A coating process for producing abrasive coatings on PET substrates

By employing a double-layer transfer printing process on PET substrates, using photocurable masterbatch and daughter adhesive, the problems of difficulty in replicating the microstructure of coated abrasives on PET substrates, balancing wear resistance and flexibility, and difficulty in demolding have been solved. This has resulted in a highly efficient and environmentally friendly coating process suitable for continuous production.

CN123103536APending Publication Date: 2026-11-17HUARONG COUNTY HENGXING BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611500170.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for producing coated abrasives on PET substrates have problems such as difficulty in replicating the microstructure, difficulty in balancing wear resistance and flexibility, and high production costs. In particular, when using UV curing technology, mold release is difficult and coating adhesion is insufficient.

Method used

A dual-layer transfer process is adopted, using photocurable masterbatch and daughter adhesive to form a masterbatch layer and a daughter adhesive layer on a PET substrate, respectively. The masterbatch layer ensures adhesion and release properties between the masterbatch layer and the PET substrate and the steel mold by compounding silane coupling agent and release agent. The daughter adhesive layer achieves a balance between flexibility and adhesion by polyurethane acrylate and siloxane segments, and combines aluminum oxide and silicon carbide abrasive to improve grinding performance.

Benefits of technology

It achieves high-precision replication of micro-nano structures, reduces production energy consumption, reduces VOC emissions, improves coating adhesion and wear resistance, lowers production costs, and the process is suitable for continuous production lines, thus improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103536A_ABST
    Figure CN123103536A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of polymer composite materials technology, specifically a coating process for producing abrasive coatings on a PET substrate. The coating process includes the following steps: First, a photocurable masterbatch is coated onto the PET substrate using a roller with micro / nano structures and then photocured to obtain a master film with micro / nano structures. Then, a photocurable daughter adhesive is coated onto a new PET substrate, and the master film is used for lamination and transfer printing, followed by photocuring to obtain the finished product. Both the masterbatch and daughter adhesive are made of polyurethane acrylate, compounded with certain monomers, photoinitiators, and additives. This invention achieves the replication of micro / nano structures through a "masterbatch molding, daughter adhesive transfer" process. The master film can be reused multiple times, and the product has good adhesion, wear resistance, and flexibility, offering advantages such as high production efficiency and low energy consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer composite material technology, specifically a coating process for producing abrasive coatings on a PET substrate. Background Technology

[0002] Coated abrasives, commonly known as sandpaper, are widely used in metal processing, wood processing, and surface treatment. Traditional manufacturing of coated abrasives primarily employs a resin (such as phenolic resin or urea-formaldehyde resin) thermosetting process. This process typically includes coating, drying, and thermosetting steps, resulting in high energy consumption, long drying times, large footprint, and volatile organic compound (VOC) emissions, which do not meet the requirements of modern green manufacturing.

[0003] With the development of ultraviolet (UV) curing technology, the fabrication of coated abrasives using UV-curable resins has gradually become a research hotspot. UV curing offers advantages such as instant curing, low energy consumption, and solvent-free emissions. However, existing technologies still face the following challenges when fabricating high-performance coated abrasives on flexible substrates such as PET (polyethylene terephthalate):

[0004] 1. Difficulty in replicating microstructures: To improve grinding efficiency and heat dissipation, it is usually necessary to fabricate specific micro / nano structures (such as arrays of square pyramids) on the surface of the abrasive. Existing direct coating and curing processes cannot guarantee high-precision replication of microstructures, and the mold is prone to sticking to the adhesive layer, leading to difficulties in demolding.

[0005] 2. Balance between abrasion resistance and flexibility: The abrasive layer needs to have extremely high hardness to bear the abrasive, while also needing good adhesion to the flexible PET substrate. Existing single-component UV adhesives are difficult to meet the requirements of high abrasion resistance and high adhesion at the same time, and are prone to coating cracking or peeling.

[0006] 3. Production cost: High-precision molds are expensive. If the mold is easily damaged or difficult to clean during demolding, it will greatly increase the production cost.

[0007] Therefore, there is an urgent need to develop a coating process that can achieve high-precision transfer of micro-nano structures, while also ensuring wear resistance and adhesion, and is environmentally friendly. Summary of the Invention

[0008] To address the above problems, this invention provides a coating process for producing coated abrasives on PET substrates, which solves the problems of high energy consumption, poor micro-nano structure replication accuracy, difficulty in mold demolding, and insufficient coating adhesion in the current technology for coated abrasive production.

[0009] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0010] A coating process for producing coated abrasives on a PET substrate includes the following steps: coating a photocurable masterbatch onto a PET substrate to form a masterbatch layer, and then performing photocuring to obtain a master film, wherein the masterbatch layer has micro-nano structures distributed on it; then coating a photocurable sub-adhesive onto the PET substrate and printing the micro-nano structures on the master film onto the sub-adhesive to form a sub-adhesive layer, and then performing photocuring to obtain PET coated abrasives;

[0011] The photocurable masterbatch is prepared by the following method: a mixture of toluene diisocyanate and 1,3-propanetriol diacrylate in a molar ratio of 1:1 is reacted, followed by a reaction with a diol oligomer to obtain polyurethane acrylate; then, the polyurethane acrylate, photocurable monomer, photoinitiator, silane coupling agent, and release agent are mixed to obtain the photocurable masterbatch; the photocurable monomer is composed of tripropylene glycol diacrylate, N-acryloylmorpholine, and tetrahydrofuran acrylate in a mass ratio of 4:1~1.5:0.8~1.2, and the silane coupling agent is composed of γ-glycidyl ether propyltrimethoxysilane and tert-butyltrimethoxysilane in a mass ratio of 3~4:1.8~2.4; the molar ratio of toluene diisocyanate to the diol oligomer is 1:0.5, and the chemical structure of the diol oligomer is as follows:

[0012] ;

[0013] The photocurable sub-adhesive is prepared by the following method: toluene diisocyanate and 1,3-propanetriol diacrylate are mixed and reacted in a molar ratio of 1:1, and then mixed and reacted with diol oligomers to obtain polyurethane acrylate, wherein the molar ratio of toluene diisocyanate and diol oligomers is 1:0.5; then the polyurethane acrylate, photocurable monomer, photoinitiator, defoamer, leveling agent, dispersant, anti-settling agent and abrasive are mixed evenly to obtain the photocurable sub-adhesive; the photocurable monomer is composed of tripropylene glycol diacrylate, (4) bisphenol A diacrylate, N-acryloylmorpholine and tetrahydrofuran acrylate in a mass ratio of 3~4:2~3:1~1.5:1.2~1.8, and the chemical structure of the diol oligomer is as follows:

[0014] .

[0015] Preferably, the photocurable masterbatch is coated onto the PET substrate to form a masterbatch layer by roller coating, and rollers with micro-nano structures are used during roller coating.

[0016] Preferably, the micro-nano structures on the roller are arranged in an array. The micro-nano structures are regular square pyramids with a base side length of 200~300μm and a pyramid depth of 20~50μm. The bases of the regular square pyramids are connected to form a full-coverage array.

[0017] Preferably, the amount of masterbatch used for coating is 40~70g / m². 2 The photocuring energy is 320~400mJ / cm. 2 The amount of adhesive used for coating is 90~120g / m². 2 The photocuring energy is 430~500mJ / cm. 2 .

[0018] Preferably, when preparing the masterbatch, the mass ratio of polyurethane acrylate, photocurable monomer and silane coupling agent is 75~80:15.5~17:0.5~0.8.

[0019] Preferably, when preparing the masterbatch, the mass ratio of polyurethane acrylate, photocurable monomer, photoinitiator, silane coupling agent and release agent is 75~80:15.5~17:7~9:0.5~0.8:2~3.

[0020] Preferably, when preparing the abrasive, the abrasive is composed of aluminum oxide and silicon carbide in a mass ratio of 6~8:4~6.

[0021] Preferably, the average particle size of the aluminum oxide is 10-15 μm, and the average particle size of the silicon carbide is 5-8 μm.

[0022] Preferably, when preparing the adhesive, the mass ratio of polyurethane acrylate, photocurable monomer, photoinitiator, defoamer, leveling agent, dispersant, anti-settling agent and abrasive is 20~40:20~30:4~8:0.2~2:0.1~0.5:0.5~1.5:0.2~1:50~70.

[0023] Preferably, when preparing the adhesive, UV color paste is also added; the mass ratio of polyurethane acrylate, photocurable monomer, photoinitiator, defoamer, leveling agent, dispersant, anti-settling agent, abrasive and UV color paste is 20~40:20~30:4~8:0.2~2:0.1~0.5:0.5~1.5:0.2~1:50~70:0.001~0.5.

[0024] Compared with existing technologies, the advantages of the coating process for producing abrasive coatings on PET substrates according to the present invention are as follows:

[0025] (1) This invention uses ultraviolet (UV) curing technology to replace the traditional thermosetting process, eliminating the need for high-temperature baking and achieving immediate curing after coating, thus reducing production energy consumption; the system is a solvent-free / low-solvent UV curing system, reducing VOC emissions. The process has a fast curing speed and continuous steps, making it suitable for continuous production lines such as unwinding, corona treatment, roller coating, pre-curing, UV curing, and rewinding, resulting in high production efficiency.

[0026] (2) This invention employs a two-layer transfer process of "master glue molding and sub-glue transfer". By compounding silane coupling agent and release agent in the master glue formula, the master glue layer has adhesion to the PET substrate and can be demolded from the steel mold; the surface of the master film can replicate micro-nano structures such as regular square pyramids. Experiments show that the master film can be reused 6 times, and the depth retention rate of the product obtained after the 6th transfer is still no less than 90% of the depth retention rate when the master film is used for the first time, effectively solving the problems of expensive precision molds and difficult demolding.

[0027] (3) Both the masterbatch and the daughter adhesive of the present invention are made of polyurethane acrylate. Fluorine / silicon segments are introduced into the masterbatch, and siloxane segments and quaternary ammonium salt structures are introduced into the daughter adhesive. In addition, a compounded photocurable monomer and silane coupling agent are used to achieve a balance between the flexibility and adhesion of the cured coating.

[0028] (4) The sub-adhesive of the present invention uses a composite abrasive of aluminum oxide and silicon carbide, and combines it with composite monomers such as tripropylene glycol diacrylate, bisphenol A diacrylate, N-acryloylmorpholine and tetrahydrofuran acrylate, so that the product has a higher amount of grinding removal and a lower amount of grinding loss under the same grinding test conditions; at the same time, the color can be adjusted by UV color paste, and the surface square pyramid array can be used to present a regular grid texture and directional reflective gloss effect. Attached Figure Description

[0029] Figure 1 Here is an image showing the appearance of the mother film prepared in Example 1;

[0030] Figure 2 Images showing the appearance of the PET-coated abrasive prepared in Example 1;

[0031] Figure 3 This is a magnified image of the regular square pyramid array structure on the PET coated abrasive surface prepared in Example 1.

[0032] Figure 4 The image shows the 1H NMR spectrum of the diol oligomer prepared in the masterbatch preparation method of Example 1.

[0033] Figure 5 The image shows the 1H NMR spectrum of the diol oligomer prepared in the gel preparation method of Example 1. Detailed Implementation

[0034] To enable those skilled in the art to better understand the technical solution, the present invention will be described in detail below with reference to embodiments. The description in this part is only exemplary and explanatory, and should not be used to limit the scope of protection of the present invention in any way.

[0035] The toluene diisocyanate used in the following examples is toluene-2,4-diisocyanate.

[0036] Example 1

[0037] The coating process for applying abrasives to a PET substrate in this embodiment includes the following steps:

[0038] (1) PET film unwinding corona treatment: Install the prepared PET film on the unwinding machine, adjust the unwinding speed to 5m / min, and keep the tension stable during the unwinding process (tension controlled at 220~240N) to avoid stretching and deformation of the PET film; then send the PET film into the corona treatment machine, adjust the corona treatment power to 300W, and the corona treatment time to 3s, to ensure that the corona value on the PET film surface is >50, and the difference in corona value between any two points is ≤5. The corona treatment improves the surface activity of the PET film and enhances the adhesion between the subsequent adhesive and the substrate. After the treatment is completed, the PET film surface is dusted to avoid impurities remaining.

[0039] (2) Roller Coating and Curing of Masterbatch: The treated PET film is fed into the roller coating equipment. A rubber roller with a hardness of 40 and a steel roller engraved with a regular square pyramid array structure (the base side length of the regular square pyramid is 200μm and the pyramid depth is 40μm) are used for roller coating. During the process, the rubber roller applies pressure to the back of the PET film, indirectly transmitting the pressure to the steel roller. The pressure applied by the rubber roller is 3kg / cm. 2 Control the amount of masterbatch used for coating to 50g / m 2 The roller coating speed is 5 m / min to ensure uniform coating without any missed areas or drips. After roller coating, the PET film coated with the masterbatch is sent to an LED pre-curing device for pre-curing for 10 seconds to allow the masterbatch to initially set. It is then sent to a UV curing machine, with the UV curing energy adjusted to 350 mJ / cm². 2 The curing time is 15 seconds to ensure complete curing of the masterbatch. During the curing process, the PET film should be kept stable to prevent displacement. See the image for the masterbatch appearance. Figure 1 As shown.

[0040] (3) Rewinding the master film for later use: The cured PET coated master film is fed into the winding machine. The winding speed is adjusted to 5m / min, the winding tension is controlled at 120~140N, and the winding taper is 50%. During the winding process, the master film is kept flat, without wrinkles or damage. After winding, the master film is placed in a clean and dry environment for later use. The later use time shall not exceed 24 hours. Avoid the surface of the master film from getting damp or contaminated.

[0041] (4) Unwinding and corona treatment of PET film: Take another roll of PET film of the same specifications and unwind, corona treatment and dust removal according to the operation method in step (1). The corona treatment parameters, unwinding speed and tension control are consistent with those in step (1) to ensure that the surface activity of the PET film meets the requirements for pressing and bonding.

[0042] (5) The PET film treated with corona in step (4) is fed into a roller coating equipment. A rubber roller with a hardness of 40 is used in conjunction with the prepared master film for roller coating. During the coating process, the rubber roller applies pressure to the back of the PET film, indirectly transmitting the pressure to the master film. The pressure applied by the rubber roller is 3 kg / cm². 2 The amount of adhesive used for coating is controlled at 100g / m. 2 The roller coating speed is 5 m / min to ensure uniform coating without any missed areas or drips; then the PET film coated with the adhesive is fed into a UV curing machine, and the UV curing energy is adjusted to 450 mJ / cm². 2 To ensure complete curing of the adhesive, the curing effect is monitored in real time during the curing process.

[0043] (6) PET-coated abrasive winding: The finished PET-coated abrasive (PET film with cured adhesive) is fed into the winding unit, and the winding tension is controlled at 100~160N for smooth winding; the mother film is recycled and wound back through the guide circuit for reuse in the next transfer printing production. The appearance of the PET-coated abrasive prepared in this embodiment is shown in the image below. Figure 2 As shown in the enlarged image, the appearance of the square pyramidal array structure on the PET coated with abrasive is as follows: Figure 3 As shown.

[0044] The masterbatch is prepared by the following method: polyurethane acrylate, photocurable monomer, and photoinitiator are stirred and mixed evenly, then a silane coupling agent and a release agent are added sequentially and stirred evenly to obtain a transfer UV-curable coating abrasive oil masterbatch; wherein the photocurable monomer is composed of tripropylene glycol diacrylate, N-acryloylmorpholine, and tetrahydrofuran acrylate in a mass ratio of 4:1:1.2, the photoinitiator is 1173, the silane coupling agent is composed of γ-glycidyl ether propyltrimethoxysilane and tert-butyltrimethoxysilane in a mass ratio of 3:1.8, and the release agent is HD-915 type release agent produced by Shanghai Dongheng Company; the mass ratio of polyurethane acrylate, photocurable monomer, photoinitiator, silane coupling agent, and release agent is 75:15.5:7:0.5:2. The polyurethane acrylate in the masterbatch is prepared by the following method:

[0045] (1) Add 15.0 mmol of 1,3-bis(3-glycidylpropyl)-1,1,3,3-tetramethyldisiloxane and 40 mL of anhydrous 1,4-dioxane to a round-bottom flask equipped with a stirrer, thermometer, condenser and nitrogen gas. After stirring evenly, add 30.0 mmol of a mixture of N-methyl-2-(pentafluoroethylthio)ethylamine and 10 mL of anhydrous 1,4-dioxane dropwise to the round-bottom flask. Control the amount of material in the round-bottom flask during the dropwise addition. The temperature was not to exceed 35℃. After the addition was complete, the temperature was raised to 60℃ and the reaction was stirred at a constant temperature for 10 hours. After the reaction was completed, the reaction solution was cooled to room temperature, and the solvent was removed by vacuum distillation to obtain the crude product. The crude product was then dissolved in 30 mL of dichloromethane and washed once with 30 mL of saturated brine. The resulting organic phase was dried with anhydrous magnesium sulfate and filtered. The filtrate was concentrated by vacuum distillation and then dried in a vacuum drying oven at 40℃ for 12 hours to obtain the diol oligomer with a yield of 83%. The chemical structure of N-methyl-2-(pentafluoroethylthio)ethylamine is as follows:

[0046] ;

[0047] The chemical structure of 1,3-bis(3-glycidylpropyl)-1,1,3,3-tetramethyldisiloxane is as follows:

[0048] ;

[0049] The 1H NMR spectrum of the diol oligomers is shown below. Figure 4 As shown, the chemical structure is as follows:

[0050] .

[0051] (2) In a reaction flask, 0.05 mol of toluene diisocyanate, 80 mL of 1,4-dioxane, the polymerization inhibitor hydroquinone, and the catalyst dibutyltin dilaurate were added sequentially. After mechanical stirring until homogeneous, 0.05 mol of 1,3-propanetriol diacrylate was added dropwise. After the addition was complete, the mixture was heated to 40°C and stirred for 5 h. Then, 0.025 mol of diol oligomer was added, the temperature was raised to 70°C, and the mixture was stirred for another 4 h. Finally, the solvent 1,4-dioxane was removed by vacuum distillation to obtain polyurethane acrylate. The mass of the polymerization inhibitor hydroquinone was 0.2% of the mass of toluene diisocyanate, 1,3-propanetriol diacrylate, and diol oligomer, and the mass of the catalyst dibutyltin dilaurate was 0.3% of the mass of toluene diisocyanate, 1,3-propanetriol diacrylate, and diol oligomer.

[0052] The sub-adhesive is prepared by the following method: polyurethane acrylate, photocurable monomer and photoinitiator are stirred and mixed evenly, and then defoamer, leveling agent, dispersant, anti-settling agent, abrasive and UV color paste are added in sequence and stirred evenly to obtain transfer UV-curable coating abrasive sub-adhesive; wherein, the photocurable monomer is composed of tripropylene glycol diacrylate, (4) bisphenol A diacrylate, N-acryloylmorpholine and tetrahydrofuran acrylate in a mass ratio of 3:2:1:1.2, the photoinitiator is 1173, the defoamer is BYK-055, the leveling agent is BYK-370, the dispersant is BYK-204, the anti-settling agent is silica (AEROSIL R972 produced by Evonik GmbH, Germany), the abrasive is composed of aluminum oxide (average particle size of 15μm) and silicon carbide (average particle size of 5μm) in a mass ratio of 6:4, and the UV color paste is Hostatint® UV Violet produced by Clariant Chemicals. The mass ratio of polyurethane acrylate, UV-curable monomer, photoinitiator, defoamer, leveling agent, dispersant, anti-settling agent, abrasive, and UV colorant is 30:20:5:0.5:0.2:0.9:0.5:55:0.05. The polyurethane acrylate in the adhesive is prepared by the following method:

[0053] (1) In a three-necked round-bottom flask equipped with a magnetic stirrer, thermometer, nitrogen delivery tube and condenser, 15.0 mmol of 5-carboxy-N,N,N-trimethyl-1-pentanemonium bromide, 7.5 mmol of 1,3-bis(3-glycidylpropyl)-1,1,3,3-tetramethyldisiloxane, 1.2 mmol of tetrabutylammonium bromide and 40 mL of anhydrous N,N-dimethylformamide were added sequentially. Under nitrogen protection, the reaction mixture was heated to 80 mL. The reaction was carried out at 0℃ for 24 hours with stirring. After the reaction was completed, the solvent was removed from the reaction solution under reduced pressure at 80℃ to obtain a concentrate. 30 mL of dichloromethane was added to the concentrate and stirred to dissolve it. The concentrate was then washed three times with saturated brine (30 mL of saturated brine was used for each wash). The washed organic phase was then dried with anhydrous magnesium sulfate and filtered. Finally, the filtrate was concentrated by reduced pressure distillation and then dried in a vacuum drying oven at 45℃ for 12 hours to obtain diol oligomers with a yield of 79%.

[0054] The 1H NMR spectrum of the diol oligomers is shown below. Figure 5 As shown, the chemical structure is as follows:

[0055] .

[0056] (2) In a reaction flask, 0.05 mol of toluene diisocyanate, 80 mL of 1,4-dioxane, the polymerization inhibitor p-hydroxyanisole, and the catalyst dibutyltin dilaurate were added sequentially. After mechanical stirring until homogeneous, 0.05 mol of 1,3-propanetriol diacrylate was added dropwise. After the addition was complete, the mixture was heated to 40°C and stirred for 5 h. Then, 0.025 mol of diol oligomer was added, the temperature was raised to 70°C, and the mixture was stirred for another 5 h. Finally, the solvent 1,4-dioxane was removed by vacuum distillation to obtain polyurethane acrylate. The mass of the polymerization inhibitor p-hydroxyanisole was 0.2% of the mass of toluene diisocyanate, 1,3-propanetriol diacrylate, and diol oligomer, and the mass of the catalyst dibutyltin dilaurate was 0.3% of the mass of toluene diisocyanate, 1,3-propanetriol diacrylate, and diol oligomer.

[0057] Example 2

[0058] The coating process for applying abrasives to a PET substrate in this embodiment includes the following steps:

[0059] (1) PET film unwinding corona treatment: Install the prepared PET film on the unwinding machine, adjust the unwinding speed to 5m / min, and keep the tension stable during the unwinding process (tension controlled at 220~240N) to avoid stretching and deformation of the PET film; then send the PET film into the corona treatment machine, adjust the corona treatment power to 300W, and the corona treatment time to 3s, to ensure that the corona value on the PET film surface is >50, and the difference in corona value between any two points is ≤5. The corona treatment improves the surface activity of the PET film and enhances the adhesion between the subsequent adhesive and the substrate. After the treatment is completed, the PET film surface is dusted to avoid impurities remaining.

[0060] (2) Roller Coating and Curing of Masterbatch: The treated PET film is fed into the roller coating equipment. A rubber roller with a hardness of 40 and a steel roller engraved with a regular square pyramid array structure (the base side length of the regular square pyramid is 200μm and the pyramid depth is 40μm) are used for roller coating. During the process, the rubber roller applies pressure to the back of the PET film, indirectly transmitting the pressure to the steel roller. The pressure applied by the rubber roller is 3kg / cm. 2 The amount of masterbatch used for coating should be controlled at 40g / m². 2 The roller coating speed is 5 m / min to ensure uniform coating without any missed areas or drips. After roller coating, the PET film coated with the masterbatch is sent to an LED pre-curing device for pre-curing for 10 seconds to allow the masterbatch to initially set. It is then sent to a UV curing machine, with the UV curing energy adjusted to 320 mJ / cm². 2 The curing time is 15 seconds to ensure that the masterbatch is completely cured. During the curing process, the PET film should be kept running smoothly to avoid displacement.

[0061] (3) Rewinding the master film for later use: The cured PET coated master film is fed into the winding machine. The winding speed is adjusted to 5m / min, the winding tension is controlled at 120~140N, and the winding taper is 50%. During the winding process, the master film is kept flat, without wrinkles or damage. After winding, the master film is placed in a clean and dry environment for later use. The later use time shall not exceed 24 hours. Avoid the surface of the master film from getting damp or contaminated.

[0062] (4) Unwinding and corona treatment of PET film: Take another roll of PET film of the same specifications and unwind, corona treatment and dust removal according to the operation method in step (1). The corona treatment parameters, unwinding speed and tension control are consistent with those in step (1) to ensure that the surface activity of the PET film meets the requirements for pressing and bonding.

[0063] (5) The PET film treated with corona in step (4) is fed into a roller coating equipment. A rubber roller with a hardness of 40 is used in conjunction with the prepared master film for roller coating. During the coating process, the rubber roller applies pressure to the back of the PET film, indirectly transmitting the pressure to the master film. The pressure applied by the rubber roller is 3 kg / cm². 2 The amount of adhesive used for coating is controlled at 90g / m. 2 The roller coating speed is 5 m / min to ensure uniform coating without any missed areas or drips; then the PET film coated with the adhesive is fed into a UV curing machine, and the UV curing energy is adjusted to 430 mJ / cm². 2 To ensure complete curing of the adhesive, the curing effect is monitored in real time during the curing process.

[0064] (6) PET coated with abrasive winding: The finished PET coated with abrasive (PET film with cured sub-adhesive) is fed into the winding unit and the winding tension is controlled at 100~160N to wind it flat; the mother film is recycled and wound through the guide circuit and reused for the next transfer production.

[0065] The masterbatch was prepared by the following method: polyurethane acrylate, photocurable monomer, and photoinitiator were mixed evenly, and then a silane coupling agent and a release agent were added sequentially and mixed evenly to obtain a transfer UV-curable coating abrasive oil masterbatch. The photocurable monomer consisted of tripropylene glycol diacrylate, N-acryloylmorpholine, and tetrahydrofuran acrylate in a mass ratio of 4:1.2:1; the photoinitiator was 1173; the silane coupling agent consisted of γ-glycidyl ether propyltrimethoxysilane and tert-butyltrimethoxysilane in a mass ratio of 3.5:2; and the release agent was HD-915 type release agent produced by Shanghai Dongheng Company. The mass ratio of polyurethane acrylate, photocurable monomer, photoinitiator, silane coupling agent, and release agent was 78:16:8:0.7:2.5. The polyurethane acrylate in the masterbatch was the same as that used in the masterbatch in Example 1.

[0066] The sub-adhesive is prepared by the following method: polyurethane acrylate, photocurable monomer and photoinitiator are stirred and mixed evenly, and then defoamer, leveling agent, dispersant, anti-settling agent, abrasive and UV color paste are added in sequence and stirred evenly to obtain transfer UV-curable coating abrasive sub-adhesive; wherein, the photocurable monomer is composed of tripropylene glycol diacrylate, (4) bisphenol A diacrylate, N-acryloylmorpholine and tetrahydrofuran acrylate in a mass ratio of 3:3:1.2:1.5, the photoinitiator is 1173, the defoamer is BYK-055, the leveling agent is BYK-370, the dispersant is BYK-204, the anti-settling agent is silica (AEROSIL R972 produced by Evonik GmbH, Germany), the abrasive is composed of aluminum oxide (average particle size of 15μm) and silicon carbide (average particle size of 5μm) in a mass ratio of 7:5, and the UV color paste is Hostatint® UV Violet produced by Clariant Chemicals. RL; The mass ratio of polyurethane acrylate, UV-curable monomer, photoinitiator, defoamer, leveling agent, dispersant, anti-settling agent, abrasive, and UV colorant is 35:22:6:0.5:0.2:0.9:0.5:60:0.07. The polyurethane acrylate in the sub-adhesive is the same as that used in the sub-adhesive in Example 1.

[0067] Example 3

[0068] The coating process for applying abrasives to a PET substrate in this embodiment includes the following steps:

[0069] (1) PET film unwinding corona treatment: Install the prepared PET film on the unwinding machine, adjust the unwinding speed to 5m / min, and keep the tension stable during the unwinding process (tension controlled at 220~240N) to avoid stretching and deformation of the PET film; then send the PET film into the corona treatment machine, adjust the corona treatment power to 300W, and the corona treatment time to 3s, to ensure that the corona value on the PET film surface is >50, and the difference in corona value between any two points is ≤5. The corona treatment improves the surface activity of the PET film and enhances the adhesion between the subsequent adhesive and the substrate. After the treatment is completed, the PET film surface is dusted to avoid impurities remaining.

[0070] (2) Roller Coating and Curing of Masterbatch: The treated PET film is fed into the roller coating equipment. A rubber roller with a hardness of 40 and a steel roller engraved with a regular square pyramid array structure (the base side length of the regular square pyramid is 200μm and the pyramid depth is 40μm) are used for roller coating. During the process, the rubber roller applies pressure to the back of the PET film, indirectly transmitting the pressure to the steel roller. The pressure applied by the rubber roller is 3kg / cm. 2 The amount of masterbatch used for coating should be controlled at 70g / m². 2The roller coating speed is 5 m / min to ensure uniform coating without any missed areas or drips. After roller coating, the PET film coated with the masterbatch is sent to an LED pre-curing device for pre-curing for 10 seconds to allow the masterbatch to initially set. It is then sent to a UV curing machine, with the UV curing energy adjusted to 400 mJ / cm². 2 The curing time is 15 seconds to ensure that the masterbatch is completely cured. During the curing process, the PET film should be kept running smoothly to avoid displacement.

[0071] (3) Rewinding the master film for later use: The cured PET coated master film is fed into the winding machine. The winding speed is adjusted to 5m / min, the winding tension is controlled at 120~140N, and the winding taper is 50%. During the winding process, the master film is kept flat, without wrinkles or damage. After winding, the master film is placed in a clean and dry environment for later use. The later use time shall not exceed 24 hours. Avoid the surface of the master film from getting damp or contaminated.

[0072] (4) Unwinding and corona treatment of PET film: Take another roll of PET film of the same specifications and unwind, corona treatment and dust removal according to the operation method in step (1). The corona treatment parameters, unwinding speed and tension control are consistent with those in step (1) to ensure that the surface activity of the PET film meets the requirements for pressing and bonding.

[0073] (5) The PET film treated with corona in step (4) is fed into a roller coating equipment. A rubber roller with a hardness of 40 is used in conjunction with the prepared master film for roller coating. During the coating process, the rubber roller applies pressure to the back of the PET film, indirectly transmitting the pressure to the master film. The pressure applied by the rubber roller is 3 kg / cm². 2 The amount of adhesive used for coating is controlled at 120g / m. 2 The roller coating speed is 5 m / min to ensure uniform coating without any missed areas or drips; then the PET film coated with the adhesive is fed into a UV curing machine, and the UV curing energy is adjusted to 500 mJ / cm². 2 To ensure complete curing of the adhesive, the curing effect is monitored in real time during the curing process.

[0074] (6) PET coated with abrasive winding: The finished PET coated with abrasive (PET film with cured sub-adhesive) is fed into the winding unit and the winding tension is controlled at 100~160N to wind it flat; the mother film is recycled and wound through the guide circuit and reused for the next transfer production.

[0075] The masterbatch was prepared by the following method: polyurethane acrylate, photocurable monomer, and photoinitiator were mixed evenly, and then a silane coupling agent and a release agent were added sequentially and mixed evenly to obtain a transfer UV-curable coating abrasive oil masterbatch. The photocurable monomer consisted of tripropylene glycol diacrylate, N-acryloylmorpholine, and tetrahydrofuran acrylate in a mass ratio of 4:1.5:0.8; the photoinitiator was 1173; the silane coupling agent consisted of γ-glycidyl ether propyltrimethoxysilane and tert-butyltrimethoxysilane in a mass ratio of 4:2.4; and the release agent was HD-915 type release agent produced by Shanghai Dongheng Company. The mass ratio of polyurethane acrylate, photocurable monomer, photoinitiator, silane coupling agent, and release agent was 80:17:9:0.8:3. The polyurethane acrylate in the masterbatch was the same as that used in the masterbatch in Example 1.

[0076] The sub-adhesive is prepared by the following method: polyurethane acrylate, photocurable monomer and photoinitiator are stirred and mixed evenly, and then defoamer, leveling agent, dispersant, anti-settling agent, abrasive and UV color paste are added in sequence and stirred evenly to obtain transfer UV-curable coating abrasive sub-adhesive; wherein, the photocurable monomer is composed of tripropylene glycol diacrylate, (4) bisphenol A diacrylate, N-acryloylmorpholine and tetrahydrofuran acrylate in a mass ratio of 4:3:1.5:1.8, the photoinitiator is 1173, the defoamer is BYK-055, the leveling agent is BYK-370, the dispersant is BYK-204, the anti-settling agent is silica (AEROSIL R972 produced by Evonik GmbH, Germany), the abrasive is composed of aluminum oxide (average particle size of 15μm) and silicon carbide (average particle size of 5μm) in a mass ratio of 8:4, and the UV color paste is Hostatint® UV Violet produced by Clariant Chemicals. RL; The mass ratio of polyurethane acrylate, UV-curable monomer, photoinitiator, defoamer, leveling agent, dispersant, anti-settling agent, abrasive, and UV colorant is 38:25:8:0.5:0.2:0.9:0.5:70:0.1. The polyurethane acrylate in the sub-adhesive is the same as that used in the sub-adhesive in Example 1.

[0077] Experimental Example 1

[0078] To investigate the effect of the masterbatch formulation on the performance of the master film product, the masterbatch and master film were prepared repeatedly according to the method in Example 1. The difference was that the 1,3-propanetriol diacrylate in step (2) of the preparation method of polyurethane acrylate used in the masterbatch preparation method was replaced with β-hydroxyethyl acrylate (Comparative Example 1), or the 1,3-propanetriol diacrylate in step (2) of the preparation method of polyurethane acrylate was replaced with pentaerythritol triacrylate (Comparative Example 2), or the photocurable monomer used in the masterbatch preparation method was replaced with tripropylene glycol diacrylate and N-acryloylmorpholine in a mass ratio of 4:2.2 (Comparative Example 3), or the photocurable monomer was replaced with tripropylene glycol diacrylate and tetrahydrofuran acrylate in a mass ratio of 4:2.2 (Comparative Example 4), or the silane coupling agent used in the masterbatch preparation method was replaced with γ-glycidyl ether propyltrimethoxysilane (Comparative Example 5), or the silane coupling agent was replaced with tert-butyltrimethoxysilane (Comparative Example 6). Then, the masterbatch film was folded 180 degrees (with the side coated with the masterbatch layer facing outwards). After folding it 50 times in the same position, the percentage of the area where the masterbatch layer cracked or peeled off at the fold was observed and measured to evaluate the adhesion performance between the coating and the substrate. At the same time, a white light interferometer was used to measure the actual depth of the square pyramidal pit after transfer, and compared with the theoretical cone depth of the square pyramid of the steel roller mold to calculate the depth retention rate. The depth retention rate is equal to the ratio of the test depth to the theoretical cone depth of the steel roller mold. The test was performed in parallel for 3 times, and the average value of the results was taken. The adhesion and transfer effect test results of the transfer UV-cured abrasive oil masterbatch prepared in each embodiment and comparative example are shown in Table 1.

[0079] Table 1. Adhesion and transfer effect of UV-cured abrasive oil masterbatch for transfer printing

[0080]

[0081] As can be seen from the test results in Table 1, the masterbatch used in this invention has good adhesion to the PET substrate, and at the same time, it exhibits good demolding effect with the steel mold during the transfer process. It can print the microstructure morphology on the steel mold onto the master film in a good manner, and the masterbatch exhibits good morphology retention performance after demolding.

[0082] Experimental Example 2

[0083] To investigate the effects of the monomer types used in the sub-adhesive and the structure of the polyurethane acrylate on the performance of PET coated abrasive products, the polyurethane acrylate used in the adhesive was prepared repeatedly according to the method in Example 1, except that the photocurable monomers in the sub-adhesive were replaced with tripropylene glycol diacrylate, N-acryloylmorpholine and tetrahydrofuran acrylate in a mass ratio of 5:1:1.2 (Comparative Example 1), or the photocurable monomers in the sub-adhesive were replaced with (4) bisphenol A diacrylate, N-acryloylmorpholine and tetrahydrofuran acrylate in a mass ratio of 5:1:1.2 (Comparative Example 2), or the photocurable monomers in the sub-adhesive were replaced with tripropylene glycol diacrylate, (4) bisphenol A diacrylate and tetrahydrofuran acrylate in a mass ratio of 3:2:2.2 (Comparative Example 3), or The photocurable monomers in the sub-adhesive were replaced with tripropylene glycol diacrylate, (4) bisphenol A diacrylate and N-acryloylmorpholine in a mass ratio of 3:2:2.2 (Comparative Example 4), or the 5-carboxy-N,N,N-trimethyl-1-pentaneammonium bromide in step (1) of the preparation method of polyurethane acrylate was replaced with (2-carboxyethyl)trimethylammonium chloride (Comparative Example 5), or the 5-carboxy-N,N,N-trimethyl-1-pentaneammonium bromide was replaced with (3-carboxypropyl)trimethylammonium chloride (Comparative Example 6), or the 1,3-bis(3-glycidylpropyl)-1,1,3,3-tetramethyldisiloxane was replaced with 2,2'-(2,2,3,3,4,4,5,5-octafluorohexane-1,6-diyl)bis(ethylene oxide) (Comparative Example 7).

[0084] Then, the PET-coated abrasive product was cut into 25mm × 100mm samples. The samples were folded 180° along the center line so that the coating layer faced outwards, and immediately a 2kg roller was applied at a speed of 10mm / s to roll them once. After holding the folded state for 2 seconds, the samples were unfolded to a straight state, which was counted as one cycle. After 10 consecutive cycles, the samples were laid flat, and the area extending 5mm (total width 10mm) to both sides of the fold line was designated as the measurement area. The area of ​​coating peeling or cracking within the measurement area was observed and counted using a magnifying glass. The proportion of the total area was used to test three parallel samples in each group to evaluate the adhesion performance between the transferred UV-cured abrasive oil and the substrate. Then, the PET abrasive film was installed on the contact wheel, and a constant pressure was applied to the stainless steel workpiece to make the workpiece rotate while the PET abrasive film remained fixed. When the grinding time reached the set value, the test was stopped, and the mass loss of the workpiece during the grinding process was measured to obtain the amount of material removed ΔW. At the same time, the mass loss of the PET abrasive film during the grinding process was measured to obtain the amount of material worn ΔM. The test results are shown in Table 2.

[0085] Table 2. Influence of monomer type and polyurethane acrylate structure on the performance of PET coated abrasive products.

[0086]

[0087] As can be seen from the test results in Table 2, the sub-adhesive formulation used in this invention exhibits good interfacial bonding with the PET film substrate and good coating flexibility. Furthermore, it demonstrates both high removal amount (ΔW) and low wear amount (ΔM) in the grinding experiment, resulting in a high grinding ratio.

[0088] Example of effect

[0089] To examine the recyclability of the master film prepared in this invention, the master film used once in step (6) of Example 1 was recycled and rewound for reuse in the roll coating of PET-coated abrasive in step (5). Each time it was reused, the depth of the printed square pyramid array structure on the resulting PET-coated abrasive product was measured, and the depth retention rate was calculated according to the method defined in Experimental Example 1. When the depth retention rate was lower than 90% of the depth retention rate when the master film was first used, it was determined that the master film was severely worn and could not meet the usage requirements, necessitating replacement with a new master film for the preparation of PET-coated abrasive products. Experimental results showed that the master film prepared in Example 1 could be reused 6 times, and the depth retention rate of the product obtained after the 6th transfer was 88.2% of the depth retention rate when the master film was first used. Therefore, the master film prepared in Example 1 can be reused 6 times, demonstrating good durability.

[0090] It should be noted that, in this document, the terms "comprising," "including," and any other variations are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Specific examples have been used in this document to illustrate the principles and implementation methods of the present invention. These examples are merely for the purpose of helping to understand the method and core ideas of the present invention. The above descriptions are only preferred embodiments of the present invention. It should be pointed out that, due to the limitations of written expression and the objective existence of infinite specific structures, those skilled in the art can make several improvements, modifications, or variations without departing from the principles of the present invention, and can also combine the above technical features in an appropriate manner. These improvements, modifications, variations, or combinations, or the direct application of the concept and technical solution of the present invention to other situations without modification, should all be considered within the scope of protection of the present invention.

Claims

1. A coating process for fabricating abrasive coatings on a PET substrate, characterized in that, The process includes the following steps: coating a photocurable masterbatch onto a PET substrate to form a masterbatch layer, then performing photocuring to obtain a master film, wherein the masterbatch layer has micro-nano structures distributed on it; then coating a photocurable sub-adhesive onto the PET substrate and printing the micro-nano structures on the master film onto the sub-adhesive to form a sub-adhesive layer, then performing photocuring to obtain PET coated abrasive. The photocurable masterbatch is prepared by the following method: a mixture of toluene diisocyanate and 1,3-propanetriol diacrylate in a molar ratio of 1:1 is reacted, followed by a reaction with a diol oligomer to obtain polyurethane acrylate; then, the polyurethane acrylate, photocurable monomer, photoinitiator, silane coupling agent, and release agent are mixed to obtain the photocurable masterbatch; the photocurable monomer is composed of tripropylene glycol diacrylate, N-acryloylmorpholine, and tetrahydrofuran acrylate in a mass ratio of 4:1~1.5:0.8~1.2, and the silane coupling agent is composed of γ-glycidyl ether propyltrimethoxysilane and tert-butyltrimethoxysilane in a mass ratio of 3~4:1.8~2.4; the molar ratio of toluene diisocyanate to the diol oligomer is 1:0.5, and the chemical structure of the diol oligomer is as follows: ; The photocurable sub-adhesive is prepared by the following method: toluene diisocyanate and 1,3-propanetriol diacrylate are mixed and reacted in a molar ratio of 1:1, and then mixed and reacted with diol oligomers to obtain polyurethane acrylate, wherein the molar ratio of toluene diisocyanate and diol oligomers is 1:0.5; then the polyurethane acrylate, photocurable monomer, photoinitiator, defoamer, leveling agent, dispersant, anti-settling agent and abrasive are mixed evenly to obtain the photocurable sub-adhesive; the photocurable monomer is composed of tripropylene glycol diacrylate, (4) bisphenol A diacrylate, N-acryloylmorpholine and tetrahydrofuran acrylate in a mass ratio of 3~4:2~3:1~1.5:1.2~1.8, and the chemical structure of the diol oligomer is as follows: 。 2. The coating process for fabricating abrasive coatings on a PET substrate according to claim 1, characterized in that, The masterbatch layer is formed by coating the photocurable masterbatch onto the PET substrate using roller coating, which is performed using rollers with micro-nano structures.

3. The coating process for fabricating abrasive coatings on a PET substrate according to claim 1, characterized in that, The micro-nano structures on the roller are arranged in an array. The micro-nano structures are regular square pyramid structures with a base side length of 200~300μm and a cone depth of 20~50μm.

4. The coating process for fabricating abrasive coatings on a PET substrate according to claim 1, characterized in that, The amount of masterbatch used for coating is 40~70g / m². 2 The photocuring energy is 320~400mJ / cm. 2 The amount of adhesive used for coating is 90~120g / m². 2 The photocuring energy is 430~500mJ / cm. 2 .

5. The coating process for fabricating abrasive coatings on a PET substrate according to claim 1, characterized in that, When preparing the masterbatch, the mass ratio of polyurethane acrylate, photocurable monomer and silane coupling agent is 75~80:15.5~17:0.5~0.

8.

6. The coating process for fabricating abrasive coatings on a PET substrate according to claim 1, characterized in that, When preparing the masterbatch, the mass ratio of polyurethane acrylate, photocurable monomer, photoinitiator, silane coupling agent and release agent is 75~80:15.5~17:7~9:0.5~0.8:2~3.

7. The coating process for fabricating abrasive coatings on a PET substrate according to claim 1, characterized in that, When preparing the abrasive, the abrasive is composed of aluminum oxide and silicon carbide in a mass ratio of 6~8:4~6.

8. The coating process for fabricating abrasive coatings on a PET substrate according to claim 1, characterized in that, The average particle size of the aluminum oxide is 10~15μm, and the average particle size of the silicon carbide is 5~8μm.

9. The coating process for fabricating abrasive coatings on a PET substrate according to claim 1, characterized in that, When preparing the adhesive, the mass ratio of polyurethane acrylate, photocurable monomer, photoinitiator, defoamer, leveling agent, dispersant, antisettling agent and abrasive is 20~40:20~30:4~8:0.2~2:0.1~0.5:0.5~1.5:0.2~1:50~70.

10. The coating process for fabricating abrasive coatings on a PET substrate according to claim 1, characterized in that, When preparing the adhesive, UV color paste is also added; the mass ratio of polyurethane acrylate, photocurable monomer, photoinitiator, defoamer, leveling agent, dispersant, anti-settling agent, abrasive and UV color paste is 20~40:20~30:4~8:0.2~2:0.1~0.5:0.5~1.5:0.2~1:50~70:0.001~0.5.