized by: Before S1, there is also the control of the pre-smelting process: converter end point control C≤0.05%, P≤0.008%, S≤0.035%; RH vacuum degree≤133Pa, vacuum treatment time≥15min, and calcium wire 80~200m is fed in after vacuum treatment.
4. The surface quality control method of a quenched and tempered high strength hydroelectric steel billet according to claim 1, characterized in that: When using a chamfered crystallizer for slab continuous casting in S1, continuous casting is carried out with full-process protective pouring. The depth of the crystallizer's submersible nozzle into the molten steel is 150-180mm. The crystallizer uses sinusoidal vibration with an amplitude of 2-3mm and a vibration frequency of 180-20V. The cooling water flow rate for the narrow face is 530–550 L / min, and the cooling water flow rate for the wide face is 3900–4100 L / min.
5. The method of surface quality control of a quenched and tempered high strength hydroelectric steel billet according to claim 1, characterized in that: The structural modifications to the secondary cooling circuit at the edge of the arc-shaped fan-shaped section in S2 include: optimizing the original three-way width adjustment to two-way, reducing the number of nozzles per row from 6 to 4, and adjusting the nozzle arrangement and spray frame structure accordingly; maintaining the original spray frame structure in the straightening section and replacing the nozzles with models compatible with the weak cooling process; and adding filters to each modified circuit to reduce the impact of nozzle blockage on the secondary cooling water volume and spray state.
6. The method of surface quality control of a quenched and tempered high strength hydroelectric steel billet according to claim 1, characterized in that: The low casting speed condition described in S3 is the unsteady-state casting condition, which includes two stages: the initial casting speed-up stage, which is the process from the start of casting until the casting speed increases to 0.8 m / min, and the entire process of the billet produced from the crystallizer before passing through the straightening section; and the final casting stage, which is the process of reducing the casting speed to 0.2 m / min at the end of casting for pouring the remaining steel in the tundish and pulling out the tail billet, and the entire process of the tail billet produced in this stage before passing through the straightening section. Under the above unsteady-state casting condition, based on the normal casting foundation water meter, the adjustment coefficients of the secondary cooling water volume in zones 1-3, 4-8, and 9-10 are set to 0.4-0.6, 0.7-0.9, and 0.9-1.1, respectively.
7. The surface quality control method of a quenched and tempered high-strength steel for a water power plant according to claim 6, characterized by: Shutting down the wide-side cooling water means shutting down the wide-side cooling water from the lower part of the curved section to the fan-shaped section 8, while retaining the compressed air in the corresponding wide-side circuit.
8. The method of surface quality control of a quenched and tempered high strength hydroelectric steel billet according to claim 1, characterized in that: The cooling water volume in S4 is gradually restored to the normal casting water volume in a preset progressive manner: it is gradually restored according to a fixed time interval, with each interval increasing to a preset multiple of the previous stage water volume, until the normal casting water volume is reached.
9. The surface quality control method of a quenched and tempered high-strength steel for a water power plant according to claim 8, characterized in that: The fixed time interval is 25 to 35 seconds, and the preset multiple is 1.03 to 1.08 times. The method also sets the minimum water volume limit for each circuit in the secondary cooling control program. When the target water volume calculated based on the pulling speed and adjustment coefficient is lower than the minimum water volume of the corresponding circuit, water is supplied according to the minimum water volume set for that circuit to ensure that the nozzle is in a stable working state. The minimum water volume of each circuit is set according to the number of nozzles, the nozzle model, and the secondary cooling area where it is located.
10. The method of surface quality control of a quenched and tempered high strength hydroelectric steel billet according to claim 1, characterized in that: After the billet is removed from the furnace, it is placed in a heat preservation pit for slow cooling. The temperature in the pit is 780-820℃, and the slow cooling time is ≥46-50h. Then, the surface is inspected and necessary grinding is performed.
Citation Information
Patent Citations
A continuous casting production process of extra-thick slab for pressure vessel steel of hydropower station
CN103611903B
Production method of 800MPa grade hydroelectric steel
CN115141969A