A high-strength, wear-resistant stainless steel welding flux-cored wire and its preparation method

By using 316L stainless steel strip and treating it with rare earth-doped titanium dioxide and polyhydroxy compounds, the problem of insufficient strength and wear resistance of flux-cored welding wire was solved, achieving a high-strength and wear-resistant welding effect.

CN123103243APending Publication Date: 2026-11-17JIANGSU JIUZHOU NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611224473.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing flux-cored welding wires do not perform well in terms of strength and wear resistance, resulting in rapid wear and affecting the overall performance of the welded structure.

Method used

316L stainless steel strip is used as the outer sheath of the welding wire, which is filled with components such as nickel powder, chromium powder, and molybdenum powder. Rare earth doped titanium dioxide and polyhydroxy compounds are added to form a uniformly dispersed weld metal, which improves hardness and wear resistance.

Benefits of technology

It significantly improves the tensile strength and wear resistance of weld metal, extends the service life of welded parts, and ensures the high strength and wear resistance of welded structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103243A_ABST
    Figure CN123103243A_ABST
Patent Text Reader

Abstract

This invention relates to the field of welding materials, specifically to a high-strength, wear-resistant stainless steel welding flux-cored wire and its preparation method. It addresses the problem that existing flux-cored wires exhibit unsatisfactory weld metal performance in terms of strength and wear resistance, leading to rapid wear and severely impacting the overall performance of the welded structure. This preparation method, by adding rare-earth-doped titanium dioxide to the welding wire flux powder and treating it with polyhydroxy compounds, significantly improves the tensile strength of the deposited metal and reduces wear loss, substantially enhancing the strength and wear resistance of the welded joint. This ensures excellent weld performance, making it suitable for welding high-strength, wear-resistant stainless steel and improving the overall service life and reliability of the welded components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of welding materials, specifically to a high-strength, wear-resistant stainless steel welding flux-cored wire and its preparation method. Background Technology

[0002] In modern industrial applications, high-strength, wear-resistant stainless steel plays an irreplaceable role in various harsh environments. This type of material is frequently used in the manufacture of parts, mechanical components, and various equipment requiring wear and corrosion resistance. Flux-cored welding wire, as a commonly used welding material, is widely applied in the welding repair and manufacturing processes of stainless steel materials due to its advantages such as high welding efficiency, good weld quality, and low cost.

[0003] However, while existing flux-cored welding wires can improve the hardness and toughness of welding materials to some extent, their performance in terms of strength and wear resistance is not ideal, resulting in rapid wear and severely affecting the overall performance of the welded structure. Therefore, developing a high-strength, wear-resistant flux-cored welding wire for stainless steel welding and its preparation method is of significant practical importance. Summary of the Invention

[0004] In order to overcome the above-mentioned technical problems, the purpose of this invention is to provide a high-strength wear-resistant stainless steel welding flux-cored wire and its preparation method, which solves the problem that the weld metal of existing flux-cored wires does not perform well in terms of strength and wear resistance, resulting in a fast wear rate and seriously affecting the overall performance of the welded structure.

[0005] The objective of this invention can be achieved through the following technical solutions: In a first aspect, this application provides a high-strength, wear-resistant stainless steel welding wire with flux core, comprising a wire sheath and welding wire flux powder; The outer sheath of the welding wire is made of 316L stainless steel strip; The welding wire powder comprises the following components in parts by weight: 8-10 parts nickel powder, 24-28 parts chromium powder, 2.5-4.5 parts molybdenum powder, 0.8-2.2 parts manganese powder, 0.5-2.1 parts rare earth-doped titanium dioxide, 0.2-0.4 parts boron nitride, 0.4-0.5 parts tungsten carbide, 9-10 parts rutile, 0.5-1.1 parts quartz powder, 2-4 parts zircon sand, 1.5-2.5 parts albite, 0.8-1 part potassium feldspar, 0.5-0.9 parts fluorite, and 45-50 parts iron powder, for later use; The rare earth-doped titanium dioxide is prepared by the following steps: Tetrabutyl titanate and anhydrous ethanol were added to a three-necked flask equipped with a stirrer, thermometer, constant pressure dropping funnel, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred for 20-25 min at a temperature of 20-25℃ and a stirring rate of 200-300 r / min. Then, a rare earth element solution was added dropwise while stirring, with the dropping rate controlled at 1-3 drops / s. After the addition was completed, the temperature was raised to 80-90℃ and the reaction was continued with stirring for 4-10 h. After the reaction was completed, the reaction product was cooled to room temperature and then allowed to stand for 10-20 h. Then, it was placed in a vacuum drying oven and dried at a temperature of 90-100℃ for 4-6 h. After that, it was placed in a muffle furnace and calcined at a temperature of 600-700℃ for 2-3 h under nitrogen protection. Then, it was cooled with the furnace to obtain rare earth-doped titanium dioxide.

[0006] In a preferred embodiment of the present invention, the ratio of the amount of tetrabutyl titanate, anhydrous ethanol and rare earth element solution is 10 mL: 10-15 mL: 40-50 mL.

[0007] In a preferred embodiment of the present invention, the rare earth element solution is composed of lanthanum nitrate, cerium nitrate, concentrated nitric acid, deionized water, and anhydrous ethanol in a dosage ratio of 1.8-3.6g: 2.5-4.5g: 1-3mL: 20-30mL: 80-90mL.

[0008] In a preferred embodiment of the present invention, the concentrated nitric acid has a mass fraction of 66-68%.

[0009] Secondly, this application provides a method for preparing a high-strength, wear-resistant stainless steel welding flux-cored wire, comprising the following steps: Step 1: Weigh the components of the welding wire powder according to the formula; Step 2: Add the welding wire powder, polyhydroxy compound and anhydrous ethanol into a ball mill and ball mill for 6-12 hours at a ball milling rate of 300-400 r / min to obtain a ball mill slurry; Step 3: Centrifuge the ball-milled slurry, wash the precipitate with distilled water 2-3 times, then place it in a vacuum drying oven and dry it at a temperature of 60-100℃ for 10-15 hours. After that, pulverize it through a 500-1000 mesh sieve to obtain fine powder. Step 4: Fill the U-shaped welding wire sheath with refined flux powder at a filling rate of 24-26%, then seal it, and then draw it to reduce the diameter to 2mm to obtain a high-strength wear-resistant stainless steel welding wire.

[0010] In a preferred embodiment of the present invention, the ratio of the welding wire powder, the polyhydroxy compound and the anhydrous ethanol is 10g:0.5-5.5g:100-110mL.

[0011] In a preferred embodiment of the present invention, the polyhydroxy compound is prepared by the following steps: Step a1: Add mercaptopropionic acid, trimethylolpropane, hypophosphite, p-toluenesulfonic acid, and toluene to a three-necked flask equipped with a stirrer, thermometer, and gas delivery tube. Purge with nitrogen for protection and stir at 20-25°C and 200-300 r / min for 10-15 min. Then raise the temperature to 80-90°C and continue stirring for 3-5 h. After that, raise the temperature to 110-120°C and continue stirring for 6-8 h. After the reaction is complete, cool the reaction product to room temperature and pour it into distilled water. Then allow it to stand and separate into layers. Dry the organic phase with anhydrous sodium sulfate and then filter under vacuum. Remove the solvent by rotary evaporation of the filtrate to obtain the polythiol compound. Step a2: Add the polythiol compound, 1,4-butenediol, α,α-dimethoxy-α-phenylacetophenone, and tetrahydrofuran to a three-necked flask equipped with a stirrer, thermometer, and gas delivery tube. Purge with nitrogen for protection and stir the reaction at 20-25℃, a stirring rate of 200-300 r / min, and under 365 nm ultraviolet light for 20-30 min. Then, raise the temperature to 70-80℃ and continue stirring for 10-20 h. After the reaction is complete, cool the reaction product to room temperature, then filter under vacuum. Remove the solvent by rotary evaporation of the filtrate, then add it to a mixed solvent. Allow the mixture to stand and separate into layers. Dry the organic phase with anhydrous sodium sulfate, then filter under vacuum and remove the solvent by rotary evaporation of the filtrate to obtain the polyhydroxy compound.

[0012] In a preferred embodiment of the present invention, the ratio of mercaptopropionic acid, trimethylolpropane, hypophosphite, p-toluenesulfonic acid and toluene in step a1 is 40-50 mmol: 10 mmol: 0.03-0.05 g: 0.08-0.12 g: 50-60 mL.

[0013] In a preferred embodiment of the present invention, the ratio of the polythiol compound, 1,4-butenediol, α,α-dimethoxy-α-phenylacetophenone, and tetrahydrofuran in step a2 is 10 mmol: 35-40 mmol: 0.2-0.4 g: 70-80 mL.

[0014] In a preferred embodiment of the present invention, the mixed solvent in step a2 is a mixture of ethyl acetate and saturated saline solution in a volume ratio of 3-5:1.

[0015] The beneficial effects of this invention are: This invention discloses a high-strength wear-resistant stainless steel welding flux-cored wire and its preparation method. The method involves ball milling welding wire powder, a polyhydroxy compound, and anhydrous ethanol to obtain a ball mill slurry. The slurry is then centrifuged, and the precipitate is washed, dried, pulverized, and sieved to obtain a refined flux powder. This refined flux powder is then filled into the outer sheath of a U-shaped welding wire. After sealing and drawing to reduce the diameter, the high-strength wear-resistant stainless steel welding flux-cored wire is obtained. This preparation method, by adding rare-earth-doped titanium dioxide to the welding wire powder and treating it with a polyhydroxy compound, can significantly improve the tensile strength of the deposited metal and reduce wear loss, greatly enhancing the strength and wear resistance of the welded joint. This ensures excellent weld performance, making it suitable for welding high-strength wear-resistant stainless steel and improving the overall service life and reliability of the welded parts.

[0016] In the preparation of flux-cored welding wire, a rare-earth-doped titanium dioxide was first prepared by using lanthanum and cerium ions for doping, forming titanium dioxide containing rare-earth ion doping. Titanium dioxide itself has excellent hardness and wear resistance. Its nano-sized particles can be uniformly dispersed in the weld metal to form "hard points," which hinder dislocation movement and improve the hardness and wear resistance of the weld. The doping of lanthanum and cerium rare-earth elements can further improve the dispersibility of titanium dioxide and prevent its agglomeration. At the same time, rare-earth elements can combine with impurities (such as oxygen and sulfur) in the weld metal to form stable compounds, reducing the impact of impurities on weld performance and further improving wear resistance. In addition, lanthanum and cerium rare-earth elements have the effect of refining grains, which can inhibit the growth of weld grains during welding, forming a fine and uniform grain structure, reducing defects such as porosity and cracks, and significantly improving the mechanical strength of the weld.

[0017] In the process of preparing flux-cored welding wire, a polyhydroxy compound is also prepared. This is achieved through a reaction between mercaptopropionic acid and trimethylolpropane, where the carboxyl group on mercaptopropionic acid reacts with the hydroxyl group on trimethylolpropane to obtain a polythiol compound. Then, through a reaction between the polythiol compound and 1,4-butenyl glycol, the thiol group on the polythiol compound undergoes a click chemical reaction with the alkenyl group on 1,4-butenyl glycol, simultaneously introducing a large number of hydroxyl groups to obtain the polyhydroxy compound. The polyhydroxy compound contains multiple hydroxyl groups in its molecular structure, exhibiting good lubricity and dispersibility. During the ball milling process of the welding wire flux powder, it can adsorb onto the surface of each component particle, reducing inter-particle friction, preventing agglomeration of components, ensuring uniform dispersion and refinement of the welding wire flux powder, improving filling uniformity, and increasing the density of the weld metal, thus significantly improving the mechanical strength and wear resistance of the weld metal. Attached Figure Description

[0018] The invention will now be further described with reference to the accompanying drawings.

[0019] Figure 1This is a schematic diagram showing the performance test results of the flux-cored welding wire for high-strength wear-resistant stainless steel welding in this invention. Detailed Implementation

[0020] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0021] Example 1: This embodiment describes a method for preparing a high-strength, wear-resistant stainless steel welding flux-cored wire, comprising the following steps: Step S1: 40 mmol mercaptopropionic acid, 10 mmol trimethylolpropane, 0.03 g hypophosphite, 0.08 g p-toluenesulfonic acid, and 50 mL toluene were added to a three-necked flask equipped with a stirrer, thermometer, and gas delivery tube. Nitrogen gas was introduced for protection. The mixture was stirred at 20 °C and 200 r / min for 10 min. The temperature was then raised to 80 °C and the mixture was stirred for 3 h. The temperature was then raised to 110 °C and the mixture was stirred for 6 h. After the reaction was completed, the reaction product was cooled to room temperature and poured into distilled water. The mixture was then allowed to stand and separate into layers. The organic phase was dried with anhydrous sodium sulfate and then filtered under vacuum. The filtrate was evaporated by rotary evaporation to remove the solvent, yielding a polythiol compound. Step S2: 10 mmol of the polythiol compound, 35 mmol of 1,4-butenediol, 0.2 g of α,α-dimethoxy-α-phenylacetophenone, and 70 mL of tetrahydrofuran were added to a three-necked flask equipped with a stirrer, thermometer, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred for 20 min at 20 °C, a stirring rate of 200 r / min, and 365 nm ultraviolet light. The mixture was then heated to 70 °C and stirred for another 10 h. After the reaction was completed, the product was cooled to room temperature and then vacuum filtered. The solvent was removed by rotary evaporation of the filtrate. The filtrate was then added to a mixed solvent of ethyl acetate and saturated brine in a volume ratio of 3:1. The mixture was allowed to stand and separate into layers. The organic phase was dried with anhydrous sodium sulfate and then vacuum filtered. The solvent was removed by rotary evaporation of the filtrate to obtain the polyhydroxy compound. Step S3: Add 10 mL of tetrabutyl titanate and 10 mL of anhydrous ethanol to a three-necked flask equipped with a stirrer, thermometer, constant pressure dropping funnel, and gas delivery tube. Purge with nitrogen for protection and stir for 20 min at 20℃ and 200 r / min. Then, while stirring, add dropwise 40 mL of a rare earth element solution composed of lanthanum nitrate, cerium nitrate, 66% concentrated nitric acid, deionized water, and anhydrous ethanol in a ratio of 1.8 g: 2.5 g: 1 mL: 20 mL: 80 mL, controlling the dropping rate to 1 drop / s. After the addition is complete, raise the temperature to 80℃ and continue stirring for 4 h. After the reaction is complete, cool the reaction product to room temperature and let it stand for 10 h. Then, place it in a vacuum drying oven and dry at 90℃ for 4 h. Then, place it in a muffle furnace and calcine at 600℃ for 2 h under nitrogen protection. Then, cool with the furnace to obtain rare earth doped titanium dioxide. Step S4: Weigh the components of the welding wire powder according to the formula, wherein the welding wire powder comprises the following components by weight: The composition includes 8 parts nickel powder, 24 parts chromium powder, 2.5 parts molybdenum powder, 0.8 parts manganese powder, 0.5 parts rare earth-doped titanium dioxide, 0.2 parts boron nitride, 0.4 parts tungsten carbide, 9 parts rutile, 0.5 parts quartz powder, 2 parts zircon sand, 1.5 parts albite, 0.8 parts potassium feldspar, 0.5 parts fluorite, and 45 parts iron powder. Step S5: Add welding wire powder, polyhydroxy compound and anhydrous ethanol to a ball mill and ball mill for 6 hours at a ball milling rate of 300 r / min to obtain ball mill slurry; the ratio of welding wire powder, polyhydroxy compound and anhydrous ethanol is 10 g: 0.5 g: 100 mL. Step S6: Centrifuge the ball-milled slurry, wash the precipitate twice with distilled water, then place it in a vacuum drying oven and dry it at 60°C for 10 hours. After that, pulverize it through a 1000-mesh sieve to obtain fine powder. Step S7: Fill the outer sheath of the 316L stainless steel strip rolled into a U-shape with refined flux powder at a filling rate of 24%. After sealing, the wire is drawn and reduced to a diameter of 2mm to obtain a high-strength wear-resistant stainless steel welding flux-cored wire.

[0022] Example 2: This embodiment describes a method for preparing a high-strength, wear-resistant stainless steel welding flux-cored wire, comprising the following steps: Step S1: 45 mmol mercaptopropionic acid, 10 mmol trimethylolpropane, 0.04 g hypophosphite, 0.1 g p-toluenesulfonic acid, and 55 mL toluene were added to a three-necked flask equipped with a stirrer, thermometer, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred at 22 °C and 250 r / min for 12 min. The temperature was then raised to 85 °C and the mixture was stirred for 4 h. The temperature was then raised to 115 °C and the mixture was stirred for 7 h. After the reaction was completed, the reaction product was cooled to room temperature and poured into distilled water. The mixture was then allowed to stand and separate into layers. The organic phase was dried with anhydrous sodium sulfate and then filtered under vacuum. The filtrate was evaporated by rotary evaporation to remove the solvent, yielding a polythiol compound. Step S2: 10 mmol of the polythiol compound, 38 mmol of 1,4-butenediol, 0.3 g of α,α-dimethoxy-α-phenylacetophenone, and 75 mL of tetrahydrofuran were added to a three-necked flask equipped with a stirrer, thermometer, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred for 25 min at 22 °C, a stirring rate of 250 r / min, and 365 nm ultraviolet light. The mixture was then heated to 75 °C and stirred for another 15 h. After the reaction was completed, the product was cooled to room temperature and then vacuum filtered. The solvent was removed by rotary evaporation of the filtrate. The filtrate was then added to a mixed solvent of ethyl acetate and saturated brine in a volume ratio of 4:1. The mixture was allowed to stand and separate into layers. The organic phase was dried with anhydrous sodium sulfate and then vacuum filtered. The solvent was removed by rotary evaporation of the filtrate to obtain the polyhydroxy compound. Step S3: Add 10 mL of tetrabutyl titanate and 12 mL of anhydrous ethanol to a three-necked flask equipped with a stirrer, thermometer, constant pressure dropping funnel, and gas delivery tube. Purge with nitrogen for protection and stir the mixture for 22 min at 22°C and a stirring rate of 250 r / min. Then, while stirring, add dropwise 45 mL of lanthanum nitrate, cerium nitrate, 67% concentrated nitric acid, deionized water, and anhydrous ethanol in a ratio of 2.7 g: 3.5 g: 2 mL. A rare earth element solution was prepared by mixing 25 mL and 85 mL of rare earth elements. The dropping rate was controlled at 2 drops / s. After the addition was completed, the temperature was raised to 85℃ and the reaction was stirred for 7 hours. After the reaction was completed, the reaction product was cooled to room temperature and then allowed to stand for 15 hours. After that, it was placed in a vacuum drying oven and dried at 95℃ for 5 hours. Then it was placed in a muffle furnace and calcined at 650℃ for 2.5 hours under nitrogen protection. After that, it was cooled with the furnace to obtain rare earth doped titanium dioxide. Step S4: Weigh the components of the welding wire powder according to the formula, wherein the welding wire powder comprises the following components by weight: The composition includes 9 parts nickel powder, 26 parts chromium powder, 3.5 parts molybdenum powder, 1.5 parts manganese powder, 1.3 parts rare earth-doped titanium dioxide, 0.3 parts boron nitride, 0.45 parts tungsten carbide, 9.5 parts rutile, 0.8 parts quartz powder, 3 parts zircon sand, 2 parts albite, 0.9 parts potassium feldspar, 0.7 parts fluorite, and 48 parts iron powder. Step S5: Add welding wire powder, polyhydroxy compound and anhydrous ethanol to a ball mill and ball mill for 9 hours at a ball milling rate of 350 r / min to obtain ball mill slurry; the ratio of welding wire powder, polyhydroxy compound and anhydrous ethanol is 10 g: 3 g: 105 mL. Step S6: Centrifuge the ball-milled slurry, wash the precipitate twice with distilled water, then place it in a vacuum drying oven and dry it at 80°C for 12 hours. After that, pulverize it through a 1000-mesh sieve to obtain fine powder. Step S7: Fill the outer sheath of the 316L stainless steel strip rolled into a U-shape with refined flux powder at a filling rate of 25%. After sealing, the wire is drawn and reduced to a diameter of 2mm to obtain a high-strength wear-resistant stainless steel welding flux-cored wire.

[0023] Example 3: This embodiment describes a method for preparing a high-strength, wear-resistant stainless steel welding flux-cored wire, comprising the following steps: Step S1: 50 mmol mercaptopropionic acid, 10 mmol trimethylolpropane, 0.05 g hypophosphite, 0.12 g p-toluenesulfonic acid, and 60 mL toluene were added to a three-necked flask equipped with a stirrer, thermometer, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred at 25 °C and a stirring rate of 300 r / min for 15 min. The temperature was then raised to 90 °C and the mixture was stirred for 5 h. The temperature was then raised to 120 °C and the mixture was stirred for 8 h. After the reaction was completed, the reaction product was cooled to room temperature and poured into distilled water. The mixture was then allowed to stand and separate into layers. The organic phase was dried with anhydrous sodium sulfate and then filtered under vacuum. The filtrate was evaporated by rotary evaporation to remove the solvent, yielding a polythiol compound. Step S2: 10 mmol of the polythiol compound, 40 mmol of 1,4-butenediol, 0.4 g of α,α-dimethoxy-α-phenylacetophenone, and 80 mL of tetrahydrofuran were added to a three-necked flask equipped with a stirrer, thermometer, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred for 30 min at 25 °C, a stirring rate of 300 r / min, and 365 nm ultraviolet light. The mixture was then heated to 80 °C and stirred for another 20 h. After the reaction was completed, the product was cooled to room temperature and then vacuum filtered. The solvent was removed by rotary evaporation of the filtrate. The filtrate was then added to a mixed solvent of ethyl acetate and saturated brine in a volume ratio of 5:1. The mixture was allowed to stand and separate into layers. The organic phase was dried with anhydrous sodium sulfate and then vacuum filtered. The solvent was removed by rotary evaporation of the filtrate to obtain the polyhydroxy compound. Step S3: Add 10 mL of tetrabutyl titanate and 15 mL of anhydrous ethanol to a three-necked flask equipped with a stirrer, thermometer, constant pressure dropping funnel, and gas delivery tube. Purge with nitrogen for protection and stir the mixture for 25 min at 25°C and a stirring rate of 300 r / min. Then, while stirring, add dropwise 50 mL of lanthanum nitrate, cerium nitrate, 68% concentrated nitric acid, deionized water, and anhydrous ethanol in a ratio of 3.6 g: 4.5 g: 3 mL. A rare earth element solution was prepared by mixing 30 mL and 90 mL of rare earth elements. The dropping rate was controlled at 3 drops / s. After the addition was completed, the temperature was raised to 90℃ and the reaction was stirred for 10 h. After the reaction was completed, the reaction product was cooled to room temperature and then allowed to stand for 20 h. After that, it was placed in a vacuum drying oven and dried at 100℃ for 6 h. Then it was placed in a muffle furnace and calcined at 700℃ for 3 h under nitrogen protection. After that, it was cooled with the furnace to obtain rare earth doped titanium dioxide. Step S4: Weigh the components of the welding wire powder according to the formula, wherein the welding wire powder comprises the following components by weight: 10 parts nickel powder, 28 parts chromium powder, 4.5 parts molybdenum powder, 2.2 parts manganese powder, 2.1 parts rare earth-doped titanium dioxide, 0.4 parts boron nitride, 0.5 parts tungsten carbide, 10 parts rutile, 1.1 parts quartz powder, 4 parts zircon sand, 2.5 parts albite, 1 part potassium feldspar, 0.9 parts fluorite, and 50 parts iron powder; Step S5: Add welding wire powder, polyhydroxy compound and anhydrous ethanol to a ball mill and ball mill for 12 hours at a ball milling rate of 400 r / min to obtain ball mill slurry; the ratio of welding wire powder, polyhydroxy compound and anhydrous ethanol is 10 g: 5.5 g: 110 mL. Step S6: Centrifuge the ball-milled slurry, wash the precipitate three times with distilled water, then place it in a vacuum drying oven and dry it at 100℃ for 15 hours. After that, pulverize it through a 1000-mesh sieve to obtain fine powder. Step S7: Fill the outer sheath of the 316L stainless steel strip rolled into a U-shape with refined flux powder at a filling rate of 26%. After sealing, the wire is drawn and reduced to a diameter of 2mm to obtain a high-strength wear-resistant stainless steel welding flux-cored wire.

[0024] Comparative Example 1: This comparative example illustrates a method for preparing a high-strength, wear-resistant flux-cored welding wire for stainless steel welding, comprising the following steps: Step S1: Weigh the components of the welding wire powder according to the formula, wherein the welding wire powder comprises the following components by weight: 10 parts nickel powder, 28 parts chromium powder, 4.5 parts molybdenum powder, 2.2 parts manganese powder, 0.4 parts boron nitride, 0.5 parts tungsten carbide, 10 parts rutile, 1.1 parts quartz powder, 4 parts zircon sand, 2.5 parts albite, 1 part potassium feldspar, 0.9 parts fluorite, and 50 parts iron powder; Step S2: Fill the outer sheath of the 316L stainless steel strip rolled into a U-shape with welding wire powder at a filling rate of 26%. After sealing, the wire is drawn and reduced to a diameter of 2mm to obtain a high-strength wear-resistant stainless steel welding wire.

[0025] Comparative Example 2: This comparative example illustrates a method for preparing a high-strength, wear-resistant flux-cored welding wire for stainless steel welding, comprising the following steps: Step S1: Add 10 mL of tetrabutyl titanate and 15 mL of anhydrous ethanol to a three-necked flask equipped with a stirrer, thermometer, constant pressure dropping funnel, and gas delivery tube. Purge with nitrogen for protection and stir the mixture for 25 min at 25°C and a stirring rate of 300 r / min. Then, while stirring, add dropwise 50 mL of lanthanum nitrate, cerium nitrate, 68% concentrated nitric acid, deionized water, and anhydrous ethanol in a ratio of 3.6 g: 4.5 g: 3 mL. A rare earth element solution was prepared by mixing 30 mL and 90 mL of rare earth elements. The dropping rate was controlled at 3 drops / s. After the addition was completed, the temperature was raised to 90℃ and the reaction was stirred for 10 h. After the reaction was completed, the reaction product was cooled to room temperature and then allowed to stand for 20 h. After that, it was placed in a vacuum drying oven and dried at 100℃ for 6 h. Then it was placed in a muffle furnace and calcined at 700℃ for 3 h under nitrogen protection. After that, it was cooled with the furnace to obtain rare earth doped titanium dioxide. Step S2: Weigh the components of the welding wire powder according to the formula, wherein the welding wire powder comprises the following components by weight: 10 parts nickel powder, 28 parts chromium powder, 4.5 parts molybdenum powder, 2.2 parts manganese powder, 2.1 parts rare earth-doped titanium dioxide, 0.4 parts boron nitride, 0.5 parts tungsten carbide, 10 parts rutile, 1.1 parts quartz powder, 4 parts zircon sand, 2.5 parts albite, 1 part potassium feldspar, 0.9 parts fluorite, and 50 parts iron powder; Step S3: Fill the outer sheath of the 316L stainless steel strip rolled into a U-shape with welding wire powder at a filling rate of 26%. After sealing, the wire is drawn and reduced to a diameter of 2mm to obtain a high-strength wear-resistant stainless steel welding wire.

[0026] Comparative Example 3: This comparative example illustrates a method for preparing a high-strength, wear-resistant flux-cored welding wire for stainless steel welding, comprising the following steps: Step S1: 50 mmol mercaptopropionic acid, 10 mmol trimethylolpropane, 0.05 g hypophosphite, 0.12 g p-toluenesulfonic acid, and 60 mL toluene were added to a three-necked flask equipped with a stirrer, thermometer, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred at 25 °C and a stirring rate of 300 r / min for 15 min. The temperature was then raised to 90 °C and the mixture was stirred for 5 h. The temperature was then raised to 120 °C and the mixture was stirred for 8 h. After the reaction was completed, the reaction product was cooled to room temperature and poured into distilled water. The mixture was then allowed to stand and separate into layers. The organic phase was dried with anhydrous sodium sulfate and then filtered under vacuum. The filtrate was evaporated by rotary evaporation to remove the solvent, yielding a polythiol compound. Step S2: 10 mmol of the polythiol compound, 40 mmol of 1,4-butenediol, 0.4 g of α,α-dimethoxy-α-phenylacetophenone, and 80 mL of tetrahydrofuran were added to a three-necked flask equipped with a stirrer, thermometer, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred for 30 min at 25 °C, a stirring rate of 300 r / min, and 365 nm ultraviolet light. The mixture was then heated to 80 °C and stirred for another 20 h. After the reaction was completed, the product was cooled to room temperature and then vacuum filtered. The solvent was removed by rotary evaporation of the filtrate. The filtrate was then added to a mixed solvent of ethyl acetate and saturated brine in a volume ratio of 5:1. The mixture was allowed to stand and separate into layers. The organic phase was dried with anhydrous sodium sulfate and then vacuum filtered. The solvent was removed by rotary evaporation of the filtrate to obtain the polyhydroxy compound. Step S3: Weigh the components of the welding wire powder according to the formula, wherein the welding wire powder comprises the following components by weight: 10 parts nickel powder, 28 parts chromium powder, 4.5 parts molybdenum powder, 2.2 parts manganese powder, 0.4 parts boron nitride, 0.5 parts tungsten carbide, 10 parts rutile, 1.1 parts quartz powder, 4 parts zircon sand, 2.5 parts albite, 1 part potassium feldspar, 0.9 parts fluorite, and 50 parts iron powder; Step S4: Add welding wire powder, polyhydroxy compound and anhydrous ethanol to a ball mill and ball mill for 12 hours at a ball milling rate of 400 r / min to obtain ball mill slurry; the ratio of welding wire powder, polyhydroxy compound and anhydrous ethanol is 10 g: 5.5 g: 110 mL. Step S5: Centrifuge the ball-milled slurry, wash the precipitate three times with distilled water, then place it in a vacuum drying oven and dry it at 100℃ for 15 hours. After that, pulverize it through a 1000-mesh sieve to obtain fine powder. Step S6: Fill the outer sheath of the 316L stainless steel strip rolled into a U-shape with refined flux powder at a filling rate of 26%. After sealing, the wire is drawn and reduced to a diameter of 2mm to obtain a high-strength wear-resistant stainless steel welding flux-cored wire.

[0027] Comparative Example 4: This comparative example illustrates a method for preparing a high-strength, wear-resistant flux-cored welding wire for stainless steel welding, comprising the following steps: Step S1: Weigh the components of the welding wire powder according to the formula, wherein the welding wire powder comprises the following components by weight: The composition includes 10 parts nickel powder, 28 parts chromium powder, 4.5 parts molybdenum powder, 2.2 parts manganese powder, 2.1 parts titanium dioxide, 0.4 parts boron nitride, 0.5 parts tungsten carbide, 10 parts rutile, 1.1 parts quartz powder, 4 parts zircon sand, 2.5 parts albite, 1 part potassium feldspar, 0.9 parts fluorite, and 50 parts iron powder; the average particle size of the titanium dioxide is 100 nm. Step S2: Add welding wire powder and anhydrous ethanol to a ball mill and ball mill for 12 hours at a ball milling rate of 400 r / min to obtain a ball mill slurry; the ratio of welding wire powder to anhydrous ethanol is 10 g: 5.5 g: 110 mL. Step S3: Centrifuge the ball-milled slurry, wash the precipitate three times with distilled water, then place it in a vacuum drying oven and dry it at 100℃ for 15 hours. After that, pulverize it through a 1000-mesh sieve to obtain fine powder. Step S4: Fill the outer sheath of the 316L stainless steel strip rolled into a U-shape with refined flux powder at a filling rate of 26%. After sealing, the wire is drawn and reduced to a diameter of 2mm to obtain a high-strength wear-resistant stainless steel welding flux-cored wire.

[0028] Performance testing The high-strength wear-resistant stainless steel welding flux-cored wires used in Examples 1-3 and Comparative Examples 1-4 were subjected to gas metal arc welding (GMAW) with C4 steel plate as the base material. Welding parameters were: welding current 190A, arc voltage 28V, welding speed 10m / h, and a nitrogen-argon mixed gas flow rate of 1L / min. The deposited metal was then subjected to performance testing, with tensile strength measured according to GB / T... Test 17853-2018: The wear resistance test was conducted using a wheel wear tester. The wear sample size was 60×30×6mm, the rubber wheel speed was 250r / min, the rubber wheel diameter was 150mm, the rubber wheel Shore hardness was 60, the load was 100N, and the abrasive was 50-mesh quartz sand. The wear loss was measured after 2000r of wear. The wear loss was calculated as follows: the weight G0 of the sample was measured using an analytical balance before wear, and the sample was washed and dried after wear, and the weight G1 after wear was measured. The difference between the two was the wear loss.

[0029] Test results are as follows Figure 1 As shown, see reference Figure 1 Based on the data, a comparison between Examples 1-3 and Comparative Examples 1-4 shows that the deposited metal of the flux-cored wire of this application has high tensile strength and low wear loss, indicating that the flux-cored wire of this application has high strength and wear resistance.

[0030] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0031] The above description is merely an example and illustration of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described or use similar methods to replace them, as long as they do not deviate from the invention or exceed the scope defined in this application, they should all fall within the protection scope of the present invention.

Claims

1. A high-strength, wear-resistant flux-cored welding wire for welding stainless steel, characterized in that, Including the outer sheath of the welding wire and the flux powder; The outer sheath of the welding wire is made of 316L stainless steel strip; The welding wire powder comprises the following components in parts by weight: 8-10 parts nickel powder, 24-28 parts chromium powder, 2.5-4.5 parts molybdenum powder, 0.8-2.2 parts manganese powder, 0.5-2.1 parts rare earth-doped titanium dioxide, 0.2-0.4 parts boron nitride, 0.4-0.5 parts tungsten carbide, 9-10 parts rutile, 0.5-1.1 parts quartz powder, 2-4 parts zircon sand, 1.5-2.5 parts albite, 0.8-1 part potassium feldspar, 0.5-0.9 parts fluorite, and 45-50 parts iron powder, for later use; The rare earth-doped titanium dioxide is prepared by the following steps: The reaction mixture of tetrabutyl titanate and anhydrous ethanol was stirred, and then a rare earth element solution was added dropwise while stirring was continued. After the reaction was completed, the reaction product was cooled, then allowed to stand, dried, and calcined, and then cooled in the furnace to obtain rare earth-doped titanium dioxide.

2. The high-strength wear-resistant stainless steel welding flux-cored wire according to claim 1, characterized in that, The ratio of the amount of tetrabutyl titanate, anhydrous ethanol, and rare earth element solution is 10 mL: 10-15 mL: 40-50 mL.

3. The high-strength wear-resistant stainless steel welding flux-cored wire according to claim 1, characterized in that, The rare earth element solution is a mixture of lanthanum nitrate, cerium nitrate, concentrated nitric acid, deionized water, and anhydrous ethanol in a ratio of 1.8-3.6g: 2.5-4.5g: 1-3mL: 20-30mL: 80-90mL; the concentrated nitric acid has a mass fraction of 66-68%.

4. A method for preparing a high-strength, wear-resistant stainless steel welding flux-cored wire, characterized in that, The method for preparing the high-strength, wear-resistant stainless steel welding wire as described in any one of claims 1-3 comprises the following steps: Step 1: Weigh the components of the welding wire powder according to the formula; Step 2: Add the welding wire powder, polyhydroxy compound and anhydrous ethanol into a ball mill and ball mill for 6-12 hours at a ball milling rate of 300-400 r / min to obtain a ball mill slurry; Step 3: Centrifuge the ball-milled slurry, wash the precipitate with distilled water 2-3 times, then place it in a vacuum drying oven and dry it at a temperature of 60-100℃ for 10-15 hours. After that, pulverize it through a 500-1000 mesh sieve to obtain fine powder. Step 4: Fill the U-shaped welding wire sheath with refined flux powder at a filling rate of 24-26%, then seal it, and then draw it to reduce the diameter to 2mm to obtain a high-strength wear-resistant stainless steel welding wire.

5. The method for preparing a high-strength wear-resistant stainless steel welding flux-cored wire according to claim 4, characterized in that, The ratio of the welding wire powder, polyhydroxy compound, and anhydrous ethanol is 10g:0.5-5.5g:100-110mL.

6. The method for preparing a high-strength wear-resistant stainless steel welding flux-cored wire according to claim 4, characterized in that, The polyhydroxy compound was prepared by the following steps: Step a1: Mercaptopropionic acid, trimethylolpropane, hypophosphite, p-toluenesulfonic acid and toluene were stirred and reacted. After the reaction was completed, the reaction product was cooled and then poured into distilled water. After standing and separating the layers, the organic phase was dried and then filtered under vacuum. The filtrate was then evaporated by rotary evaporation to obtain the polythiol compound. Step a2: The polythiol compound, 1,4-butenediol, α,α-dimethoxy-α-phenylacetophenone, and tetrahydrofuran were stirred and reacted. After the reaction was completed, the reaction product was cooled, then vacuum filtered, the filtrate was rotary evaporated, and then added to a mixed solvent. After standing and separating the layers, the organic phase was dried, then vacuum filtered, and the filtrate was rotary evaporated to obtain the polyhydroxy compound.

7. The method for preparing a high-strength wear-resistant stainless steel welding flux-cored wire according to claim 6, characterized in that, The ratio of mercaptopropionic acid, trimethylolpropane, hypophosphite, p-toluenesulfonic acid, and toluene in step a1 is 40-50 mmol: 10 mmol: 0.03-0.05 g: 0.08-0.12 g: 50-60 mL.

8. The method for preparing a high-strength wear-resistant stainless steel welding flux-cored wire according to claim 6, characterized in that, The ratio of the polythiol compound, 1,4-butenediol, α,α-dimethoxy-α-phenylacetophenone, and tetrahydrofuran in step a2 is 10 mmol: 35-40 mmol: 0.2-0.4 g: 70-80 mL.

9. The method for preparing a high-strength wear-resistant stainless steel welding flux-cored wire according to claim 6, characterized in that, The mixed solvent in step a2 is a mixture of ethyl acetate and saturated saline solution in a volume ratio of 3-5:1.