A magnesium-aluminum dissimilar metal ultrasonic brazing filler metal, its preparation method, and the brazed joint thereof.

By using Zn-Ag-Cu alloy brazing filler metal and ultrasonic-assisted brazing technology, the problem of welding magnesium alloys and aluminum alloys has been solved, achieving high-strength and high-precision connections, avoiding the formation of brittle compounds, and reducing production costs.

CN123103247APending Publication Date: 2026-11-17CHINA NAT PETROLEUM CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510633923.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Welding dissimilar metals such as magnesium alloys and aluminum alloys is difficult due to their susceptibility to oxidation and the formation of brittle intermetallic compounds. Existing brazing techniques suffer from cumbersome processes, high costs, and poor weld quality.

Method used

Using a Zn-Ag-Cu alloy as the brazing filler metal, and employing an ultrasonic-assisted brazing method, direct contact between magnesium and aluminum elements is avoided, forming a solid solution metallurgical bond that ensures a high-strength and high-dimensional-precision connection.

Benefits of technology

This technology achieves a high-performance metallurgical bond between magnesium alloys and aluminum alloys, avoids the formation of brittle intermetallic compounds, improves the strength and toughness of the welded joint, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103247A_ABST
    Figure CN123103247A_ABST
Patent Text Reader

Abstract

This invention relates to a magnesium-aluminum dissimilar metal ultrasonic brazing filler metal, its preparation method, and the brazed joint. The filler metal comprises (84 wt.%–92 wt.%) Zn–(3 wt.%–6 wt.%) Ag–(5 wt.%–10 wt.%) Cu. This filler metal can form a high-performance metallurgical bonding interface with the base materials on both sides during the welding process of magnesium alloy and aluminum alloy, while effectively preventing direct contact between magnesium and aluminum elements to form brittle intermetallic compounds, thus achieving a reliable connection between magnesium alloy and aluminum alloy with high strength and high dimensional accuracy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of non-ferrous metal brazing technology, specifically to a magnesium-aluminum dissimilar metal ultrasonic brazing filler metal, its preparation method, and the brazed joint. Background Technology

[0002] With the increasing adoption of lightweight strategies for oil and gas equipment in major oilfields, the application of high-strength, low-density metallic structural materials in oil and gas tools and equipment is becoming more widespread, such as titanium alloy drill pipes and tubing, aluminum alloy drill pipes, packers, fracturing balls, and magnesium alloy bridge plugs. Magnesium and aluminum alloys, in particular, possess characteristics such as low density, high specific strength, and high specific stiffness, making their application prospects in the oil and gas tools and equipment field increasingly broad. Due to the differences in performance characteristics and advantages between magnesium and aluminum alloys, such as elongation, absolute strength, and dissolution process, composite structures combining magnesium and aluminum alloys may be necessary in applications such as well completion tools. Therefore, combining magnesium, aluminum, and their alloys into composite structures is essential. Magnesium alloys, due to their extremely reactive chemical properties, are among the most difficult metal materials to weld, and welding dissimilar metals containing magnesium alloys is even more challenging. The main problems in magnesium-aluminum dissimilar metal welding are that the magnesium alloy base material is highly susceptible to oxidation, and the high thermal conductivity of aluminum alloys easily leads to cracks, porosity, or other welding defects. Furthermore, magnesium alloys are chemically highly reactive. If conventional non-ferrous metal brazing filler metals are used for brazing, the contact between aluminum and magnesium elements in the liquid filler metal during the brazing process easily generates a large amount of brittle intermetallic compounds, resulting in the inability to obtain high-performance brazed joints. This significantly reduces the mechanical properties of the welded joint. The main techniques for magnesium-aluminum welding include vacuum diffusion welding, friction stir welding, laser welding, TIG welding, and brazing. Among these processes, vacuum diffusion welding can be used to join metals whose liquid phases are immiscible and easily form intermetallic compounds, but the diffusion welding time is too long and the scrap rate is high. Friction stir welding is a common method for joining dissimilar metals, but it has very high requirements for sample size, leading to significant limitations in its application. In addition, in friction stir welding of magnesium and aluminum, direct contact between magnesium and aluminum elements in a small area can lead to the formation of a large amount of brittle intermetallic compounds. TIG welding is widely used for joining similar and dissimilar non-ferrous metals, but the liquid phase region of the base material is relatively large during the welding process. If used for joining dissimilar metals such as magnesium and aluminum, it is easy to generate a large amount of brittle intermetallic compounds in the liquid phase region. Compared to other welding techniques, brazing is not limited by the shape and size of the base material, and the welding temperature is low, making it suitable for welding complex and precision structural components such as blind pipes. After brazing, the deformation of the base material is small, and the dimensional control accuracy is high. Therefore, brazing is commonly used for joining magnesium alloys, aluminum alloys, and other heat-sensitive materials.

[0003] Chinese patent application CN 116652314 A discloses a method for brazing dissimilar metals of magnesium and aluminum, comprising the following steps: nickel plating of a magnesium alloy base material, followed by ultrasonic-assisted brazing of the nickel-plated magnesium alloy base material with an aluminum alloy base material after removing the oxide layer and impurities using a brazing filler metal; wherein the thickness of the nickel plating layer in the joint after ultrasonic-assisted brazing is 7.5–20 μm, the magnesium alloy base material is AZ31 magnesium alloy, and the aluminum alloy base material is 6061 aluminum alloy; the brazing filler metal is Sn 96.5 wt.% - Ag 3 wt.% - Cu 0.5 wt.%. This brazing filler metal has the following problems: nickel plating of the magnesium alloy base material is required before welding, increasing the complexity of the process and production costs; the main material of the brazing filler metal is Sn, which has low strength, significantly limiting the guarantee of the strength of the welded joint.

[0004] The invention patent with publication number CN105562956A discloses a brazing filler metal suitable for brazing magnesium-aluminum dissimilar alloys and its preparation method. The brazing filler metal is (25~35)Mg-(25~35)Al-(20~30)Zn-(20~30)Sn. The preparation method includes the following steps: (1) preparing raw materials: taking each component metal according to the proportion and putting it into a crucible; (2) melting: placing the crucible into a vacuum furnace, evacuating the furnace, introducing argon gas, setting the furnace temperature, holding the temperature for 30min~2h, and then cooling it to room temperature with the furnace to obtain the filler metal. The brazing filler metal has the following problem: the filler metal contains a large amount of Al element, which will cause a large amount of brittle intermetallic compound Mg to be generated in the brazing weld. 17 Al 12 This severely deteriorates the mechanical properties of the brazed joint. Summary of the Invention

[0005] In order to solve one or more technical problems existing in the prior art, the present invention provides a magnesium-aluminum dissimilar metal ultrasonic brazing filler metal, its preparation method and brazing joint.

[0006] Specifically, the following technical solutions are included:

[0007] In a first aspect, a magnesium-aluminum dissimilar metal ultrasonic brazing filler metal is provided, the filler metal comprising (84wt.% to 92wt.%)Zn-(3wt.% to 6wt.%)Ag-(5wt.% to 10wt.%)Cu.

[0008] The first aspect provides a magnesium-aluminum dissimilar metal ultrasonic brazing filler metal, which can form a high-performance metallurgical bonding interface with the base materials on both sides during the welding process of magnesium alloy and aluminum alloy. At the same time, it effectively avoids the direct contact between magnesium and aluminum elements to form brittle intermetallic compounds, thus achieving a reliable connection between magnesium alloy and aluminum alloy with high strength and high dimensional accuracy.

[0009] In conjunction with the first aspect, it should be noted that the preferred composition of the brazing filler metal of the present invention is 91 wt.% Zn - 4 wt.% Ag - 5 wt.% Cu.

[0010] In conjunction with the first aspect, it should be noted that the preferred composition of the brazing filler metal of the present invention is 86 wt.% Zn - 4 wt.% Ag - 10 wt.% Cu.

[0011] In conjunction with the first aspect, it should be noted that the solder composition of the present invention may be 90.5 wt.% Zn-4.5 wt.% Ag-5 wt.% Cu.

[0012] In conjunction with the first aspect, it should be noted that the solder of the present invention may have a composition of 85.5 wt.% Zn-4.5 wt.% Ag-10 wt.% Cu.

[0013] In conjunction with the first aspect, it should be noted that the solder of the present invention may have a composition of 90 wt.% Zn-5 wt.% Ag-5 wt.% Cu.

[0014] In conjunction with the first aspect, it should be noted that the solder of the present invention may have a composition of 85 wt.% Zn-5 wt.% Ag-10 wt.% Cu.

[0015] In conjunction with the first aspect, it should be noted that the solder composition of the present invention may be 89.5 wt.% Zn-5.5 wt.% Ag-5 wt.% Cu.

[0016] In conjunction with the first aspect, it should be noted that the solder of the present invention may have a composition of 84.5 wt.% Zn-5.5 wt.% Ag-10 wt.% Cu.

[0017] In conjunction with the first aspect, it should be noted that the solder of the present invention may have a composition of 89 wt.% Zn-6 wt.% Ag-5 wt.% Cu.

[0018] In conjunction with the first aspect, it should be noted that the solder of the present invention may have a composition of 84 wt.% Zn-6 wt.% Ag-10 wt.% Cu.

[0019] In the first aspect of this invention, the brazing filler metal uses Zn as the main alloying element of the magnesium-aluminum alloy brazing filler metal. From the Mg-Zn and Al-Zn phase diagrams, it can be inferred that Zn, Mg, and Al all have a wide range of solid solution formation content. Solid solution-type metallurgical bonding at the interface of different metals is the most reliable interfacial bonding method, achieving excellent interfacial bonding strength. Ag is used as the first auxiliary element of the magnesium-aluminum alloy brazing filler metal. Ag is one of the most commonly used alloying elements in non-ferrous metal brazing operations. Adding an appropriate amount of Ag to the brazing filler metal significantly improves its fluidity and wettability, while also improving weld toughness and corrosion resistance to a certain extent. Using Cu as the second auxiliary element in magnesium-aluminum alloy brazing filler metal, it can be deduced from the Mg-Cu and Al-Cu phase diagrams that, through a reasonable element content ratio, Mg and Al can form Mg-Cu solid solutions and Al-Cu solid solutions respectively, which can effectively avoid direct contact between Mg and Al. At the same time, Ag, Cu and Zn form a ternary alloy, which has a significant solid solution strengthening effect, thus establishing the necessary conditions for ensuring good strength of the brazed joint.

[0020] Secondly, the present invention provides a method for preparing ultrasonic brazing filler metal for magnesium-aluminum dissimilar metals, comprising the following steps:

[0021] S1, set the furnace temperature of the induction melting furnace to the first set temperature, take the metal raw materials of each component of the prepared brazing filler metal according to the proportion, first add pure silver and pure copper to the melting container of the induction melting furnace, and keep it warm for the first set time.

[0022] S2, then add pure zinc to the melting container, keep it at the temperature for a second set time, then remove the melting container from the furnace and cool it to room temperature to complete the preparation of the brazing filler metal.

[0023] In the second aspect of the present invention, pure copper and pure silver are smelted first, and then pure zinc is added. This avoids the loss of Zn element and contamination of the equipment cavity caused by the high smelting temperature, the low melting point of pure zinc, and the easy volatilization at high temperatures when smelting the three raw materials at the same time.

[0024] In conjunction with the second aspect, it should be noted that the furnace temperature of the induction melting furnace is set to 900℃~1100℃.

[0025] In a second aspect of the present invention, the furnace temperature of the induction melting furnace, i.e., the first set temperature, can be selected as 900℃, 910℃, 920℃, 930℃, 940℃, 950℃, 960℃, 970℃, 980℃, 990℃, 1000℃, 1010℃, 1020℃, 1030℃, 1040℃, 1050℃, 1060℃, 1070℃, 1080℃, 1090℃, or 1100℃.

[0026] In conjunction with the second aspect, the induction melting furnace is an optional induction melting furnace. The specifications of the induction melting furnace can be greater than 10kg or less than 10kg, with a 10kg induction melting furnace being preferred.

[0027] In conjunction with the second aspect, it should be noted that the first set time is 3 to 8 minutes; the second set time is 2 to 5 minutes.

[0028] In a second aspect of the present invention, the first set time can be selected as 3 min, 4 min, 5 min, 6 min, 7 min, or 8 min. The second set time can be selected as 2 min, 3 min, 4 min, or 5 min.

[0029] In conjunction with the second aspect, it should be noted that the smelting container is a corundum crucible.

[0030] Thirdly, the present invention also provides a brazed joint, comprising an aluminum alloy base material and a magnesium alloy base material, wherein the aluminum alloy base material and the magnesium alloy base material are welded using the above-mentioned magnesium-aluminum dissimilar metal ultrasonic brazing filler metal and an ultrasonic-assisted brazing method.

[0031] The brazed joint provided in the third aspect is made of 6063 aluminum alloy base material and AZ31B magnesium alloy base material.

[0032] Optionally, in the brazed joint provided by the third aspect, one end of the aluminum alloy base material overlaps with one end of the magnesium alloy base material, and the overlap forms a weld seam.

[0033] Specifically, the overlap length of the aluminum alloy base material and the magnesium alloy base material can be 8 to 15 mm, preferably 10 mm. Attached Figure Description

[0034] Figure 1 The image shows the microstructure of the solder alloy of the present invention with a composition of 91 wt.% Zn-4 wt.% Ag-5 wt.% Cu.

[0035] Figure 2 This is a microstructure diagram of the weld obtained using a brazing filler metal with a composition of 91 wt.% Zn-4 wt.% Ag-5 wt.% Cu in this invention.

[0036] Figure 3 This is a microstructure diagram of the solder alloy of the present invention with a composition of 86 wt.% Zn-4 wt.% Ag-10 wt.% Cu;

[0037] Figure 4 This is a microstructure diagram of the weld obtained using a brazing filler metal with a composition of 86 wt.% Zn-4 wt.% Ag-10 wt.% Cu in this invention.

[0038] Figure 5 This is a schematic diagram of the overlapping structure of the aluminum alloy base material and the magnesium alloy base material of the present invention. Figure 1 ;

[0039] Figure 6 This is a schematic diagram of the overlapping structure of the aluminum alloy base material and the magnesium alloy base material of the present invention. Figure 2 ;

[0040] Figure 7 This is a schematic diagram of the welding process between the aluminum alloy base material and the magnesium alloy base material of the present invention. Figure 1 ;

[0041] Figure 8 This is a schematic diagram of the welding process between the aluminum alloy base material and the magnesium alloy base material of the present invention. Figure 2 .

[0042] The attached diagram lists the components represented by each number as follows:

[0043] 1. Aluminum alloy base material; 2. Magnesium alloy base material; 3. Brazing joint; 4. Molten brazing filler metal; 5. Induction heat source; 6. Ultrasonic vibrating head. Detailed Implementation

[0044] The principles and features of the present invention are described below with reference to the accompanying drawings. The examples given are only for explaining the present invention and are not intended to limit the scope of the present invention.

[0045] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.

[0046] Unless otherwise specified, all materials and reagents used in the following examples are commercially available.

[0047] Example 1

[0048] The magnesium-aluminum dissimilar metal ultrasonic brazing filler metal of this embodiment comprises 91wt.%Zn-4wt.%Ag-5wt.%Cu.

[0049] This invention provides a method for preparing ultrasonic brazing filler metal for magnesium-aluminum dissimilar metals, comprising the following steps:

[0050] S1, set the furnace temperature of the 10kg induction melting furnace to 1000℃, take the metal raw materials of each component of the prepared brazing filler metal according to the proportion, first add pure silver and pure copper to the melting container of the induction melting furnace, and keep it at the temperature for 5 minutes; wherein, the melting container is a corundum crucible.

[0051] S2, then add pure zinc to the melting container, keep it at a constant temperature for 3 minutes, then remove the melting container from the furnace and cool it to room temperature to complete the preparation of the brazing filler metal.

[0052] A brazed joint 3 in this embodiment includes an aluminum alloy base material 1 and a magnesium alloy base material 2. The aluminum alloy base material and the magnesium alloy base material are welded using the above-mentioned magnesium-aluminum dissimilar metal ultrasonic brazing filler metal and ultrasonic-assisted brazing method.

[0053] Optionally, the aluminum alloy base material is 6063 aluminum alloy base material, and the magnesium alloy base material is AZ31B magnesium alloy base material. One end of the aluminum alloy base material overlaps with one end of the magnesium alloy base material, and a weld seam is formed at the overlap.

[0054] Example 2

[0055] This embodiment provides a magnesium-aluminum dissimilar metal ultrasonic brazing filler metal comprising 86 wt.% Zn, 4 wt.% Ag, and 10 wt.% Cu.

[0056] This invention provides a method for preparing ultrasonic brazing filler metal for magnesium-aluminum dissimilar metals, comprising the following steps:

[0057] S1, set the furnace temperature of the 10kg induction melting furnace to 1000℃, take the metal raw materials of each component of the prepared brazing filler metal according to the proportion, first add pure silver and pure copper to the melting container of the induction melting furnace, and keep it at the temperature for 5 minutes; wherein, the melting container is a corundum crucible.

[0058] S2, then add pure zinc to the melting container, keep it at a constant temperature for 3 minutes, then remove the melting container from the furnace and cool it to room temperature to complete the preparation of the brazing filler metal.

[0059] A brazed joint 3 in this embodiment includes an aluminum alloy base material 1 and a magnesium alloy base material 2. The aluminum alloy base material and the magnesium alloy base material are welded using the above-mentioned magnesium-aluminum dissimilar metal ultrasonic brazing filler metal and ultrasonic-assisted brazing method.

[0060] Optionally, the aluminum alloy base material is 6063 aluminum alloy base material, and the magnesium alloy base material is AZ31B magnesium alloy base material. One end of the aluminum alloy base material overlaps with one end of the magnesium alloy base material, and a weld seam is formed at the overlap.

[0061] Example 3

[0062] The magnesium-aluminum dissimilar metal ultrasonic brazing filler metal of this embodiment comprises 90.5 wt.% Zn-4.5 wt.% Ag-5 wt.% Cu.

[0063] This invention provides a method for preparing ultrasonic brazing filler metal for magnesium-aluminum dissimilar metals, comprising the following steps:

[0064] S1, set the furnace temperature of the 10kg induction melting furnace to 1000℃, take the metal raw materials of each component of the prepared brazing filler metal according to the proportion, first add pure silver and pure copper to the melting container of the induction melting furnace, and keep it at the temperature for 5 minutes; wherein, the melting container is a corundum crucible.

[0065] S2, then add pure zinc to the melting container, keep it at a constant temperature for 3 minutes, then remove the melting container from the furnace and cool it to room temperature to complete the preparation of the brazing filler metal.

[0066] A brazed joint 3 in this embodiment includes an aluminum alloy base material 1 and a magnesium alloy base material 2. The aluminum alloy base material and the magnesium alloy base material are welded using the above-mentioned magnesium-aluminum dissimilar metal ultrasonic brazing filler metal and ultrasonic-assisted brazing method.

[0067] Optionally, the aluminum alloy base material is 6063 aluminum alloy base material, and the magnesium alloy base material is AZ31B magnesium alloy base material. One end of the aluminum alloy base material overlaps with one end of the magnesium alloy base material, and a weld seam is formed at the overlap.

[0068] Example 4

[0069] The magnesium-aluminum dissimilar metal ultrasonic brazing filler metal of this embodiment comprises 85.5 wt.% Zn-4.5 wt.% Ag-10 wt.% Cu.

[0070] This invention provides a method for preparing ultrasonic brazing filler metal for magnesium-aluminum dissimilar metals, comprising the following steps:

[0071] S1, set the furnace temperature of the 10kg induction melting furnace to 1000℃, take the metal raw materials of each component of the prepared brazing filler metal according to the proportion, first add pure silver and pure copper to the melting container of the induction melting furnace, and keep it at the temperature for 5 minutes; wherein, the melting container is a corundum crucible.

[0072] S2, then add pure zinc to the melting container, keep it at a constant temperature for 3 minutes, then remove the melting container from the furnace and cool it to room temperature to complete the preparation of the brazing filler metal.

[0073] A brazed joint 3 in this embodiment includes an aluminum alloy base material 1 and a magnesium alloy base material 2. The aluminum alloy base material and the magnesium alloy base material are welded using the above-mentioned magnesium-aluminum dissimilar metal ultrasonic brazing filler metal and ultrasonic-assisted brazing method.

[0074] Optionally, the aluminum alloy base material is 6063 aluminum alloy base material, and the magnesium alloy base material is AZ31B magnesium alloy base material. One end of the aluminum alloy base material overlaps with one end of the magnesium alloy base material, and a weld seam is formed at the overlap.

[0075] Example 5

[0076] This embodiment provides a magnesium-aluminum dissimilar metal ultrasonic brazing filler metal comprising 90 wt.% Zn, 5 wt.% Ag, and 5 wt.% Cu.

[0077] This invention provides a method for preparing ultrasonic brazing filler metal for magnesium-aluminum dissimilar metals, comprising the following steps:

[0078] S1, set the furnace temperature of the 10kg induction melting furnace to 1000℃, take the metal raw materials of each component of the prepared brazing filler metal according to the proportion, first add pure silver and pure copper to the melting container of the induction melting furnace, and keep it at the temperature for 5 minutes; wherein, the melting container is a corundum crucible.

[0079] S2, then add pure zinc to the melting container, keep it at a constant temperature for 3 minutes, then remove the melting container from the furnace and cool it to room temperature to complete the preparation of the brazing filler metal.

[0080] A brazed joint 3 in this embodiment includes an aluminum alloy base material 1 and a magnesium alloy base material 2. The aluminum alloy base material and the magnesium alloy base material are welded using the above-mentioned magnesium-aluminum dissimilar metal ultrasonic brazing filler metal and ultrasonic-assisted brazing method.

[0081] Optionally, the aluminum alloy base material is 6063 aluminum alloy base material, and the magnesium alloy base material is AZ31B magnesium alloy base material. One end of the aluminum alloy base material overlaps with one end of the magnesium alloy base material, and a weld seam is formed at the overlap.

[0082] Example 6

[0083] This embodiment provides a magnesium-aluminum dissimilar metal ultrasonic brazing filler metal comprising 85wt.%Zn-5wt.%Ag-10wt.%Cu.

[0084] This invention provides a method for preparing ultrasonic brazing filler metal for magnesium-aluminum dissimilar metals, comprising the following steps:

[0085] S1, set the furnace temperature of the 10kg induction melting furnace to 1000℃, take the metal raw materials of each component of the prepared brazing filler metal according to the proportion, first add pure silver and pure copper to the melting container of the induction melting furnace, and keep it at the temperature for 5 minutes; wherein, the melting container is a corundum crucible.

[0086] S2, then add pure zinc to the melting container, keep it at a constant temperature for 3 minutes, then remove the melting container from the furnace and cool it to room temperature to complete the preparation of the brazing filler metal.

[0087] A brazed joint 3 in this embodiment includes an aluminum alloy base material 1 and a magnesium alloy base material 2. The aluminum alloy base material and the magnesium alloy base material are welded using the above-mentioned magnesium-aluminum dissimilar metal ultrasonic brazing filler metal and ultrasonic-assisted brazing method.

[0088] Optionally, the aluminum alloy base material is 6063 aluminum alloy base material, and the magnesium alloy base material is AZ31B magnesium alloy base material. One end of the aluminum alloy base material overlaps with one end of the magnesium alloy base material, and a weld seam is formed at the overlap.

[0089] Example 7

[0090] The magnesium-aluminum dissimilar metal ultrasonic brazing filler metal of this embodiment comprises 89.5 wt.% Zn-5.5 wt.% Ag-5 wt.% Cu.

[0091] This invention provides a method for preparing ultrasonic brazing filler metal for magnesium-aluminum dissimilar metals, comprising the following steps:

[0092] S1, set the furnace temperature of the 10kg induction melting furnace to 1000℃, take the metal raw materials of each component of the prepared brazing filler metal according to the proportion, first add pure silver and pure copper to the melting container of the induction melting furnace, and keep it at the temperature for 5 minutes; wherein, the melting container is a corundum crucible.

[0093] S2, then add pure zinc to the melting container, keep it at a constant temperature for 3 minutes, then remove the melting container from the furnace and cool it to room temperature to complete the preparation of the brazing filler metal.

[0094] A brazed joint 3 in this embodiment includes an aluminum alloy base material 1 and a magnesium alloy base material 2. The aluminum alloy base material and the magnesium alloy base material are welded using the above-mentioned magnesium-aluminum dissimilar metal ultrasonic brazing filler metal and ultrasonic-assisted brazing method.

[0095] Optionally, the aluminum alloy base material is 6063 aluminum alloy base material, and the magnesium alloy base material is AZ31B magnesium alloy base material. One end of the aluminum alloy base material overlaps with one end of the magnesium alloy base material, and a weld seam is formed at the overlap.

[0096] Example 8

[0097] The magnesium-aluminum dissimilar metal ultrasonic brazing filler metal of this embodiment comprises 89-84.5 wt.% Zn-5.5 wt.% Ag-10 wt.% Cu.

[0098] This invention provides a method for preparing ultrasonic brazing filler metal for magnesium-aluminum dissimilar metals, comprising the following steps:

[0099] S1, set the furnace temperature of the 10kg induction melting furnace to 1000℃, take the metal raw materials of each component of the prepared brazing filler metal according to the proportion, first add pure silver and pure copper to the melting container of the induction melting furnace, and keep it at the temperature for 5 minutes; wherein, the melting container is a corundum crucible.

[0100] S2, then add pure zinc to the melting container, keep it at a constant temperature for 3 minutes, then remove the melting container from the furnace and cool it to room temperature to complete the preparation of the brazing filler metal.

[0101] A brazed joint 3 in this embodiment includes an aluminum alloy base material 1 and a magnesium alloy base material 2. The aluminum alloy base material and the magnesium alloy base material are welded using the above-mentioned magnesium-aluminum dissimilar metal ultrasonic brazing filler metal and ultrasonic-assisted brazing method.

[0102] Optionally, the aluminum alloy base material is 6063 aluminum alloy base material, and the magnesium alloy base material is AZ31B magnesium alloy base material. One end of the aluminum alloy base material overlaps with one end of the magnesium alloy base material, and a weld seam is formed at the overlap.

[0103] Example 9

[0104] The magnesium-aluminum dissimilar metal ultrasonic brazing filler metal of this embodiment comprises 89wt.%Zn-6wt.%Ag-5wt.%Cu.

[0105] This invention provides a method for preparing ultrasonic brazing filler metal for magnesium-aluminum dissimilar metals, comprising the following steps:

[0106] S1, set the furnace temperature of the 10kg induction melting furnace to 1000℃, take the metal raw materials of each component of the prepared brazing filler metal according to the proportion, first add pure silver and pure copper to the melting container of the induction melting furnace, and keep it at the temperature for 5 minutes; wherein, the melting container is a corundum crucible.

[0107] S2, then add pure zinc to the melting container, keep it at a constant temperature for 3 minutes, then remove the melting container from the furnace and cool it to room temperature to complete the preparation of the brazing filler metal.

[0108] A brazed joint 3 in this embodiment includes an aluminum alloy base material 1 and a magnesium alloy base material 2. The aluminum alloy base material and the magnesium alloy base material are welded using the above-mentioned magnesium-aluminum dissimilar metal ultrasonic brazing filler metal and ultrasonic-assisted brazing method.

[0109] Optionally, the aluminum alloy base material is 6063 aluminum alloy base material, and the magnesium alloy base material is AZ31B magnesium alloy base material. One end of the aluminum alloy base material overlaps with one end of the magnesium alloy base material, and a weld seam is formed at the overlap.

[0110] Example 10

[0111] The magnesium-aluminum dissimilar metal ultrasonic brazing filler metal of this embodiment comprises 84wt.%Zn-6wt.%Ag-10wt.%Cu.

[0112] This invention provides a method for preparing ultrasonic brazing filler metal for magnesium-aluminum dissimilar metals, comprising the following steps:

[0113] S1, set the furnace temperature of the 10kg induction melting furnace to 1000℃, take the metal raw materials of each component of the prepared brazing filler metal according to the proportion, first add pure silver and pure copper to the melting container of the induction melting furnace, and keep it at the temperature for 5 minutes; wherein, the melting container is a corundum crucible.

[0114] S2, then add pure zinc to the melting container, keep it at a constant temperature for 3 minutes, then remove the melting container from the furnace and cool it to room temperature to complete the preparation of the brazing filler metal.

[0115] A brazed joint 3 in this embodiment includes an aluminum alloy base material 1 and a magnesium alloy base material 2. The aluminum alloy base material and the magnesium alloy base material are welded using the above-mentioned magnesium-aluminum dissimilar metal ultrasonic brazing filler metal and ultrasonic-assisted brazing method.

[0116] Optionally, the aluminum alloy base material is 6063 aluminum alloy base material, and the magnesium alloy base material is AZ31B magnesium alloy base material. One end of the aluminum alloy base material overlaps with one end of the magnesium alloy base material, and a weld seam is formed at the overlap.

[0117] The chemical composition of the solders in Examples 1 to 10 was determined using a Thermo Scientific ARL4460 fluorescence spectrometer under atmospheric conditions, and the results are shown in Table 1. The metallographic structures of Examples 1 and 2 were observed using a Hitachi SU6600 scanning electron microscope under room temperature vacuum conditions, and the morphologies are shown in the figures below. Figure 1 and Figure 3 As shown. (Through) Figure 1 and Figure 3 Analysis shows that the solder microstructure consists of a proeutectic phase and a eutectic phase. In Examples 3-10, since the Cu content did not show a new value and the Ag content changed only slightly, not crossing the Ag-Zn eutectic point, the corresponding solder alloy microstructures are similar to... Figure 1 , Figure 3 Similarly, they are all composed of a proeutectic phase and a eutectic phase, which will not be repeated here.

[0118] Table 1 Chemical composition of brazing alloy (wt%)

[0119] element Ag Cu Zn Example 1 4.0 5.0 margin Example 2 4.0 10.0 margin Example 3 4.5 5.0 margin Example 4 4.5 10.0 margin Example 5 5.0 5.0 margin Example 6 5.0 10.0 margin Example 7 5.5 5.0 margin Example 8 5.5 10.0 margin Example 9 6.0 5.0 margin Example 10 6.0 10.0 margin

[0120] Brazing experiments were conducted on the brazing filler metals of Examples 1 to 10 using their respective brazing methods. During the experiments, the aluminum alloy base material 1 and magnesium alloy base material 2 could be rectangular plates. One end of the aluminum alloy base material 1 along its length and one end of the magnesium alloy base material 2 along its length were overlapped vertically. For example, if the aluminum alloy base material 1 has a length of 50mm, a width of 25mm, and a thickness of 3mm, and the magnesium alloy base material 2 has a length of 50mm, a width of 25mm, and a thickness of 3mm, one side of the aluminum alloy base material 1 and one side of the magnesium alloy base material 2 could be overlapped, with an overlap length of approximately 10mm. Figure 5 and Figure 6 As shown. The aluminum alloy base material 1 can be heated using the induction heat source 5, causing the brazing filler metal 4 to form molten brazing filler metal 4 on the aluminum alloy base material 1. Then, the magnesium alloy base material 2 is placed on the molten brazing filler metal 4, and vibration welding is performed using the ultrasonic vibration head 6. Figure 7 and Figure 8 As shown.

[0121] The microstructure of the brazed joints of Examples 1 and 2 was observed using a Hitachi SU6600 scanning electron microscope under room temperature vacuum conditions, as shown below. Figure 2 and Figure 4 As shown. (Through) Figure 2 and Figure 4 Analysis shows that the brazing filler metal formed a good metallurgical bond with both base metals. Apart from proeutectic dendrites and eutectic phases, no intermetallic compound phases appeared in the overall weld microstructure, indicating that the brazing filler metal effectively prevented the direct contact between Mg and Al elements to form brittle intermetallic compounds (Mg). 17 Al 12 .

[0122] The shear strength of the brazed joints in Examples 1 to 10 was tested using a Shimadzu UH-F500KNI mechanical property testing machine, and the results are shown in Table 2.

[0123] Table 2 Shear Strength of Brazed Joints

[0124] Shear strength (MPa) Example 1 31 Example 2 52 Example 3 46 Example 4 56 Example 5 47 Example 6 62 Example 7 45 Example 8 70 Example 9 44 Example 10 69

[0125] As shown in Table 2, under the same Ag content, the joint strength increases significantly with the increase of Cu content; under the same Cu content, the joint strength first gradually increases with the increase of Ag content, and then tends to fluctuate slightly after reaching a certain strength level, without changing significantly with the increase of Ag content. Specifically, when the Cu content is 5%, the joint strength reaches its peak when the Ag content reaches 5%; when the Cu content is 10%, the joint strength reaches its peak when the Ag content reaches 5.5%.

[0126] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.

Claims

1. A magnesium-aluminum dissimilar metal ultrasonic brazing filler metal, characterized in that, The brazing filler metal comprises (84 wt.% to 92 wt.%) Zn-(3 wt.% to 6 wt.%) Ag-(5 wt.% to 10 wt.%) Cu.

2. The magnesium-aluminum dissimilar metal ultrasonic brazing filler metal according to claim 1, characterized in that, The brazing filler metal comprises 91 wt.% Zn, 4 wt.% Ag, and 5 wt.% Cu.

3. The magnesium-aluminum dissimilar metal ultrasonic brazing filler metal according to claim 1, characterized in that, The brazing filler metal comprises 86 wt.% Zn, 4 wt.% Ag, and 10 wt.% Cu.

4. A method for preparing the magnesium-aluminum dissimilar metal ultrasonic brazing filler metal according to any one of claims 1 to 3, characterized in that, Includes the following steps: S1, set the furnace temperature of the induction melting furnace to the first set temperature, take the metal raw materials of each component of the prepared brazing filler metal according to the proportion, first add pure silver and pure copper to the melting container of the induction melting furnace, and keep it warm for the first set time. S2, then add pure zinc to the melting container, keep it at the temperature for a second set time, then remove the melting container from the furnace and cool it to room temperature to complete the preparation of the brazing filler metal.

5. The method for preparing the magnesium-aluminum dissimilar metal ultrasonic brazing filler metal according to claim 4, characterized in that, The furnace temperature of the induction melting furnace is set to 900℃~1100℃.

6. The method for preparing the magnesium-aluminum dissimilar metal ultrasonic brazing filler metal according to claim 4, characterized in that, The first set time is 3 to 8 minutes; the second set time is 2 to 5 minutes.

7. The method for preparing the magnesium-aluminum dissimilar metal ultrasonic brazing filler metal according to claim 4, characterized in that, The smelting container is a corundum crucible.

8. A brazed joint, characterized in that, It includes an aluminum alloy base material and a magnesium alloy base material, wherein the aluminum alloy base material and the magnesium alloy base material are welded using the magnesium-aluminum dissimilar metal ultrasonic brazing filler metal described in any one of claims 1 to 3 and using an ultrasonic-assisted brazing method.

9. The brazed joint according to claim 8, characterized in that, The aluminum alloy base material is 6063 aluminum alloy base material, and the magnesium alloy base material is AZ31B magnesium alloy base material.

10. The brazed joint according to claim 8, characterized in that, One end of the aluminum alloy base material overlaps with one end of the magnesium alloy base material, and a weld seam is formed at the overlap.

Citation Information

Patent Citations

  • Brazing filler metal suitable for braze welding of magnesium-aluminum dissimilar alloys and preparation method for brazing filler metal

    CN105562956A

  • Brazing method for magnesium / aluminum dissimilar metal

    CN116652314A