A method for controlling the uniformity of powder filling in a silicon carbide-lined annular mold cavity
By establishing compression ratio-density response curves and non-uniform filling control, the problem of uneven density in the annular mold cavity of silicon carbide ceramic liner was solved, thereby improving density uniformity and product quality.
Patent Information
- Application Number
- CN202611275187.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-17
AI Technical Summary
During the powder filling process of the annular mold cavity of silicon carbide ceramic lining, there are differences in compression ratio due to the step or variable cross-section structure, resulting in uneven density, which in turn affects the wear resistance and thermal shock resistance of the ceramic lining, and may even lead to warping deformation and cracking.
By establishing a compression ratio-density response curve, the required initial powder filling amount for each region is calculated in reverse, a spatial distribution map is generated, and non-uniform filling is achieved through control commands of the sprinkling mechanism. Combined with a laser displacement sensor for real-time adjustment and step-by-step pressing process, density uniformity is ensured.
It effectively reduces the root causes of density unevenness, improves the product quality and service reliability of silicon carbide ceramic liners, reduces the risk of warping and cracking, and improves density uniformity.
Smart Images

Figure CN123103848A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of ceramic forming process control technology, specifically a method for controlling the uniformity of powder filling in a silicon carbide-lined annular mold cavity. Background Technology
[0002] Silicon carbide ceramic liners are widely used in annular cavity components that need to withstand strong wear, high temperature, or corrosive environments in fields such as special equipment for ceramic product manufacturing due to their excellent wear resistance, corrosion resistance, and high temperature stability. In the powder filling molding process of annular mold cavities for silicon carbide ceramic liners, a uniform material distribution method is usually adopted. That is, a feeding mechanism that rotates at a uniform speed around the central axis of the annular mold cavity spreads silicon carbide powder in various areas of the annular mold cavity at a uniform feeding speed and amount. Then, the powder is pressed into a ceramic liner green body of the required shape through a pressing process. Since the process can realize the near-net-shape production of silicon carbide ceramic liners in batches, it has significant advantages such as high material utilization, high production efficiency, and suitability for molding complex-shaped products. It has become one of the mainstream process routes for the preparation of silicon carbide ceramic liners.
[0003] However, in actual production using the uniform material distribution process, the compression ratios of complex annular mold cavities with steps or variable cross-sections differ in different areas during subsequent pressing. At the root of the step, the abrupt change in cross-section, and the side of the mandrel, powder flow is obstructed during pressing, resulting in a much smaller actual compression than other areas. Because the uniform material distribution process ensures the same initial filling height of the powder throughout the annular mold cavity, areas with high compression ratios form higher densities after pressing, while areas with low compression ratios have lower densities. This leads to a severely uneven overall density distribution in the annular ceramic liner green body. Consequently, areas with high density experience greater shrinkage during subsequent sintering, while areas with low density experience less shrinkage. This mismatch in shrinkage directly causes warping, internal microcracks, and even cracking and scrapping of the ceramic liner. Simultaneously, low-density areas struggle to achieve the target density after sintering, reducing the wear resistance and thermal shock resistance of the ceramic liner and directly impacting the service life and operational reliability of specialized equipment for ceramic product manufacturing.
[0004] Therefore, the present invention provides a method for controlling the uniformity of powder filling in a silicon carbide-lined annular mold cavity. Summary of the Invention
[0005] In order to overcome the shortcomings of the prior art, at least one technical problem raised in the background art is solved.
[0006] The technical solution adopted by this invention to solve its technical problem is: a method for controlling the uniformity of powder filling in a silicon carbide-lined annular mold cavity, comprising the following steps:
[0007] Obtain the geometric parameters of the annular mold cavity, establish the compression ratio distribution model of each region of the annular mold cavity, and obtain the final compression density of each region of the annular mold cavity under different compression ratio conditions through finite element simulation, thus forming the compression ratio-density response curve of each region.
[0008] Based on the compression ratio-density response curves of each region, and combined with the final compression density target value, the initial powder filling amount required for each region of the annular mold cavity to achieve the final compression density target value is calculated in reverse, and the spatial distribution map of the initial powder filling amount required for each region of the annular mold cavity is obtained.
[0009] The control instructions for the feeding mechanism are generated based on the initial powder filling amount and spatial distribution map. The control instructions include the feeding speed setting value, residence time setting value and powder release amount setting value at different circumferential angle positions.
[0010] Based on control commands, the powder feeding mechanism is controlled to perform powder filling operations, so that the powder forms a preset non-uniform initial distribution in the annular mold cavity that conforms to the spatial distribution pattern. The powder in the annular mold cavity after filling is pressed and shaped, so that each area of the annular mold cavity reaches the final pressing density target value after undergoing a pressing process with different compression ratios.
[0011] The beneficial effects of this invention are as follows:
[0012] This invention proposes a reverse control method to compensate for the compression ratio difference during the pressing stage by using spatial non-uniform filling. By establishing the compression ratio-density response curve of each region, the originally invisible compression ratio difference is transformed into engineering data. Then, by calculating the required initial powder filling amount for each region in reverse, a spatial distribution map is generated, so that regions with a large compression ratio receive a larger initial filling amount and regions with a small compression ratio receive a smaller initial filling amount. This allows for pre-compensation of the compression ratio difference during the filling stage, i.e., the pressing stage, fundamentally reducing the root cause of density inhomogeneity.
[0013] This invention constructs a closed-loop control system covering the entire chain from theoretical calculation to engineering execution. By converting spatial distribution maps into formatted control commands for the dispensing mechanism, differentiated filling schemes can be implemented on actual equipment. During the filling process, the actual filling height at each circumferential angle position is measured in real time using a laser displacement sensor or a laser contour scanner. When a deviation is detected that exceeds the allowable range, the adjacent positions are immediately adjusted to compensate for it. This resists the interference of mechanical positioning errors of the dispensing mechanism and fluctuations in powder flowability on the preset filling amount, enabling high-fidelity realization of the spatial distribution map at the engineering level.
[0014] This invention employs a step-by-step pressing process in the pressing and molding stage, allowing the powder to initially solidify under low pressure to form a powder layer with a certain strength. Through mold wall lubrication treatment, the frictional resistance between the powder and the mold wall in the subsequent final pressing stage is significantly reduced, suppressing the lateral flow of the powder caused by mold wall friction in the high-pressure final pressing stage. This makes the powder in each area closer to the ideal state of in-situ compression, thereby ensuring that the non-uniform distribution pattern preset in the filling stage can be accurately transformed into a uniform density distribution after pressing, improving the product quality and service reliability of silicon carbide ceramic liners. Attached Figure Description
[0015] The invention will now be further described with reference to the accompanying drawings.
[0016] Figure 1 This is a flowchart of the steps in an embodiment of the present invention;
[0017] Figure 2 This is a flowchart of the judgment process in step S1 of this embodiment of the invention;
[0018] Figure 3 This is a flowchart of the judgment process in step S2 of this embodiment of the invention;
[0019] Figure 4 This is a flowchart of the judgment process in step S3 of this embodiment of the invention;
[0020] Figure 5 This is a flowchart of the judgment process in step S4 of this embodiment of the invention. Detailed Implementation
[0021] To make the technical means, creative features, objectives and effects of this invention easier to understand, the invention will be further described below in conjunction with specific embodiments.
[0022] Example
[0023] Please see Figures 1-5 As shown in the embodiment of the present invention, a method for controlling the uniformity of powder filling in a silicon carbide-lined annular mold cavity includes the following steps:
[0024] Step S1: Obtain the geometric structural parameters of the annular mold cavity, establish the compression ratio distribution model of each region of the annular mold cavity, and obtain the final compression density corresponding to each region of the annular mold cavity under different compression ratio conditions through finite element simulation, forming the compression ratio-density response curve of each region.
[0025] Obtain the design drawings or three-dimensional digital model of the annular mold cavity to be filled with silicon carbide ceramic lining, and extract the geometric structural parameters of the annular mold cavity from the design drawings or three-dimensional digital model.
[0026] Among them, the geometric structural parameters include at least: wall thickness distribution data at various circumferential angle positions of the annular mold cavity, cross-sectional change data at various height positions from top to bottom along the axial direction of the annular mold cavity, and position coordinates and corresponding transition fillet size data of all step transition areas on the inner wall surface of the annular mold cavity;
[0027] Based on the obtained geometric parameters, the annular cavity is divided into multiple discrete evaluation regions;
[0028] Specifically, the division method is as follows: along the circumference of the annular mold cavity, the annular mold cavity is divided into multiple circumferential sectors at preset angle intervals; along the axial direction of the annular mold cavity, the annular mold cavity is divided into multiple axial layers at preset height intervals; along the wall thickness direction of the annular mold cavity, the annular mold cavity is divided into multiple thickness layers at preset thickness intervals.
[0029] The circumferential sector, axial layer and thickness layer are spatially combined to form multiple discrete evaluation regions. Each evaluation region has a unique spatial coordinate position and corresponding local geometric features.
[0030] For each evaluation area, the compression ratio in the subsequent compression molding process is determined separately;
[0031] Specifically, the compression ratio is determined as follows: obtain the initial filling height of the evaluation area after the powder filling is completed, obtain the target pressing height of the evaluation area after pressing is completed, divide the difference between the initial filling height and the target pressing height by the initial filling height, and the resulting ratio is the compression ratio of the evaluation area.
[0032] The compression ratio calculations for all evaluation areas are completed sequentially to obtain the compression ratio distribution data for the entire annular cavity, thus forming a compression ratio distribution model.
[0033] Based on the geometric parameters of the annular mold cavity and the compression ratio distribution model, a finite element model for preventing the compression molding of powder in the annular mold cavity is constructed.
[0034] Specifically: A three-dimensional geometric model of the annular cavity is established in the finite element simulation software. The three-dimensional geometric model is then meshed according to the evaluation area division method, so that each mesh element in the finite element simulation model corresponds to the evaluation area.
[0035] Set the material property parameters of silicon carbide powder in the finite element simulation model;
[0036] Among them, the material property parameters include: particle size distribution parameters of silicon carbide powder, friction coefficient between powder and inner wall of annular mold cavity, and compression characteristics of powder under different pressing pressures;
[0037] The material property parameters of silicon carbide powder are obtained through the following methods:
[0038] A standard cylindrical test mold is provided. Under the same pressing conditions as the annular mold cavity, multiple sets of calibration pressing experiments with different pressing pressures are carried out on silicon carbide powder. The correspondence between the actual pressing density and the compression ratio of the powder under each calibration experiment is measured. The material property parameters in the finite element simulation model are corrected with the calibration experiment results, so that the error between the predicted pressing density output by the simulation model under the same compression ratio conditions and the actual pressing density measured in the calibration experiment is controlled within the preset tolerance range.
[0039] Preferably, the preset tolerance range is ±3% of the measured compression density value;
[0040] Take any evaluation area as the target analysis area;
[0041] Keeping the boundary conditions of other evaluation regions outside the target analysis region unchanged, the compression ratio of the target analysis region is gradually increased from the minimum preset value to the maximum preset value. Each step adds a fixed compression ratio increment. The final compression density of the target analysis region after the simulation compression is completed under each compression ratio condition is recorded. The above operation is repeated until the simulation of each evaluation region under different compression ratio conditions is completed, and multiple sets of corresponding data of compression ratio and final compression density for each evaluation region are obtained.
[0042] The fixed compression ratio increment is set as follows: based on the total number of evaluation regions obtained and the overall span of the compression ratio change amplitude shown by each evaluation region in the compression ratio distribution model, the overall span of the compression ratio change amplitude is multiplied by a preset discretization coefficient and then divided by the product of the total number of evaluation regions and the preset sampling rate factor to obtain the fixed compression ratio increment.
[0043] Preferably, the preset discretization coefficient is between 0.1 and 0.5, and the preset sampling factor is between 5 and 20, so that the compression ratio increment corresponding to each simulation step is sufficient to form no less than the preset number of sampling points on the compression ratio-density response curve, thereby ensuring the accuracy of subsequent curve fitting, while avoiding the overall efficiency being affected by excessive simulation calculation due to too small compression ratio increment.
[0044] For each evaluation region, a corresponding compression ratio-density response curve is fitted, where the compression ratio is the x-axis and the final compressed density is the y-axis.
[0045] It should be noted that the compression ratio-density response curve characterizes the density response properties of the evaluation region under different compression ratio conditions.
[0046] Step S1 extracts the geometric structural parameters of the annular mold cavity, establishes a compression ratio distribution model for each region, and uses finite element simulation to obtain density response data for each region under different compression ratio conditions, forming a complete set of compression ratio-density response curves. Its purpose is to transform the inherent, originally invisible compression ratio differences of the annular mold cavity due to geometric features such as steps and variable cross sections into engineering data, so that the subsequent control strategy of pre-setting differentiated filling amounts for different compression ratio regions has a quantitative basis, fundamentally supporting the realization of compensating for compression ratio differences with spatial non-uniform filling.
[0047] Step S2: Based on the compression ratio-density response curve of each region, and combined with the final compression density target value, calculate the initial powder filling amount required for each region of the annular mold cavity to achieve the final compression density target value, and obtain the spatial distribution map of the initial powder filling amount required for each region of the annular mold cavity.
[0048] Among them, the spatial distribution map represents the filling amount configuration scheme in which the powder is distributed non-uniformly along the circumference and axial direction in the annular mold cavity.
[0049] Obtain the final pressing density target value of the annular mold cavity for silicon carbide ceramic liner. The final pressing density target value is a uniform density target value that should be achieved by each area of the annular mold cavity after pressing and molding, which is pre-set according to the performance requirements of silicon carbide ceramic liner.
[0050] For each assessment area;
[0051] Extract the corresponding compression ratio-density response curve, use the final density suppression target value as the target value on the vertical axis, find the corresponding horizontal axis value, and use it as the target compression ratio required to achieve the final suppression density target value in the evaluation area.
[0052] Based on the target compression ratio, the initial powder filling amount required for the evaluation area is calculated in reverse.
[0053] Specifically, the calculation process for the initial powder filling amount is as follows:
[0054] The target pressing height of the evaluation area after pressing and molding is obtained. The target pressing height is determined by the cross-sectional change data in the geometric parameters of the annular mold cavity.
[0055] Since the compression ratio is equal to the difference between the initial fill height and the target compression height divided by the initial fill height, it can be deduced that the initial fill height is the difference between the target compression height divided by one and the target compression ratio.
[0056] The initial filling height is expressed by the target compression height and the target compression ratio, and the required initial powder filling height for the evaluation area is calculated.
[0057] The initial powder filling height is multiplied by the projected area of the evaluation area on the horizontal plane to obtain the initial powder filling volume required for the evaluation area, i.e., the initial powder filling amount.
[0058] Identify whether there are negative or zero values in the initial powder filling amount of each evaluation area within the annular mold cavity;
[0059] If the initial powder filling amount of the evaluation area is negative or zero, it indicates that the evaluation area cannot achieve the final compaction density target value by adjusting the initial filling amount under the current geometric conditions. At this time, a prompt message is output, suggesting that the local geometric parameters of the evaluation area be modified or the final compaction density target value be reduced.
[0060] If the initial powder filling amount in all evaluation areas is positive, then the current solution is deemed feasible.
[0061] The initial powder filling amount of all evaluation areas is arranged and combined according to the spatial coordinate position of each evaluation area to form a spatial distribution map of the initial powder filling amount of the entire annular mold cavity.
[0062] In the spatial distribution map, each spatial coordinate position corresponds to an initial powder filling amount value. The initial powder filling amount values at different spatial coordinate positions show a differentiated distribution along the circumference and axial direction of the annular mold cavity. Specifically, the evaluation area with a large compression ratio corresponds to a larger initial powder filling amount value, while the evaluation area with a small compression ratio corresponds to a smaller initial powder filling amount value. This achieves the purpose of compensating for the compression ratio difference in the pressing stage with the spatial non-uniform distribution in the filling stage.
[0063] The purpose of step S2 is to convert the requirement of uniform final product density into the initial powder filling amount required for each region of the annular mold cavity during the filling stage through the compression ratio-density response curve, generate a spatial distribution map, and provide spatial distribution data input for the generation of control commands for the subsequent material feeding mechanism.
[0064] Step S3: Generate control instructions for the feeding mechanism based on the initial powder filling amount and spatial distribution map. The control instructions include the feeding speed setting value, residence time setting value, and powder release amount setting value at different circumferential angle positions.
[0065] Obtain the structural and operational parameters of the material dispensing mechanism;
[0066] The structural parameters include at least the effective distribution width of the discharge port of the sprinkling mechanism in the radial direction of the annular mold cavity and the effective distribution length of the discharge port in the axial direction of the annular mold cavity.
[0067] The operating parameters include at least the adjustable range of the angular velocity of the sprinkling mechanism rotating around the central axis of the annular mold cavity, the adjustable range of the feeding speed at the discharge port, and the maximum instantaneous powder release from the discharge port;
[0068] Based on the spatial distribution map of the initial powder filling amount, the initial powder filling amount of each evaluation area of the annular mold cavity is grouped and merged according to the circumferential angle coordinates in the spatial distribution map;
[0069] The initial powder filling amounts of all axial and thickness layer evaluation areas belonging to the same circumferential angular coordinate are summed to obtain the total powder filling amount required at the circumferential angular position;
[0070] The cumulative calculation of all circumferential angle positions is completed sequentially to obtain the total powder filling amount distribution data required for each circumferential angle position along the entire circumference of the annular mold cavity;
[0071] The effective distribution width of the material spraying mechanism's outlet is taken as the effective coverage range of the material spraying mechanism in the radial direction of the annular mold cavity in a single operation.
[0072] Based on the wall thickness of the annular mold cavity and the effective distribution width of the discharge port, determine the number of times the spraying mechanism needs to complete the total powder filling at each circumferential angle position. The number of spraying times is the value obtained by dividing the wall thickness of the annular mold cavity at the circumferential angle position by the effective distribution width of the discharge port and rounding it up.
[0073] The ratio of the total amount of powder required at each circumferential angle position to the number of times of powder application is required at each circumferential angle position is used as the amount of powder that the powder application mechanism needs to release in each application stroke at each circumferential angle position.
[0074] It should be noted that when the total powder filling amount cannot be divided evenly by the number of spraying strokes, the remainder is evenly distributed to the first few spraying strokes or to the last spraying stroke, so that the sum of the powder release amount of all spraying strokes equals the total powder filling amount.
[0075] The amount of powder to be released is set as the powder release amount for each spraying stroke at the circumferential angle position;
[0076] For each circumferential angular position of the spreading mechanism, the actual residence time set value required for the spreading stroke is calculated. The process is as follows:
[0077] Obtain the rotation angle difference between two adjacent circumferential angle positions of the spraying mechanism, obtain the rated rotational angular velocity of the spraying mechanism rotating around the central axis of the annular mold cavity, divide the rotation angle difference by the rated rotational angular velocity, and obtain the rotational movement time required for the spraying mechanism to move from the current circumferential angle position to the next circumferential angle position;
[0078] Obtain the rated feeding speed of the discharge port of the sprinkling mechanism, obtain the set value of the powder release amount for each sprinkling stroke at the circumferential angle position, divide the set value of the powder release amount by the rated feeding speed, and obtain the theoretical residence time required for the sprinkling mechanism to complete one sprinkling stroke at the circumferential angle position.
[0079] The start-up acceleration time and stop-deceleration time of the discharge port of the feeding mechanism are obtained, and the start-up acceleration time and stop-deceleration time are averaged to obtain the average acceleration and deceleration compensation time.
[0080] Add the theoretical residence time to the average acceleration / deceleration compensation time to obtain the actual residence time setting value for each feeding stroke at the circumferential angle position;
[0081] The rotational movement time and actual dwell time settings are arranged and combined according to the movement sequence of the spreading mechanism through each circumferential angle position to form a sequence of dwell time settings for the spreading mechanism at each circumferential angle position.
[0082] The actual residence time set value sequence of the sprinkling mechanism at each circumferential angle position is obtained. Under the premise that the rated feeding speed of the discharge port remains unchanged, the amount of powder to be released at each circumferential angle position is evenly distributed to the corresponding actual residence time. The proportion of the discharge port opening time to the actual residence time corresponding to each circumferential angle position is used as the feeding speed set value at the position.
[0083] The powder release amount setting value, feeding speed setting value and residence time setting value at each circumferential angle position for each spraying stroke are encoded and converted according to the motion sequence of the spraying mechanism to generate a formatted control command that can be directly read and executed by the control system of the spraying mechanism.
[0084] The formatted control instructions include at least the positioning information for each circumferential angular position, the feeding speed setting, the residence time setting, and the powder release setting.
[0085] Step S3 serves to transform the spatial distribution map, which represents the spatial distribution data of the required powder filling amount in each area of the annular mold cavity, into specific control instructions that the programmable spraying mechanism can recognize and execute. By merging the initial powder filling amount of the evaluation area to each circumferential angle position, calculating the single spraying release amount, matching the rotation movement time and dwell time, and finally encoding and generating formatted instructions, the connection between theoretical calculation data and engineering execution instructions is realized, enabling differentiated filling schemes to be implemented on actual equipment through the spraying mechanism.
[0086] Step S4: Based on the control command, control the powder feeding mechanism to perform the powder filling operation, so that the powder forms a preset non-uniform initial distribution in the annular mold cavity that conforms to the spatial distribution pattern. After the powder in the annular mold cavity is filled, it is pressed and shaped so that each area of the annular mold cavity reaches the final pressing density target value after undergoing the pressing process with different compression ratios.
[0087] The format control command is obtained and read. It is then determined whether the sum of the powder release setpoints at all circumferential angle positions is consistent with the total initial powder filling amount in the entire area of the spatial distribution map. If they are consistent, the verification is successful. If they are inconsistent, an alarm signal is output and execution is terminated.
[0088] The control mechanism for dispensing material begins to rotate around the central axis of the annular mold cavity according to the circumferential angle position sequence in the formatted control instructions. The dispensing mechanism starts from the starting position and passes through each circumferential angle position defined in the formatted control instructions in sequence.
[0089] When the material spreading mechanism reaches a certain circumferential angle position;
[0090] The dispensing mechanism is controlled to perform a dwell operation according to the corresponding dwell time setting value. During the dwell operation, the opening degree of the dispensing mechanism outlet is controlled according to the corresponding feeding speed setting value, so that the dispensing mechanism releases powder at the set feeding speed within the dwell time, and the amount of powder released is equal to the corresponding powder release amount setting value. When the dwell time ends, the dispensing mechanism outlet is controlled to close, completing the dispensing stroke at the circumferential angle position.
[0091] After completing the spraying stroke at the current circumferential angle position, the spraying mechanism is controlled to rotate and move to the next circumferential angle position at the rated rotational angular velocity according to the positioning information of the next circumferential angle position in the formatted control command.
[0092] During the rotation and movement, the discharge port of the feeding mechanism remains closed and does not release powder.
[0093] After the material spraying mechanism reaches the next circumferential angle position, it stops spraying. This process is repeated, and the material spraying operation is completed sequentially at all circumferential angle positions according to the order of the circumferential angle positions in the formatted control instructions.
[0094] After the material spraying mechanism completes the spraying operation at all circumferential angle positions, it is controlled to return to the starting position to complete the powder filling operation;
[0095] It is important to note that after the dispensing mechanism completes the dispensing stroke at each circumferential angle position, the actual filling height of the powder surface at the circumferential angle position is measured by a laser displacement sensor or laser contour scanner installed above the annular mold cavity. The actual filling height is compared with the corresponding preset initial powder filling height, and the deviation value of the filling height is calculated. If the deviation value exceeds the preset allowable deviation range, it is determined that there is a filling amount deviation. When the dispensing mechanism subsequently rotates to the adjacent circumferential angle position, the powder release amount setting value at the adjacent position is adjusted compensatorily according to the deviation value, so that the powder release amount at the adjacent position is increased or decreased by the compensation amount corresponding to the deviation value based on the original setting value.
[0096] Preferably, the allowable deviation range is ±5% of the preset initial powder filling height at the corresponding circumferential angle position;
[0097] The amount of powder received by each area in the annular mold cavity is distributed according to the set value of powder release corresponding to each circumferential angle position. The initial filling amount of powder at each circumferential angle position in the annular mold cavity is different, and the overall shape presents a preset non-uniform initial distribution pattern that conforms to the spatial distribution pattern. That is, the initial powder filling amount corresponding to the area with a large compression ratio in the annular mold cavity is greater than the initial powder filling amount corresponding to the area with a small compression ratio.
[0098] After the powder filling is completed, pressing pressure is applied to the powder in the annular mold cavity to press and shape it;
[0099] It should be noted that the compression molding process adopts a step-by-step compression process. In the first step, a first compression pressure is applied to the powder in the annular mold cavity to bring the powder to a pre-compression state. In the pre-compression state, the powder is initially solidified in the annular mold cavity, but density differences still exist in different areas. After releasing the first compression pressure, lubrication treatment is applied to the inner wall of the annular mold cavity or a lubrication layer is preset on the inner wall of the annular mold cavity to reduce the frictional resistance between the powder and the mold wall in the subsequent final compression stage. In the second step, a second compression pressure is applied to the pre-compressed powder. The second compression pressure is greater than the first compression pressure, and the final compression molding is completed under the second compression pressure.
[0100] Preferably, the first pressing pressure is 20% to 40% of the second pressing pressure;
[0101] During the pressing process, the powder in each region of the annular mold cavity is compressed from its initial filling height to its target pressing height. The compression ratio of each region is different. The powder in the region with a large compression ratio is compressed to a greater extent, while the powder in the region with a small compression ratio is compressed to a lesser extent.
[0102] Because areas with high compression ratios are pre-filled with a larger initial powder amount during the filling stage, while areas with low compression ratios are pre-filled with a smaller initial powder amount, the final density achieved by each area after pressing is close to the set final pressing density target value, thus making the overall density distribution of the silicon carbide ceramic lining green body more uniform.
[0103] Step S4 serves to: convert the formatted control commands into actual mechanical actions through the dispensing mechanism, causing the powder to form a preset non-uniform initial distribution within the annular mold cavity that conforms to the spatial distribution pattern. This realizes the transformation from data to physical form of the theoretical scheme of compensating for compression ratio differences through spatial non-uniform filling. During the filling process, the actual filling height at each circumferential angle position is detected online using a laser displacement sensor or laser contour scanner, and the detected filling height deviation is fed back to the subsequent dispensing stroke through adjacent compensation, forming a closed loop in the filling stage. This effectively resists the interference of mechanical positioning errors of the dispensing mechanism and powder flowability fluctuations on the preset filling amount. In the pressing and molding stage... By employing a step-by-step pressing process—first, low-pressure pre-compression to initially solidify the powder, then releasing the pressure and applying lubrication to the inner wall of the mold cavity to reduce frictional resistance, and finally applying high pressure to complete the final compression—the lateral flow of the powder due to mold wall friction during the final compression stage is reduced. This process brings the powder in each region closer to the ideal state of in-situ compression, ensuring that the non-uniform distribution pattern preset in the filling stage can be effectively transformed into a uniform density distribution after pressing. Under the online compensation mechanism in the filling stage and the step-by-step pressing action in the pressing stage, after experiencing their respective compression ratios, the final density of each region of the annular mold cavity approaches the set final pressing density target value, making the overall density distribution of the silicon carbide ceramic liner green body more uniform.
[0104] This embodiment replaces global uniform filling with spatial non-uniform filling, fundamentally optimizing the problem of uneven pressing density caused by geometric features such as steps and variable cross-sections in the annular mold cavity. Through the closed-loop control logic of steps S1 to S4, especially the introduction of online deviation detection and adjacent compensation mechanisms during the filling process, and the use of step-by-step pressing and lubrication assistance during the pressing stage, it effectively resists the interference of powder batch fluctuations, mechanical errors of the feeding mechanism, and lateral flow of powder during the pressing process on the preset distribution pattern. The silicon carbide ceramic liner green body obtained by filling and pressing in this embodiment can control the density difference of each region along the circumference and axial direction within a reasonable range of the target density value, and the density uniformity is significantly improved. The warping deformation rate and cracking scrap rate of the annular ceramic liner in the subsequent sintering process are reduced.
[0105] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method of controlling the uniformity of powder fill of a silicon carbide lined annular die cavity, the method comprising: Includes the following steps: Obtain the geometric parameters of the annular mold cavity, establish the compression ratio distribution model of each region of the annular mold cavity, and obtain the final compression density of each region of the annular mold cavity under different compression ratio conditions through finite element simulation, thus forming the compression ratio-density response curve of each region. Based on the compression ratio-density response curves of each region, and combined with the final compression density target value, the initial powder filling amount required for each region of the annular mold cavity to achieve the final compression density target value is calculated in reverse, and the spatial distribution map of the initial powder filling amount required for each region of the annular mold cavity is obtained. The control instructions for the feeding mechanism are generated based on the initial powder filling amount and spatial distribution map. The control instructions include the feeding speed setting value, residence time setting value and powder release amount setting value at different circumferential angle positions. Based on control commands, the powder feeding mechanism is controlled to perform powder filling operations, so that the powder forms a preset non-uniform initial distribution in the annular mold cavity that conforms to the spatial distribution pattern. The powder in the annular mold cavity after filling is pressed and shaped, so that each area of the annular mold cavity reaches the final pressing density target value after undergoing a pressing process with different compression ratios.
2. A method of controlling the uniformity of filling of a powder into a ring-shaped mold cavity lined with silicon carbide according to claim 1, characterized in that: The process of establishing the compression ratio distribution model is as follows: The annular mold cavity is divided into multiple discrete evaluation regions along the circumferential, axial and wall thickness directions. For each evaluation region, the initial filling height and the target pressing height after the powder filling are obtained. The difference between the initial filling height and the target pressing height is divided by the initial filling height to obtain the compression ratio of the evaluation region. The compression ratio of all evaluation areas is calculated sequentially to form a compression ratio distribution model.
3. The method for controlling the uniformity of powder filling in a silicon carbide-lined annular mold cavity according to claim 1, characterized in that: The process of obtaining the compression ratio-density response curve is as follows: A three-dimensional geometric model of the annular cavity is established in the finite element simulation software. The three-dimensional geometric model is meshed according to the evaluation region division method. The material property parameters of silicon carbide powder are set in the finite element simulation model. For any evaluation region as the target analysis region, keep the boundary conditions of other evaluation regions outside the target analysis region unchanged, and increase the compression ratio of the target analysis region from the minimum preset value to the maximum preset value according to a fixed compression ratio increment. Record the final compression density of the target analysis region after the simulation compression is completed under each compression ratio condition. Obtain multiple sets of data corresponding to compression ratio and final compression density for each evaluation area, and fit the corresponding compression ratio-density response curve.
4. The method for controlling the uniformity of powder filling in a silicon carbide-lined annular mold cavity according to claim 1, characterized in that: The process of obtaining the spatial distribution map is as follows: Based on the target compression ratio, the target compression height of the evaluation area after compression molding is obtained. Since the compression ratio is equal to the difference between the initial filling height and the target compression height divided by the initial filling height, it is deduced that the initial filling height is the target compression height divided by one minus the difference of the target compression ratio. The initial powder filling height required for the evaluation area is calculated. The initial powder filling height is multiplied by the projected area of the evaluation area on the horizontal plane to obtain the initial powder filling amount required for the evaluation area. The initial powder filling amount of all evaluation areas is arranged and combined according to the spatial coordinate position of each evaluation area to form a spatial distribution map of the initial powder filling amount of the entire annular mold cavity.
5. The method for controlling the uniformity of powder filling in a silicon carbide-lined annular mold cavity according to claim 4, characterized in that: The process of obtaining the target compression ratio is as follows: Obtain the final target value of the compression density of the annular mold cavity lined with silicon carbide ceramic; For each evaluation region, the corresponding compression ratio-density response curve is extracted. The final compression density target value is used as the target value on the vertical axis, and the corresponding horizontal axis value is found as the target compression ratio required for the evaluation region to achieve the final compression density target value.
6. The method for controlling the uniformity of powder filling in a silicon carbide-lined annular mold cavity according to claim 1, characterized in that: The process for obtaining the powder release rate setpoint is as follows: The initial powder filling amounts of all axial and thickness layer evaluation areas under the same circumferential angular coordinate are summed to obtain the total powder filling amount; The number of spraying times is obtained by dividing the wall thickness of the annular cavity at the circumferential angle position by the effective distribution width of the discharge port and rounding it up. The ratio of the total amount of powder required at each circumferential angle position to the number of times of powder application is required at each circumferential angle position is used as the set value for the amount of powder released per application stroke at each circumferential angle position.
7. The method for controlling the uniformity of powder filling in a silicon carbide-lined annular mold cavity according to claim 6, characterized in that: The process of obtaining the dwell time setting value is as follows: Divide the powder release rate setting by the rated feeding speed of the discharge port of the spraying mechanism to obtain the theoretical dwell time required for the spraying mechanism to complete the current spraying stroke at this circumferential angle position; The start-up acceleration time and stop-deceleration time of the discharge port of the feeding mechanism are obtained, and the start-up acceleration time and stop-deceleration time are averaged to obtain the average acceleration and deceleration compensation time. The theoretical residence time is added to the average acceleration / deceleration compensation time to obtain the actual residence time setting for each feeding stroke at the circumferential angle position.
8. The method for controlling the uniformity of powder filling in a silicon carbide-lined annular mold cavity according to claim 7, characterized in that: The process of obtaining the feeding speed setpoint is as follows: The rotational movement time and actual dwell time settings are arranged and combined according to the movement sequence of the spreading mechanism through each circumferential angle position to form a sequence of dwell time settings for the spreading mechanism at each circumferential angle position. The sequence of actual residence time settings for the feeding mechanism at each circumferential angle position is obtained. Under the premise that the rated feeding speed of the discharge port remains unchanged, the amount of powder to be released at each circumferential angle position is evenly distributed to the corresponding actual residence time. The proportion of the discharge port opening time to the actual residence time at each circumferential angle position is used as the feeding speed setting value at that position.
9. The method for controlling the uniformity of powder filling in a silicon carbide-lined annular mold cavity according to claim 1, characterized in that: Controlling the powder dispensing mechanism to perform powder filling operations includes: The control mechanism rotates around the central axis of the annular mold cavity according to the circumferential angle position sequence in the formatted control instructions, passing through each circumferential angle position in sequence; When the feeding mechanism reaches a certain circumferential angle position, it performs a dwell operation according to the corresponding dwell time setting value, and during the dwell period, it controls the opening degree of the discharge port according to the corresponding feeding speed setting value, so that the amount of powder released is equal to the corresponding powder release amount setting value. After completing the material spraying at the current circumferential angle position, control the spraying mechanism to rotate to the next circumferential angle position while keeping the outlet closed; after completing the spraying operation at all circumferential angle positions in sequence, control the spraying mechanism to return to the starting position to complete the powder filling operation.
10. The method for controlling the uniformity of powder filling in a silicon carbide-lined annular mold cavity according to claim 9, characterized in that: Controlling the powder dispensing mechanism to perform powder filling operations also includes: After the spraying mechanism completes the spraying stroke at each circumferential angle position, the actual filling height of the powder surface at the circumferential angle position is measured; the difference between the actual filling height and the preset initial powder filling height is calculated to obtain the deviation value of the filling height; if the deviation value exceeds the preset allowable deviation range, it is determined that there is a filling amount deviation. When the spraying mechanism rotates to the adjacent circumferential angle position, the powder release amount setting value at the adjacent position is adjusted compensatorily according to the deviation value.