A process for preparing small-aperture diamond copper by sintering and metallization
By employing a process chain of laser hole preparation, mixed acid decarburization, plasma decarburization and RF sputtering seed layer, vacuum slurry sintering and chemical mechanical polishing, the problems of difficult removal of residual graphite and carbon impurities on the hole walls, reduced seed layer coverage and difficulty in electroplating filling in the metallization of small-diameter diamond through holes have been solved. This has enabled efficient and reliable metallization layer preparation, which is suitable for third-generation semiconductor high thermal conductivity packaging substrates.
Patent Information
- Application Number
- CN202611374853.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for metallizing small-diameter diamond through-holes suffer from problems such as difficulty in removing residual graphite and carbon impurities from the pore walls, reduced coverage of the seed layer steps, difficulty in electroplating filling, and complex processes with low yields. These issues lead to failures in metallizing small-diameter, high-aspect-ratio through-holes and significant challenges in mass production.
A process chain is adopted, which includes laser hole making, mixed acid decarburization, plasma decarburization and micro-roughening, radio frequency magnetron sputtering seed layer, vacuum slurry sintering and chemical mechanical polishing, combined with nano copper paste filling and stepped temperature sintering, to achieve continuous and dense filling of hole wall purification, seed layer deposition and metallization layer.
It significantly improves the bonding strength and electrical continuity of small-aperture diamond through-holes, shortens the preparation cycle, improves product yield and reliability, and is suitable for large-scale industrial production.
Smart Images

Figure CN123103000A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of high thermal conductivity packaging substrates for third-generation semiconductors, specifically to a process for preparing diamond copper sintering metallization with small apertures. Background Technology
[0002] The mainstream process route for metallizing through-holes in diamond substrates is as follows: laser processing of through-holes → hole wall cleaning → physical vapor deposition (PVD) seed layer → electroplating for hole filling. Previous research has achieved single-crystal diamond through-hole filling with a 50µm diameter and a depth-to-diameter ratio of 7:1 using a segmented electroplating process, and copper filling of diamond through-holes with a depth-to-diameter ratio of 10:1 using a bottom-up electroplating technique. However, when the through-hole diameter is further reduced to 50–150µm and the depth-to-diameter ratio reaches 4:3 to 10:1, the existing technology still has the following shortcomings: First, there is a lack of effective means to remove the graphite and carbon impurities remaining on the borehole walls after laser drilling. Laser processing causes graphitization of the diamond surface, especially in small-diameter deep holes. The graphite layer and carbon-embedded impurities remaining on the borehole walls are difficult to reach and remove by conventional cleaning methods, which seriously affects the bonding strength between the subsequent seed layer and the substrate. Existing cleaning methods are mostly aimed at planar surfaces, and their carbon removal effect on the inner walls of small-diameter deep holes is limited. It is difficult to balance thoroughness and non-destructiveness to the substrate, and it is impossible to provide a clean and highly active bonding interface for seed layer deposition.
[0003] Second, the seed layer's step coverage capability decreases sharply as the pore size decreases. For small-diameter, high-aspect-ratio through-holes of 50-150µm, traditional DC magnetron sputtering suffers from severe shielding due to the linear transport of ions. This results in excessively thick deposition at the pore opening while the film at the bottom and middle of the pore wall is extremely thin or even broken, preventing subsequent filling from forming a continuous conductive path. This is one of the main reasons for the failure of metallization in small-diameter through-holes.
[0004] Third, electroplating fills small-diameter, high-aspect-ratio through-holes with inherent defects. When the pore size is 50-150µm and the aspect ratio is 4:3 or higher, the electroplating solution has difficulty convection within the micropores, and air bubbles are easily trapped, forming internal voids. At the same time, the current density distribution within the micropores is extremely uneven, and premature sealing of the pore opening leads to central voids, making it difficult to achieve defect-free dense filling. Furthermore, the electroplating cycle can be as long as 5-20 hours, severely restricting mass production efficiency.
[0005] Fourth, the existing process route is complex, difficult to control, and has a low yield. Seed layer deposition and electroplating filling are each subject to multiple factors, and fluctuations in any step can lead to product failure. For small-diameter through holes of 50-150um, the process window is even narrower, the risk of failure is higher, and the overall yield and reliability are difficult to guarantee, which cannot meet the needs of large-scale mass production of small-diameter diamond through holes.
[0006] In summary, existing miniaturized diamond through-holes (hole diameter 50-150um, hole depth 200-500um, depth-to-diameter ratio 4:3-10:1) suffer from a series of technical defects, including poor step coverage of traditional DC sputtering, difficulty in convection of electroplating solution in small holes, easy generation of internal voids, insufficient coating density, poor conductivity consistency, and excessively long preparation cycle.
[0007] Therefore, it is necessary to provide a suitable sintering metallization process for small-aperture diamond copper. Summary of the Invention
[0008] The present invention provides a sintering metallization process for diamond copper with small aperture, which effectively solves the existing problems.
[0009] The technical solution adopted in this invention is: a process for preparing small-aperture diamond copper sintering metallization, comprising the following steps: S1, processing and pre-treating a diamond substrate with through holes; S2, chemically decarburizing the through hole walls; S3, plasma decarburizing and micro-roughening treatment of the through hole walls; S4, depositing a seed layer on the through hole walls using physical vapor deposition; S5, filling the through holes with metal paste and sintering and solidifying; S6, planarizing the substrate surface.
[0010] Furthermore, in step S1, the through-hole processing and pretreatment includes: preparing through-holes on a diamond substrate using laser processing, and then removing molten carbon slag and surface slag from the holes by airflow punching; the thickness of the diamond substrate is 200-600 μm, and the diameter of the through-hole is 50-150 μm.
[0011] Furthermore, in step S2, the chemical decarbonization treatment includes: immersing the diamond substrate in an oxidizing mixed acid solution to remove the graphite layer and carbon impurities remaining from laser processing; cleaning and drying are performed after decarbonization; the oxidizing mixed acid solution is a compound solution of 98% concentrated sulfuric acid and 68% concentrated nitric acid, with a volume ratio of 4:1 between concentrated sulfuric acid and concentrated nitric acid, an immersion temperature of 60-65°C, and an immersion time of 16-20 minutes.
[0012] Furthermore, in step S3, the plasma decarburization and micro-roughening treatment includes: sending the substrate after chemical decarburization into a plasma etching apparatus, using oxygen-containing mixed plasma to perform fine decarburization on the hole walls, and simultaneously forming a micro-uneven structure on the hole wall surface; the plasma etching uses a mixed gas of O2 and CF4, with a radio frequency power of 130W, an O2 flow rate of 40sccm, a CF4 flow rate of 8-12sccm, a working gas pressure of 2.8-3.2mTorr, and an etching time of 8-12min.
[0013] Furthermore, in step S4, the physical vapor deposition process is an RF magnetron sputtering process; before depositing the seed layer, the substrate is first vacuum baked to remove gas and evacuated to a base vacuum level of 9×10⁻⁶. -7 The substrate is pre-cleaned with in-situ argon plasma below Torr; the radio frequency frequency of the radio frequency magnetron sputtering is 13.56MHz, and the substrate rotates at a constant speed during the deposition process.
[0014] Furthermore, in step S4, the seed layer comprises a Ti adhesion barrier layer and a Cu conductive seed layer deposited sequentially; the radio frequency power density of the Ti layer is 4.0–4.5 W / cm². 2 The substrate bias voltage is -40 to -45V, and the film thickness is 80 to 120 nm; the radio frequency power density of the Cu layer is 3.5 to 4.0 W / cm². 2 The substrate bias voltage is -28 to -32V, and the film thickness is 800 to 1200nm.
[0015] Furthermore, in step S5, the metal paste is a nano-copper paste, which uses 30-50nm spherical nano-copper powder as filler, has a solid content of 88-90wt%, and a room temperature viscosity of 1800-2200mPa·s.
[0016] Furthermore, in step S5, the through holes are filled using a vacuum negative pressure grouting method: the substrate is placed in a vacuum environment to purge the gas inside the through holes, with a vacuum degree of -0.095 to -0.098 MPa, and then micro positive pressure grouting is used, with a grouting pressure of 0.25 to 0.3 MPa, and pressure is maintained for 8 to 12 minutes.
[0017] Furthermore, in step S5, the sintering and solidification adopts a stepped heating sintering process: first, the temperature is raised to 110-130℃ and held for 20-40 minutes, then the temperature is raised to 280-300℃ and held for 70-110 minutes, so that the nano-copper particles are densified and formed.
[0018] Furthermore, in step S6, the planarization process employs a double-sided chemical mechanical polishing process to remove excess sintered metal layers from the substrate surface, retaining only the solid metal pillars inside the through holes.
[0019] Beneficial effects of the invention: 1. This application constructs a complete process chain of "laser hole making → mixed acid decarburization → plasma roughening → radio frequency sputtering seed layer → vacuum slurry casting → chemical mechanical polishing (CMP)". The processes are closely connected and coordinated, overcoming the drawbacks of traditional processes where sputtering and electroplating are subject to multiple constraints and fluctuations in any step can lead to product failure. Addressing the issues of narrow process windows and high failure risk for 50-150µm small-diameter through-holes, this application significantly widens the overall process window and greatly improves product yield through refined control and coordinated operation of each process. Furthermore, the process is simplified and highly repeatable, stably adaptable to the large-scale industrial production of diamond substrates with a full depth of 200-600µm and a hole diameter of 50-150µm, effectively solving the industry problems of low metallization yield, poor reliability, and high mass production difficulty for small-diameter diamond through-holes.
[0020] 2. To address the challenge of removing residual graphite and carbon-embedded impurities from laser-drilled deep pores with small apertures (50-150µm), this invention employs a dual decarburization process combining chemical and plasma decarburization. First, the strong oxidizing and dehydrating properties of a concentrated sulfuric acid / nitric acid mixed acid system are utilized to directionally ablate the amorphous graphite layer and carbonized deposits on the pore wall surface. Then, a fine etching process using O2 / CF4 mixed plasma thoroughly removes trace amounts of embedded carbon impurities that are difficult to reach through acid washing, while simultaneously forming a uniform micro-uneven structure on the pore wall surface. This two-step synergistic effect achieves comprehensive deep purification of the pore wall and the construction of a physical anchoring interface, providing a clean and highly active bonding surface for the subsequent seed layer, significantly improving the film-substrate bonding strength, and ensuring the long-term reliability of the metallization layer.
[0021] 3. Addressing the inherent defects of DC sputtering in 50-150µm aperture and aspect ratio (4:3 to 10:1) micropores, which suffer from shielding effects due to linear transport and are prone to film breakage, this invention employs 13.56MHz high-frequency radio frequency magnetron sputtering technology. Utilizing the migration characteristics of radio frequency ions through random scattering, it significantly improves the film coverage of the sidewalls and bottom of high aspect ratio micropores, achieving a film thickness coverage of 58%–65% on the pore walls. Combined with a gradient design of high bias voltage for enhanced anchoring of the Ti layer and low bias voltage for the Cu layer to avoid backsputtering losses, and an ultra-high vacuum environment, continuous, dense, and uninterrupted deposition of the Ti / Cu composite seed layer is achieved throughout the entire small-aperture deep-hole region, completely solving the film breakage problem in small-aperture deep-hole applications.
[0022] 4. Addressing the inherent drawbacks of 50-150µm micropore electroplating solutions, such as difficult convection, severe polarization, easy bubble trapping, and central voids, coupled with a long cycle of 5-20 hours, this invention abandons traditional electroplating methods and employs an integrated filling technology combining vacuum negative pressure injection of nano-copper paste and stepped low-temperature sintering. By using a vacuum negative pressure of -0.095 to -0.098 MPa to fully expel trapped air from the micropores, combined with micro-positive pressure injection, the low-viscosity nano-copper paste completely fills the entire through-hole area, fundamentally eliminating bubble trapping and internal voids. The 280-300℃ low-temperature stepped sintering effectively reduces shrinkage stress, preventing cracking and depression of the copper pillars. The filling density approaches 100%, and the entire filling process takes only about 2 hours, significantly shortening the preparation cycle and greatly improving mass production efficiency. Attached Figure Description
[0023] Figure 1 A flowchart illustrating a small-aperture diamond-copper sintering metallization preparation process provided for embodiments of this application. Detailed Implementation
[0024] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0025] like Figure 1 As shown in the embodiments of this application, an adaptive small-aperture diamond-copper sintering metallization preparation process is provided, including the following steps: S1, processing and pre-treating a diamond substrate with through holes; S2, chemically decarburizing the through hole walls; S3, plasma decarburizing and micro-roughening treatment of the through hole walls; S4, depositing a seed layer on the through hole walls using physical vapor deposition; S5, filling the through holes with metal paste and sintering and solidifying; S6, planarizing the substrate surface.
[0026] In the above design, a complete process chain is employed, including through-hole processing and pretreatment, chemical decarburization, plasma decarburization and micro-roughening, physical vapor deposition seed layer, metal slurry filling, sintering and curing, and planarization, achieving full-process controllability of through-hole metallization on diamond substrates. Compared to existing technologies, this method avoids the problems of internal voids and insufficient coating density caused by difficult chemical convection and severe polarization in traditional electroplating through-holes with small diameter and high aspect ratio. The close connection and synergistic effect between each process can stably achieve high-density filling of through-hole metallization, significantly improving product yield and reliability. At the same time, the process is simplified and the preparation cycle is greatly shortened, showing good prospects for large-scale industrial production.
[0027] Specifically: In step S1, the through-hole processing and pretreatment includes: preparing through-holes on a diamond substrate using laser processing, and then removing molten carbon slag and surface slag from the holes by airflow punching; the thickness of the diamond substrate is 200-600 μm, and the diameter of the through-hole is 50-150 μm.
[0028] In the above design, by further defining the through-hole processing and pretreatment steps, laser processing is used to prepare through-holes with a diameter of 50-150 μm on a diamond substrate with a thickness of 200-600 μm. Combined with airflow punching to remove molten carbon slag and surface dross from the holes, this ensures the unobstructed flow of the small-diameter, high-aspect-ratio through-holes, providing a clean and transparent channel foundation for subsequent decarburization and metallization processes. The combination of laser processing and airflow punching in this step effectively removes macroscopic impurities, preventing large carbon slag pieces from causing poor adhesion or filling defects on the hole walls in subsequent processes, further ensuring the stability and consistency of the metallization quality.
[0029] Specifically, in step S2, the chemical decarbonization process includes: immersing the diamond substrate in an oxidizing mixed acid solution to remove the graphite layer and carbon impurities remaining from laser processing; cleaning and drying after decarbonization; the oxidizing mixed acid solution is a compound solution of 98% concentrated sulfuric acid and 68% concentrated nitric acid, with a volume ratio of 4:1 between the concentrated sulfuric acid and concentrated nitric acid, an immersion temperature of 60-65°C, and an immersion time of 16-20 minutes.
[0030] In the above design, an oxidizing mixed acid solution, composed of concentrated sulfuric acid and concentrated nitric acid in a 4:1 volume ratio, is used. The solution is immersed at 60–65°C for 16–20 minutes. Utilizing the strong oxidizing and dehydrating properties of the mixed acid system, the amorphous graphite layer, carbonized deposits, and embedded carbon impurities remaining after laser drilling are directionally dissolved. Simultaneously, the diamond substrate is chemically stable and unaffected by strong acid corrosion, exhibiting good selectivity for carbon removal. Combined with multi-stage overflow cleaning with ultrapure water and ultrasonic cleaning, residual acid within the pores and on the plate surface is thoroughly removed, ensuring the cleanliness of the pore wall interface. This provides a highly active bonding interface for subsequent seed layer deposition, effectively improving the film-substrate bonding strength and preventing seed layer peeling or void expansion caused by residual carbon impurities.
[0031] Specifically: In step S3, the plasma decarburization and micro-roughening treatment includes: sending the substrate after chemical decarburization into a plasma etching equipment, using oxygen-containing mixed plasma to finely decarburize the hole walls, and simultaneously forming a micro-uneven structure on the surface of the hole walls; the plasma etching uses a mixed gas of O2 and CF4, with a radio frequency power of 130W, an O2 flow rate of 40sccm, a CF4 flow rate of 8-12sccm, a working gas pressure of 2.8-3.2mTorr, and an etching time of 8-12min.
[0032] In the above design, by refining the plasma decarburization and micro-roughening steps, a mixed plasma of O2 and CF4 (RF power 130W, O2 flow rate 40sccm, CF4 flow rate 8-12sccm, gas pressure 2.8-3.2mTorr, etching 8-12min) is further used to treat the hole walls on the basis of chemical decarburization. This can thoroughly remove trace embedded carbon impurities that are difficult to remove by acid washing, and at the same time form a uniform micro-uneven structure on the hole wall surface. This micro-uneven structure can significantly increase the mechanical anchoring contact area between the hole wall and the subsequent sputtered seed layer, significantly improve the adhesion strength and anti-peeling ability of the seed layer, and the plasma dry process will not cause thermal or mechanical damage to the diamond substrate. It is especially suitable for micro-aperture through holes with high aspect ratio and small hole wall area, ensuring the uniformity and repeatability of the hole wall treatment.
[0033] Specifically: In step S4, the physical vapor deposition process is an RF magnetron sputtering process; before depositing the seed layer, the substrate is first vacuum baked to remove gas and evacuated to a base vacuum level of 9×10⁻⁶. -7 The substrate is pre-cleaned with in-situ argon plasma below Torr; the radio frequency frequency of the radio frequency magnetron sputtering is 13.56MHz, and the substrate rotates at a constant speed during the deposition process.
[0034] In the above design, by limiting the pretreatment steps before RF magnetron sputtering deposition of the seed layer, the substrate is first vacuum baked and degassed and then evacuated to a base vacuum level of 9×10⁻⁶ before the seed layer is deposited. -7 Below Torr and with in-situ argon plasma pre-cleaning, adsorbed moisture on the substrate and cavity is thoroughly removed, eliminating metal oxidation caused by residual oxygen in the cavity. Simultaneously, the diamond hole wall surface is activated, and the micro-oxide layer is removed, providing an ultra-high vacuum and highly active interface environment for seed layer deposition. A 13.56MHz radio frequency, combined with the substrate's uniform rotation, utilizes the random scattering characteristics of radio frequency ions to significantly improve the step coverage capability of micro-aperture, high aspect ratio through-holes. This solves the technical challenge of film fragmentation in small-hole deep-hole sputtering, ensuring the continuity and uniformity of the seed layer across the entire hole wall.
[0035] Specifically, in step S4, the seed layer comprises a Ti adhesion barrier layer and a Cu conductive seed layer deposited sequentially; the radio frequency power density of the Ti layer is 4.0–4.5 W / cm². 2 The substrate bias voltage is -40 to -45V, and the film thickness is 80 to 120 nm; the radio frequency power density of the Cu layer is 3.5 to 4.0 W / cm². 2 The substrate bias voltage is -28 to -32V, and the film thickness is 800 to 1200nm.
[0036] In the above design, by refining the seed layer structure and deposition parameters, the initial RF power density is 4.0–4.5 W / cm².2 A Ti adhesion barrier layer of 80–120 nm is deposited at a substrate bias of -40 to -45 V. The high bias enhances the ion bombardment and migration capabilities of titanium atoms, causing the titanium layer to be tightly anchored to the diamond micropore wall structure, forming a dense and stable barrier adhesion layer. Then, an RF power density of 3.5–4.0 W / cm² is applied. 2 A Cu conductive seed layer of 800–1200 nm is deposited at a substrate bias of -28 to -32 V. The low bias avoids back sputtering loss in the soft copper film, ensuring a continuous, uniform, and uninterrupted conductive seed layer between the microvia sidewalls and the bottom of the microvia. This Ti / Cu composite seed layer structure combines excellent adhesion barrier properties with conductivity properties. Furthermore, the two layers are deposited continuously without breaking the vacuum and without interface oxidation, providing a high-quality conductive connection foundation for subsequent metal paste sintering and filling.
[0037] Specifically: In step S5, the metal paste is a nano copper paste, which uses 30-50nm spherical nano copper powder as filler, has a solid content of 88-90wt%, and a room temperature viscosity of 1800-2200mPa·s.
[0038] In the above design, by limiting the composition of the metal slurry, 30-50nm spherical nano-copper powder is used as filler. The nano-copper slurry has a solid content of 88-90wt% and a room temperature viscosity of 1800-2200mPa·s. It has excellent fluidity and uniform particle dispersion, and can penetrate deep into the 50-150um micro-pores without particle bridging or void retention. This slurry formulation is specifically adapted to the penetration and filling requirements of small-diameter, high-aspect-ratio through-holes. It ensures the smooth flow of the slurry in the narrow channels during the grouting process, and also ensures the density and conductivity of the copper column after sintering, which facilitates the formation of a dense layer of metal slurry without bubbles or voids.
[0039] Specifically: In step S5, the through holes are filled using a vacuum negative pressure grouting method: the substrate is placed in a vacuum environment to purge the gas inside the through holes, with a vacuum degree of -0.095 to -0.098 MPa, and then micro positive pressure grouting is used, with a grouting pressure of 0.25 to 0.3 MPa, and pressure is maintained for 8 to 12 minutes.
[0040] In the above design, by refining the vacuum negative pressure grouting process, the substrate is placed in a vacuum environment of -0.095 to -0.098 MPa to fully expel the air trapped in the through-holes. Then, grouting is performed under a micro-positive pressure of 0.25 to 0.3 MPa and pressure is maintained for 8 to 12 minutes. Utilizing the synergistic effect of negative pressure venting and positive pressure penetration, the nano-copper paste completely fills the entire through-hole area. This process is specifically adapted for through-holes with a small aperture and high aspect ratio of 50-150 μm, effectively avoiding bubble defects caused by gas trapping inside the hole and ensuring close contact between the paste and the seed layer on the hole wall.
[0041] Specifically: In step S5, the sintering and solidification adopts a stepped heating sintering process: first, the temperature is raised to 110-130℃ and held for 20-40 minutes, then the temperature is raised to 280-300℃ and held for 70-110 minutes, so that the nano-copper particles are densified and formed.
[0042] In the above design, the temperature is first raised to 110-130℃ and held for 20-40 minutes to dry the solvent and remove trace amounts of moisture from the slurry. Then, the temperature is raised to 280-300℃ and held for 70-110 minutes to allow the nano-copper particles to fully melt, agglomerate, and densify. Finally, the slurry is cooled in the furnace. This effectively reduces the shrinkage stress of the nano-copper slurry during sintering, avoiding defects such as cracking, denting, or separation from the hole wall caused by excessive shrinkage. This ensures the dense integrity of the copper pillar structure and the tight bonding between the copper pillar and the hole wall interface, thereby ensuring the consistency and long-term reliability of the conductivity of the through-hole.
[0043] Specifically: In step S6, the planarization process adopts a double-sided chemical mechanical polishing process to remove excess sintered metal layers on the substrate surface, leaving only the solid metal pillars inside the through holes.
[0044] In the above design, the post-processing planarization step uses a double-sided chemical mechanical polishing process to remove excess sintered metal layers from the substrate surface, leaving only solid metal pillars inside the through holes. This results in a smooth and clean substrate on both sides after polishing, free of residual copper and defects caused by polishing paste embedding. This ensures both the cleanliness and flatness of the substrate surface and precisely preserves the integrity and conductivity of the metal pillars inside the through holes, resulting in a highly reliable and dense diamond interconnect substrate product.
[0045] In further detail, it should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A process for preparing small-aperture diamond-copper sintering metallization, characterized in that: The process includes the following steps: S1, processing and pre-treating through holes in the diamond substrate; S2, chemically decarburizing the through hole walls; S3, plasma decarburizing and micro-roughening treatment of the through hole walls; S4, depositing a seed layer on the through hole walls using physical vapor deposition; S5, filling the through holes with metal paste and sintering and curing; S6, planarizing the substrate surface.
2. The adaptive small-aperture diamond-copper sintering metallization preparation process according to claim 1, characterized in that: In step S1, the through-hole processing and pretreatment includes: preparing through-holes on a diamond substrate using laser processing, and then removing molten carbon slag and surface slag from the holes by airflow punching; the thickness of the diamond substrate is 200-600 μm, and the diameter of the through-hole is 50-150 μm.
3. The adaptive small-aperture diamond-copper sintering metallization preparation process according to claim 1, characterized in that: In step S2, the chemical decarbonization treatment includes: immersing the diamond substrate in an oxidizing mixed acid solution to remove the graphite layer and carbon impurities remaining from laser processing; cleaning and drying after decarbonization; the oxidizing mixed acid solution is a compound solution of 98% concentrated sulfuric acid and 68% concentrated nitric acid, with a volume ratio of 4:1 between concentrated sulfuric acid and concentrated nitric acid, an immersion temperature of 60-65°C, and an immersion time of 16-20 minutes.
4. The adapted small-aperture diamond-copper sintering metallization preparation process according to claim 1, characterized in that: In step S3, the plasma decarburization and micro-roughening treatment includes: sending the substrate after chemical decarburization into a plasma etching equipment, using oxygen-containing mixed plasma to finely decarburize the hole walls, and simultaneously forming a micro-uneven structure on the hole wall surface; the plasma etching uses a mixed gas of O2 and CF4, with a radio frequency power of 130W, an O2 flow rate of 40sccm, a CF4 flow rate of 8-12sccm, a working gas pressure of 2.8-3.2mTorr, and an etching time of 8-12min.
5. The adapted small-aperture diamond-copper sintering metallization preparation process according to claim 1, characterized in that: In step S4, the physical vapor deposition process is an RF magnetron sputtering process; before depositing the seed layer, the substrate is first vacuum baked to remove gas and evacuated to a base vacuum level of 9×10⁻⁶. -7 The substrate is pre-cleaned with in-situ argon plasma below Torr; the radio frequency frequency of the radio frequency magnetron sputtering is 13.56MHz, and the substrate rotates at a constant speed during the deposition process.
6. The adapted small-aperture diamond-copper sintering metallization preparation process according to claim 1, characterized in that: In step S4, the seed layer comprises a Ti adhesion barrier layer and a Cu conductive seed layer deposited sequentially; the radio frequency power density of the Ti layer is 4.0–4.5 W / cm². 2 The substrate bias voltage is -40 to -45V, and the film thickness is 80 to 120 nm; the radio frequency power density of the Cu layer is 3.5 to 4.0 W / cm². 2 The substrate bias voltage is -28 to -32V, and the film thickness is 800 to 1200nm.
7. The adaptive small-aperture diamond-copper sintering metallization preparation process according to claim 1, characterized in that: In step S5, the metal paste is a nano-copper paste, which uses 30-50nm spherical nano-copper powder as filler, has a solid content of 88-90wt%, and a room temperature viscosity of 1800-2200mPa·s.
8. The adaptive small-aperture diamond-copper sintering metallization preparation process according to claim 1, characterized in that: In step S5, the through holes are filled using a vacuum negative pressure grouting method: the substrate is placed in a vacuum environment to purge the gas inside the through holes, with a vacuum degree of -0.095 to -0.098 MPa, and then micro positive pressure grouting is used, with a grouting pressure of 0.25 to 0.3 MPa, and pressure is maintained for 8 to 12 minutes.
9. The adaptive small-aperture diamond-copper sintering metallization preparation process according to claim 1, characterized in that: In step S5, the sintering and solidification adopts a stepped heating sintering process: first, the temperature is raised to 110-130℃ and held for 20-40 minutes, then the temperature is raised to 280-300℃ and held for 70-110 minutes, so that the nano-copper particles are densified and formed.
10. The adaptive small-aperture diamond-copper sintering metallization preparation process according to claim 1, characterized in that: In step S6, the planarization process employs a double-sided chemical mechanical polishing process to remove excess sintered metal layers from the substrate surface, leaving only solid metal pillars inside the through holes.