A quartz glass-driven dry thermochemical mechanical processing system and method for silicon carbide crystals
By using quartz glass tools to conduct thermochemical reactions with silicon carbide at the solid-solid interface, the problems of dependence on liquid media and difficulty in controlling interface reactions in existing silicon carbide processing have been solved, achieving efficient and low-damage silicon carbide processing.
Patent Information
- Application Number
- CN202611322483.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing chemical mechanical processing technology for silicon carbide relies on hard abrasives and liquid grinding fluids. The processing is complex, making it difficult to achieve efficient and low-damage material removal, and the reaction state at the solid-solid interface is difficult to actively control.
Using quartz glass abrasives or cutting tools as reactive solid processing media, combined with off-axis lasers, resistance wires, or coaxial lasers for thermal assistance, the synergistic effect of thermal and mechanical energy promotes interfacial thermochemical reactions between quartz glass and silicon carbide at the solid-solid interface, weakening the strong covalent bonds of Si–C and achieving dry thermochemical machining.
Without the need for a liquid medium, it improves material removal efficiency and surface quality, simplifies the processing flow, reduces the risk of environmental pollution, and enables real-time temperature control and stable interface reaction in the processing area.
Smart Images

Figure CN123103885A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of ultra-precision machining technology for hard and brittle carbide crystals, specifically relating to a dry thermochemical mechanical machining system and method for silicon carbide crystals driven by quartz glass. Background Technology
[0002] Single-crystal silicon carbide possesses high hardness, high thermal conductivity, strong wear resistance, and high thermochemical stability, making it widely used in high-power semiconductor devices, precision optical components, and high-performance structural parts. However, the strong covalent bonds between Si and C within silicon carbide make the material hard, brittle, and chemically inert, resulting in extremely difficult processing and a high risk of surface breakage and subsurface damage. Current processing methods typically involve first removing machining allowances using diamond turning, grinding, or lapping, followed by chemical mechanical polishing (CMP) to eliminate the damage incurred earlier and obtain a high-quality surface. Although diamond turning, grinding, and lapping have high material removal capabilities, the action of hard tools or abrasives can easily cause localized spalling, microcracks, and subsurface damage, accompanied by tool or grinding wheel wear. CMP typically modifies the silicon carbide surface with chemical components such as oxidants, and then uses polishing pads and nano-abrasives to remove the reaction layer. While this method improves surface quality, it has low processing efficiency, and the preparation, transportation, recovery, waste treatment, and post-processing cleaning of the polishing slurry are complex. Therefore, existing processing methods still struggle to simultaneously achieve high material removal efficiency and low processing damage, and they are highly dependent on hard abrasives and liquid processing media. It is necessary to develop a processing technology that can synergistically carry out interfacial chemical reactions and mechanical removal, while taking into account processing efficiency, surface quality, and process simplicity.
[0003] Patent CN119820471B discloses a chemical mechanical grinding system and method for hard and brittle semiconductor wafers. This method uses an organic thermally decomposable oxidant, an organic photodecomposable oxidant, polyethylene glycol, glycerol, and vegetable oil to formulate an oil-based thermally active-photoactive composite grinding fluid, constructing a diamond abrasive wheel chemical mechanical grinding system with ultraviolet irradiation function. The grinding heat and ultraviolet irradiation energy induce the decomposition of the organic oxidant in the composite grinding fluid to generate active free radicals. Under the synergistic effect of mechanical stress, free radical oxidation reactions occur on the surface of hard and brittle semiconductor materials such as silicon carbide, forming an oxide layer with low hardness and low interfacial bonding strength. Subsequently, diamond abrasive grains are used to remove the oxide layer with low-load micro-cutting, thereby reducing processing damage caused by single mechanical grinding and ultimately improving material removal efficiency and surface quality. However, the chemical mechanical grinding method proposed in this patent still has the following limitations: (1) This method requires a continuous supply of oil-based active grinding fluid containing a variety of organic components and oxidants, and is equipped with a corresponding fluid supply device, which increases the processes of grinding fluid preparation, transportation, recycling, residue treatment and post-processing cleaning, making it difficult to form a completely dry processing environment; (2) This method adopts the material removal mechanism of "free radical oxidation modification - diamond abrasive mechanical removal". The chemical modification of the silicon carbide surface mainly depends on the active free radicals in the grinding fluid, while the removal of the modified layer mainly depends on the mechanical cutting of diamond abrasive. The chemical reaction and mechanical removal are undertaken by different media. It has not yet involved the processing method in which the processing tool body participates in the interfacial chemical reaction during the direct contact between the continuous solid processing tool and the single crystal silicon carbide, and promotes the removal of surface material in a coordinated manner under continuous relative motion and interfacial shearing.
[0004] Patent CN115816287B discloses a finishing apparatus and method for silicon carbide wafers. This apparatus integrates a photocatalytic component and an ultrasonic component into a chemical mechanical polishing (CMP) device, and employs a liquid polishing slurry containing nano-photocatalysts and polishing particles. During processing, ultraviolet light excites the nano-photocatalysts to generate oxidizing free radicals, promoting the formation of a relatively easily removable oxide layer on the surface of the single-crystal silicon carbide. Simultaneously, ultrasonic vibration is used to increase the kinetic energy and effective participation of the polishing particles, enhancing the mechanical removal of the oxide layer by the polishing particles, thereby improving material removal efficiency and processing precision. However, the finishing method still has the following limitations: (1) The processing requires the participation of polishing pad, liquid polishing liquid containing nano-photocatalyst and SiO2 polishing particles, and ultrasonic vibration. Material removal still depends on the mechanical action between free polishing particles in the liquid environment and the silicon carbide surface; (2) The device needs to be equipped with multiple functional components such as chemical mechanical polishing, photocatalysis, ultrasonic vibration, polishing liquid supply and polishing pad dressing. Each auxiliary action and the processing process need to be coordinated. The equipment composition and multi-field coordinated control are relatively complex; (3) The method improves the motion activity and effective participation of free polishing particles through ultrasonic vibration. The material removal state is affected to a certain extent by the dispersion, migration and effective contact state of photocatalyst and polishing particles in the polishing liquid. Therefore, it is difficult to establish a continuous, stable and controllable solid-solid reaction contact interface between the processing tool and single crystal silicon carbide.
[0005] Patent CN116214359B discloses a method for polishing single-crystal silicon carbide with photoelectrocatalytic enhanced bonded abrasive. The method first involves mixing, molding, sintering, and granulating diamond particles, piezoelectric luminescent materials, and photocatalytic materials to form a polymeric abrasive. This polymeric abrasive is then composited with a polymer matrix and hot-pressed to obtain a bonded abrasive polishing pad. During processing, the contact stress and friction between the polymeric abrasive and the single-crystal silicon carbide cause the piezoelectric luminescent material to emit light and excite the photocatalytic material. Simultaneously, combined with piezoelectric discharge, a polishing circuit, and an electrolyte-containing hydrogen peroxide polishing solution, the oxidation and softening of the single-crystal silicon carbide surface are enhanced, which is then mechanically removed by the bonded diamond abrasive. However, the method still has the following limitations: (1) Polymer abrasives need to be prepared by multiple processes such as mixing, molding, debinding, sintering, crushing and grading of diamond particles, piezoelectric light-emitting materials and photocatalytic materials, and further composite molding with polymer matrix. The material composition and preparation process of polishing tools are relatively complicated; (2) The processing process still requires the participation of solidified diamond abrasives, hydrogen peroxide polishing liquid containing electrolytes and polishing circuits. Material removal still depends on the mechanical action of hard diamond abrasives. At the same time, liquid chemical media and electrochemical conditions are required to assist surface oxidation. It still has a certain dependence on hard abrasives and liquid reaction media; (3) In this method, the chemical activation of the surface of single crystal silicon carbide is mainly driven by the piezoelectric light-emitting, photocatalytic and anodic oxidation effects generated by the force of polymer abrasives. Its reaction state is coupled with local contact stress, the force state of polymer abrasives and electrochemical conditions. It has not yet involved the use of an independent adjustable heat source to actively heat the processing area, and combined with real-time monitoring and feedback adjustment of the processing area temperature to continuously control the thermochemical reaction state of the solid-solid contact interface.
[0006] In summary, existing chemical mechanical processing (CMP) technologies for silicon carbide typically utilize hard abrasives such as diamond, free abrasive particles, and liquid grinding or polishing fluids to achieve material processing through the synergistic effect of surface chemical modification and mechanical removal. While these methods can reduce the processing difficulty of silicon carbide and improve material removal efficiency and surface quality to some extent, material removal still largely depends on the mechanical action of hard abrasive particles or free polishing particles. Furthermore, the use of liquid processing media adds steps such as fluid supply, recovery, residue treatment, and post-processing cleaning. In addition, the media or functional components responsible for chemical activation and mechanical removal in existing methods usually have a clear functional division, lacking the ability to utilize the solid processing tool itself to directly participate in the interfacial chemical reaction of silicon carbide, thus simultaneously promoting material removal during solid-solid contact. Moreover, there is still room for improvement in the active regulation and real-time feedback control of the thermochemical reaction state at the solid-solid contact interface. Summary of the Invention
[0007] To address the problems of existing silicon carbide chemical mechanical processing (CMP) processes still heavily reliant on hard abrasives such as diamond and liquid grinding or polishing fluids, and the difficulty in actively controlling the reaction state at the solid-solid interface due to the fact that chemical activation and mechanical removal are usually undertaken by different media or functional components, this invention provides a quartz glass-driven dry thermochemical mechanical processing system and method for silicon carbide crystals. This method uses a quartz glass abrasive or a monolithic quartz glass tool as the reactive solid processing medium. Without introducing liquid cutting fluid, grinding fluid, or polishing fluid, it employs off-axis laser, resistance wire, or coaxial laser for thermal assistance depending on the processing mode, combined with real-time temperature monitoring and feedback adjustment. This allows the quartz glass and silicon carbide to undergo an interfacial thermochemical reaction during solid-solid contact and continuous relative motion. Through the synergistic effect of thermal and mechanical energy, the strong covalent bonds of Si–C on the silicon carbide surface are weakened, promoting plastic removal of the surface material and achieving dry thermochemical mechanical processing of silicon carbide crystals.
[0008] To achieve the above objectives, the technical solution adopted by the present invention is as follows: In a first aspect, this invention proposes a quartz glass-driven dry thermochemical mechanical processing method for silicon carbide crystals. The method employs a quartz glass processing tool to dry process the silicon carbide crystal. The quartz glass tool forms a stable solid-solid interface with the silicon carbide. While performing mechanical action, the quartz glass tool participates in the thermochemical reaction at the processing interface. The Si-O structure on the quartz glass surface undergoes an interfacial thermochemical reaction with the silicon carbide surface layer, forming a C-O-Si chemical bridging structure. This induces the dynamic formation, fracture, and reconstruction of the C-O phase key bond structure, weakening the bonding stability of the strong Si-C covalent bonds on the silicon carbide surface layer. Under interfacial shearing, this promotes dislocation slip and plastic removal of the surface material.
[0009] As a further technical solution, the quartz glass-driven dry thermochemical mechanical processing method for silicon carbide crystals includes a surface grinding mode, an end face grinding mode, or a turning mode.
[0010] As a further technical solution, when the processing method is surface grinding, a side-axis laser generator is used to locally preheat the area to be processed in front of the grinding contact area.
[0011] As a further technical solution, when the processing method is end face grinding mode, a resistance wire heating device is used to stably maintain the overall temperature of the silicon carbide workpiece within the set value of 25~500 ℃.
[0012] As a further technical solution, when the processing mode is turning, the laser beam output by the coaxial laser generator is guided by the integral quartz glass tool to the contact area between the quartz glass tool and the silicon carbide workpiece, so as to perform in-situ stable heating of the processing area.
[0013] As a further technical solution, when the quartz glass processing tool is a quartz glass abrasive, the SiO2 content in the quartz glass abrasive grains is not less than 99%, and the abrasive grain size is 1~20 μm.
[0014] As a further technical solution, when the quartz glass processing tool is a quartz glass cutting tool, the initial surface roughness... S a The diameter is not greater than 5 nm and the diameter is 3~8 mm; the SiO2 content in the quartz glass cutting tool is not less than 99%.
[0015] As a further technical solution, the quartz glass cutter is a monolithic quartz round bar with an initial surface roughness of S a The diameter is not greater than 5 nm and the diameter is 3~8 mm; the SiO2 content in the quartz glass cutting tool is not less than 99%.
[0016] In a second aspect, the present invention provides a system for realizing the dry thermochemical mechanical processing method of silicon carbide crystal driven by quartz glass, including a machine tool body, a workpiece rotation and movement device, a quartz glass grinding wheel unit, a quartz glass cutting tool turning unit, a heating device, and a temperature monitoring and control system. The workpiece rotary moving device is mounted on the machine tool body. The rotary moving device is equipped with a workpiece clamping worktable. The rotary moving device is used to drive the silicon carbide workpiece to rotate around the central axis and move along the X-axis and Y-axis. The quartz glass grinding unit includes a quartz glass grinding wheel, a grinding wheel chuck, a high-speed air hydrostatic spindle, and a spindle indexing rotary table. The quartz glass grinding wheel, grinding wheel chuck, and high-speed air hydrostatic spindle are connected in sequence. The high-speed air hydrostatic spindle is mounted on the spindle indexing rotary table. The spindle indexing rotary table is connected to a standard air hydrostatic guide rail to achieve Z-axis movement. The standard air hydrostatic guide rail is connected to a high-precision linear drive motor to adjust the relative position between the silicon carbide workpiece and the quartz glass grinding wheel. The spindle indexing rotary table is used to adjust the spatial posture of the high-speed air hydrostatic spindle, allowing it to switch between surface grinding mode and end face grinding mode to achieve end face grinding or surface grinding of the surface to be processed. The quartz glass tool turning unit includes a micro-motion tool holder and a quartz glass tool; the turning unit is connected to a standard air hydrostatic guide rail to realize Z-axis movement, the quartz glass tool, the micro-motion tool holder and the standard air hydrostatic guide rail are connected in sequence, and the standard air hydrostatic guide rail is connected to a high-precision linear drive motor to adjust the relative position between the silicon carbide workpiece and the quartz glass tool, so as to realize the rotary turning of the surface to be processed and the quartz glass tool; The precision heating device includes a resistance wire heating device, a side-axis laser generator, and a coaxial laser generator. The resistance wire heating device is located inside the workpiece clamping table to achieve efficient and uniform heating of large-sized silicon carbide workpieces. The side-axis laser generator is fixed on a standard air hydrostatic guide rail by a multi-degree-of-freedom fixture to achieve synchronous linear motion with the quartz glass grinding wheel. It is used to preheat the area to be processed in front of the grinding contact area. The coaxial laser generator is connected to the micro-motion tool holder and acts directly on the processing area through the quartz glass tool to achieve in-situ heating. The temperature monitoring and control system includes a non-contact temperature measuring device and a temperature controller; the temperature measuring device is used to detect the temperature of the processing area and transmit the temperature detection signal to the temperature controller; the temperature controller is connected to the precision heating device and is used to adjust the parameters of the resistance wire heating device and the laser generator according to the deviation between the detected temperature and the set temperature.
[0017] As a further technical solution, the system also includes a gas chip removal device, which includes a gas source and flow control component and a gas nozzle. The gas source and flow control component is connected to the gas nozzle, and the gas nozzle delivers dry, high-speed, and high-pressure compressed air to the processing area to quickly remove chips from the surface of the workpiece.
[0018] The beneficial effects of this invention are as follows: 1. This invention uses quartz glass abrasive wheels or integral quartz glass cutting tools as reactive solid machining media. Without introducing liquid grinding fluid or polishing fluid, it enables the quartz glass machining tool to form a stable solid-solid interface with silicon carbide. Under the synergistic effect of thermal and mechanical energy, the quartz glass machining tool participates in the thermochemical reaction at the machining interface while undertaking mechanical action. This promotes the formation of C–O–Si bridging structures and the reconstruction of the surface bonding state of silicon carbide, weakens the stability of the strong Si–C covalent bonds on the surface, and promotes dislocation slip and plastic removal under interfacial shearing. Therefore, it can reduce the localized high stress caused by direct mechanical cutting with traditional hard abrasives, achieving "soft grinding hard" low-damage machining of high-hardness silicon carbide using quartz glass.
[0019] 2. This invention integrates three machining modes—surface grinding, end face grinding, and turning—on a single high-precision machining system, employing off-axis laser local preheating, resistance wire overall heating, and coaxial laser in-situ heating respectively, tailored to different contact methods. Surface grinding and end face grinding can be switched between different grinding modes by altering the working state of the high-speed air hydrostatic spindle via a spindle indexing rotary table. An integral quartz glass tool is used for turning. This allows for synergistic matching of the heat-assisted method with different machining modes, improving the flexibility, adaptability, and system integration of the machining process.
[0020] 3. This invention employs a high-precision air static pressure turntable, air static pressure guide rails, and a linear drive motor to achieve workpiece rotation, planar movement, and tool positioning and feeding. A non-contact temperature measurement device monitors the temperature of the machining area in real time. A temperature controller adjusts at least one of the following based on temperature feedback: heating device power, laser output power, or pulse repetition frequency, forming a closed-loop control system of real-time temperature monitoring, feedback, and parameter adjustment. This improves the controllability and repeatability of the machining area temperature, cutting depth, and relative motion state, providing conditions for stabilizing the solid-solid interface thermochemical reaction and material removal process.
[0021] 4. Compared to existing chemical mechanical machining methods that rely on liquid grinding fluids, polishing slurries, and free abrasive grains, this invention eliminates the need for liquid cutting fluids, grinding fluids, or polishing fluids as machining media. Furthermore, dry compressed air is used to promptly remove interfacial reaction products, grinding debris, and chips, reducing the retention and repeated entrapment of machining products in the contact area. Therefore, it avoids the need for continuous supply and subsequent processing of liquid machining media during machining, simplifies auxiliary machining processes, reduces the environmental pollution risks associated with the use of liquid media, and minimizes post-machining cleaning issues. Attached Figure Description
[0022] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.
[0023] Figure 1 This is a schematic diagram of the overall structure and three processing modes (turning, face grinding, and surface grinding) of the quartz glass-driven dry thermochemical mechanical processing system for silicon carbide crystals according to the present invention; 1 – high-precision machine tool body, 2 – linear drive motor, 3 – high-precision air static pressure rotary table, 4 – workpiece clamping table, 5 – resistance wire heating device, 6 – vacuum adsorption fixture, 7 – single crystal silicon carbide workpiece, 8 – infrared thermal imager, 9 – temperature controller, 10 – gas nozzle, 11 – high-precision air static pressure guide rail, 12 – micro-motion tool holder, 13 – integral quartz glass tool, 14 – coaxial laser generator, 15 – spindle indexing rotary table, 16 – high-speed air static pressure spindle, 17 – grinding wheel chuck, 18 – quartz glass grinding wheel, 19 – off-axis laser generator.
[0024] Figure 2 This is a flowchart of a quartz glass-driven dry thermochemical mechanical processing method for silicon carbide crystals according to the present invention. Figure 3This diagram illustrates the thermochemical-mechanical removal mechanism of the solid-solid interface between a quartz glass grinding wheel and single-crystal silicon carbide under typical end-face grinding mode of this invention. The left side represents the initial contact state between the quartz glass grinding wheel and the surface of single-crystal silicon carbide, while the right side represents the interfacial chemical reaction between the Si-O structure on the quartz glass surface and the surface layer of single-crystal silicon carbide under the synergistic effect of thermal energy and interfacial mechanical action. This reaction forms a C-O-Si bridging structure, accompanied by the formation, breakage, and reconstruction of related chemical bonds. This weakens the bonding stability of the strong Si-C covalent bonds on the surface layer of single-crystal silicon carbide, and promotes the plastic deformation of the surface material and its removal from the matrix under interfacial shearing action.
[0025] Figure 4 This is a scanning electron microscope image of the surface of a silicon carbide workpiece processed in surface grinding mode.
[0026] Figure 5 This is a laser confocal C-DIC micrograph of the surface of a silicon carbide workpiece under turning mode.
[0027] Figure 6 This is a photograph of the wear on the working end of a solid quartz glass cutting tool after machining in turning mode. Detailed Implementation
[0028] In this invention, the terms used to describe the position, connection relationship and direction of movement of components are all illustrated with the structure shown in the accompanying drawings as an example. Without changing the technical concept of this invention, the installation position, arrangement direction and relative movement of each component can be adjusted accordingly according to actual processing requirements.
[0029] As described in the background section, existing technologies have technical problems. Therefore, it is necessary to develop a dry thermochemical mechanical processing technology that uses quartz glass as a reactive solid processing medium, without the need to introduce liquid cutting fluid, grinding fluid, or polishing fluid. This technology promotes a chemical reaction at the solid-solid interface between quartz glass and silicon carbide through the synergistic effect of controllable thermal and mechanical energy. This allows the quartz glass processing tool to directly participate in the interfacial chemical reaction while performing mechanical functions, thereby weakening the strong covalent bonds of Si–C on the surface of silicon carbide and promoting the removal of surface material.
[0030] like Figure 1 As shown, this embodiment also provides a quartz glass driven silicon carbide crystal dry thermochemical mechanical processing system, including a high-precision machine tool body 1, a workpiece rotation and movement device, a quartz glass grinding unit, a quartz glass tool turning unit, a precision heating device, a temperature monitoring and control system, and a gas chip removal device; the system can switch between three processing modes: turning, end face grinding, and surface grinding according to processing requirements.
[0031] The workpiece rotation and movement device is mounted on the high-precision machine tool body and includes a linear drive motor 2, a high-precision air static pressure rotary table 3, and a workpiece clamping table 4. The linear drive motor 2 is mounted on the high-precision machine tool body 1, the high-precision air static pressure rotary table 3 is mounted on the moving part of the linear drive motor 2, and the workpiece clamping table 4 is mounted on the high-precision air static pressure rotary table 3. The silicon carbide workpiece 7 is fixed to the workpiece clamping table 4 by a vacuum adsorption fixture 6. The linear drive motor 2 drives the high-precision air static pressure rotary table 3, the workpiece clamping table 4, and the silicon carbide workpiece 7 to move along the X-axis or Y-axis. The high-precision air static pressure rotary table 3 drives the workpiece clamping table 4, the vacuum adsorption fixture 6, and the silicon carbide workpiece 7 to rotate around its rotational central axis. That is, the high-precision air static pressure rotary table achieves rotational motion around the central axis, and the linear drive motor drives the high-precision air static pressure rotary table to achieve precise linear motion along the X-axis and Y-axis. The high-precision air static pressure turntable 3 has a rotational speed of 5~2000 rpm, and the linear drive motor provides X-axis and Y-axis linear accuracy of 0.15 μm / 200 mm.
[0032] The quartz glass grinding unit includes a quartz glass grinding wheel, a grinding wheel chuck 17, a high-speed air hydrostatic spindle 16, and a spindle indexing rotary table 15. The quartz glass grinding wheel, grinding wheel chuck, and high-speed air hydrostatic spindle are connected sequentially. The high-speed air hydrostatic spindle 16 is mounted on the spindle indexing rotary table 15. The spindle indexing rotary table 15 is connected to a standard air hydrostatic guide rail 11 to achieve Z-axis movement. The standard air hydrostatic guide rail 11 is connected to a high-precision linear drive motor to adjust the relative position between the quartz glass grinding wheel and the silicon carbide workpiece. The spindle indexing rotary table 15 is used to adjust the spatial attitude of the high-speed air hydrostatic spindle, allowing it to switch between surface grinding mode and end-face grinding mode, thereby achieving surface grinding or end-face grinding of the silicon carbide workpiece. The grinding wheel chuck 17 is mounted on the output end of the high-speed air hydrostatic spindle 16. The quartz glass grinding wheel 18 is used for the quartz glass grinding wheel and is fixed on the grinding wheel chuck 17. After the high-speed air static pressure spindle 16 is started, it drives the quartz glass grinding wheel 18 to rotate at high speed around its own central axis through the grinding wheel chuck 17.
[0033] The quartz glass tool turning unit includes a micro-motion tool holder 12 and an integral quartz glass tool 13. The quartz glass tool 13 is mounted on the micro-motion tool holder 12, which is positioned on a moving part of a standard air-static guide rail 11. The turning unit achieves position-controlled feed along the Z-axis through the standard air-static guide rail and a high-precision linear drive motor to adjust the relative position between the quartz glass tool and the silicon carbide workpiece. In turning mode, the integral quartz glass tool 13 remains stationary. The standard air-static guide rail 11 drives the integral quartz glass tool 13 to perform position-controlled feed along the Z-axis, and the relative turning motion is formed by the rotation and linear motion of the silicon carbide workpiece 7. The standard air-static guide rail 11 is mounted on the high-precision machine tool body 1 and connected to the high-precision linear drive motor. It is used to drive the corresponding machining tool to perform precise position-controlled feed along the Z-axis toward or away from the silicon carbide workpiece 7 to adjust the relative position and machining depth between the machining tool and the silicon carbide workpiece 7.
[0034] Furthermore, the spindle indexing rotary table 15 is used to adjust the spatial posture of the high-speed air-static spindle 16, enabling it to switch between face grinding mode and surface grinding mode. In face grinding mode, the spindle indexing rotary table 15 adjusts the high-speed air-static spindle 16 to face grinding mode, so that the working area of the end face of the quartz glass grinding wheel 18 is opposite to the surface to be processed of the silicon carbide workpiece 7; in surface grinding mode, the spindle indexing rotary table 15 adjusts the high-speed air-static spindle 16 to surface grinding mode, so that the circumferential working area of the quartz glass grinding wheel 18 participates in grinding. The specific indexing direction and indexing angle of the spindle indexing rotary table 15 can be set according to the machine tool coordinate system and the installation method of the machining unit.
[0035] Furthermore, the quartz glass grinding wheel 18 is a metal-bonded quartz glass abrasive grinding wheel, which is configured as a quartz glass end face grinding wheel or a quartz glass surface grinding wheel depending on the processing mode. The metal bond is mainly composed of copper, tin, and metal powders such as nickel and zinc; the SiO2 content in the quartz glass abrasive is not less than 99%, and the abrasive particle size is 1~20μm. The high-speed air hydrostatic spindle 16 rotates at a speed of 10~10000 rpm, and the feed speed of the quartz glass grinding wheel 18 along the Z-axis is 0.1~100 μm / s.
[0036] Furthermore, the integral quartz glass cutter 13 is a quartz glass rod with a diameter of 3-8 mm, and the SiO2 content in the quartz glass is not less than 99%. The initial surface roughness of the working end surface is... S a Not greater than 5 nm; the feed speed of the integral quartz glass tool 13 along the Z-axis is 0.1~200 μm / s.
[0037] Furthermore, the precision heating device includes a resistance wire heating device 5, a coaxial laser generator 14, and a side-axis laser generator 19, which are used to provide corresponding thermal assistance during end face grinding, turning, and surface grinding processes, respectively.
[0038] The resistance wire heating device 5 is located inside the workpiece clamping table 4. The heat generated is transferred to the silicon carbide workpiece 7 via the workpiece clamping table 4 and the vacuum adsorption fixture 6, and is used to heat the silicon carbide workpiece 7 as a whole in the end face grinding mode. The stable heating range of the resistance wire heating device 5 is 25~500 ℃.
[0039] In turning mode, the coaxial laser generator 14 is connected to the micro-motion tool holder 12, and its output laser beam is coupled into the tool along the axial direction of the integral quartz glass tool 13, and transmitted to the working end of the tool through the integral quartz glass tool 13, so that the laser energy acts on the contact area between the integral quartz glass tool 13 and the silicon carbide workpiece 7 or its adjacent area, thereby realizing in-situ heating of the processing area.
[0040] In surface grinding mode, the off-axis laser generator 19 is mounted on a standard air hydrostatic guide rail 11 via a multi-degree-of-freedom fixture and moves synchronously with the grinding unit. The off-axis laser beam irradiates the area to be processed in front of the grinding contact area, locally preheating the silicon carbide surface about to enter the grinding contact area. Specifically, by adjusting the irradiation position and incident direction of the off-axis laser generator 19, the laser beam irradiates the area to be processed in front of the grinding contact area, locally preheating the silicon carbide workpiece 7 about to enter the grinding area of the quartz glass grinding wheel 18. Preferably, the coverage size of the laser spot is not less than the effective grinding width of the quartz glass surface grinding wheel.
[0041] The coaxial laser generator 14 and the off-axis laser generator 19 are preferably near-infrared pulsed fiber lasers with a center wavelength of 1064±5 nm, a rated average output power of 100 W, and a power adjustment range of 10% to 100% of the rated average output power. When the pulse width is 350 ns, the pulse repetition frequency can be adjusted from 1 to 400 kHz, and the spot diameter at the laser output end is 2 to 10 mm.
[0042] The temperature monitoring and control system includes a non-contact temperature measuring device and a temperature controller 9. The non-contact temperature measuring device is used to detect the temperature of the processing area and its adjacent areas, and transmits the temperature detection signal to the temperature controller; the temperature controller is connected to a precision heating device, and adjusts the operating parameters of the corresponding heating device according to the deviation between the detected temperature and the set temperature, so that the temperature of the processing area is maintained within the set range.
[0043] The non-contact temperature measurement device uses an infrared thermal imager 8, which is set towards the processing area or its adjacent measurable area to collect surface temperature field information of the processing area in real time and transmit the temperature detection signal to the temperature controller 9; the temperature measurement range of the infrared thermal imager 8 is 0~600 ℃.
[0044] The temperature controller 9 is connected to the control interface signals of the resistance wire heating device 5, the coaxial laser generator 14, and the off-axis laser generator 19, respectively. Based on the deviation between the detected temperature and the set processing temperature, it adjusts the input power of the resistance wire heating device 5, or adjusts at least one of the output power and pulse repetition frequency of the corresponding laser generator, so that the temperature of the processing area is maintained within the set range, forming a closed-loop control system of real-time temperature monitoring-feedback-parameter adjustment.
[0045] The gas chip removal device 10 includes a gas source and flow control component and a gas nozzle. The gas source and flow control component is connected to the gas nozzle via a gas delivery pipeline. The gas nozzle is positioned facing the processing area or its adjacent area. The gas source and flow control component is used to deliver dry compressed air with a flow rate of 5~20 L / min and a pressure of 0.3~0.8 MPa to the gas nozzle. The gas nozzle is used to promptly blow away interfacial reaction products, grinding debris, and chips generated during the processing, reducing the retention and repeated entrapment of processing products in the solid-solid contact area.
[0046] Furthermore, this embodiment also proposes a quartz glass-driven dry thermochemical mechanical processing method for silicon carbide crystals. A quartz glass processing tool is used to dry process the silicon carbide crystal. The quartz glass tool and silicon carbide form a stable solid-solid interface. While undertaking mechanical action, the quartz glass processing tool participates in the thermochemical reaction at the processing interface. The Si-O structure on the quartz glass surface undergoes an interfacial thermochemical reaction with the silicon carbide surface layer, forming a C-O-Si chemical bridging structure. This induces the dynamic formation, fracture, and reconstruction of the C-O phase key bond structure, weakening the bonding stability of the strong Si-C covalent bonds on the silicon carbide surface layer. Under interfacial shearing, it promotes dislocation slip and plastic removal of the surface material.
[0047] Furthermore, the aforementioned processing methods include surface grinding, end face grinding, or turning.
[0048] When the processing method is surface grinding mode, a side-axis laser generator is used to locally preheat the area to be processed in front of the grinding contact area.
[0049] When the machining method is end face grinding, a resistance wire heating device is used to stably maintain the overall temperature of the silicon carbide workpiece at 25~500℃. The set value within the range.
[0050] When the machining mode is turning, the laser beam output from the coaxial laser generator is guided to the quartz glass tool via the integral quartz glass tool. The contact area with the silicon carbide workpiece is subjected to in-situ stable heating of the processing area.
[0051] This embodiment describes in detail the quartz glass-driven dry thermochemical mechanical processing method for single-crystal silicon carbide based on the aforementioned processing system. The following is a detailed explanation in conjunction with... Figure 2 The process shown illustrates its specific implementation steps.
[0052] S1. Clean and dry the single-crystal silicon carbide workpiece 7 and the corresponding quartz glass processing tools respectively. Fix the single-crystal silicon carbide workpiece 7 to the workpiece clamping table 4 through the vacuum adsorption fixture 6, and install the corresponding quartz glass processing tools according to the processing mode. Install the quartz glass surface grinding wheel in the surface grinding mode, install the quartz glass end face grinding wheel in the end face grinding mode, and install the integral quartz glass tool 13 in the turning mode.
[0053] S2. The single-crystal silicon carbide workpiece 7 is moved along the X-axis or Y-axis by the workpiece rotation and moving device, and the corresponding quartz glass processing tool is moved along the Z-axis by the standard air static pressure guide rail 11. The relative position between the quartz glass processing tool and the single-crystal silicon carbide workpiece 7 is adjusted so that the two maintain a preset gap before processing begins.
[0054] S3. Start the corresponding precision heating device according to the selected processing mode.
[0055] In surface grinding mode, the off-axis laser generator 19 is activated to irradiate the area to be processed in front of the grinding contact area, so that the coverage size of the laser spot is not less than the effective grinding width of the quartz glass surface grinding wheel, and the silicon carbide surface that is about to enter the grinding contact area is locally preheated. In the end face grinding mode, the resistance wire heating device 5 set inside the workpiece clamping table 4 is activated, so that heat is transferred to the single crystal silicon carbide workpiece 7 through the workpiece clamping table 4 and the vacuum adsorption fixture 6 to heat the workpiece as a whole. In turning mode, the coaxial laser generator 14 is activated, and the laser beam is guided through the integral quartz glass tool 13 to the predetermined contact area between the integral quartz glass tool 13 and the single crystal silicon carbide workpiece 7, so as to heat the processing area in situ.
[0056] S4. The infrared thermal imager 8 is used to detect the surface temperature of the processing area and its adjacent areas in real time, and the temperature detection signal is transmitted to the temperature controller 9. The temperature controller 9 adjusts the input power of the resistance wire heating device 5, or adjusts at least one of the output power and pulse repetition frequency of the corresponding laser generator, according to the deviation between the detected temperature and the set processing temperature, until the processing area reaches the set temperature range. Temperature monitoring and feedback adjustment are continuously performed in subsequent processing.
[0057] S5. Once the temperature of the area to be processed reaches the set range, the corresponding processing motion is started according to the selected processing mode.
[0058] In the surface grinding mode, the high-speed air static pressure spindle 16 is adjusted to the surface grinding mode by the spindle indexing rotary table 15, and the high-speed air static pressure spindle 16 is started to drive the quartz glass surface grinding wheel to rotate. The silicon carbide workpiece 7 is fed linearly (moves linearly along the X-axis or Y-axis at a preset speed) while the high-precision air static pressure rotary table 3 remains stationary. In the end face grinding mode, the single crystal silicon carbide workpiece 7 is first moved along the X-axis or Y-axis to the preset processing position by the workpiece rotary moving device. The high-speed air static pressure spindle 16 is adjusted to the end face grinding mode by the spindle indexing rotary table 15. The high-speed air static pressure spindle 16 is started to drive the quartz glass end face grinding wheel to rotate. At the same time, the high-precision air static pressure rotary table 3 is started to drive the silicon carbide workpiece 7 to rotate. In turning mode, the high-precision air static pressure turntable 3 is activated to drive the silicon carbide workpiece 7 to rotate and move along the X-axis according to the preset turning trajectory, while the integral quartz glass tool 13 remains stationary.
[0059] S6. Start the high-precision linear drive motor connected to the standard air static pressure guide rail 11, and drive the corresponding quartz glass processing tool to perform position control feed along the Z-axis toward the single crystal silicon carbide workpiece 7; when the quartz glass processing tool forms contact with the surface of the silicon carbide workpiece 7 and reaches the preset processing depth, stop further Z-axis feed and maintain the Z-axis position, thereby establishing a stable solid-solid contact interface.
[0060] S7. Start the gas chip removal device 10, continuously supplying dry compressed air to the processing area through its gas nozzles, and executing the preset processing trajectory according to the selected processing mode. In surface grinding mode, the silicon carbide workpiece 7 moves along the X-axis or Y-axis according to the preset surface grinding trajectory, while keeping the laser spot of the off-axis laser generator 19 in front of the grinding contact area; in end face grinding mode, the silicon carbide workpiece 7 is kept rotating at the preset speed, while maintaining the set speed and Z-axis processing position of the quartz glass end face grinding wheel; in turning mode, the silicon carbide workpiece 7 is kept rotating and moves linearly according to the preset turning trajectory. The interface reaction products, grinding chips, or shavings generated during the processing are promptly blown away from the processing area by the dry compressed air.
[0061] S8. Without introducing liquid cutting fluid, grinding fluid, or polishing fluid into the machining area, maintain the set machining temperature, the Z-axis position of the quartz glass machining tool, and the corresponding machining motion, so that the quartz glass machining tool and the single-crystal silicon carbide workpiece 7 continuously move relative to each other in a solid-solid contact state. Specifically, gradually reach the preset cutting depth according to the preset Z-axis feed rate; when the quartz glass machining tool and the silicon carbide workpiece form a solid-solid contact and reach the preset cutting depth, stop further Z-axis feed and maintain the Z-axis position.
[0062] Under the combined action of thermal and mechanical energy, the Si–O structure on the surface of quartz glass undergoes an interfacial thermochemical reaction with the surface layer of single-crystal silicon carbide, forming a C–O–Si chemical bridging structure. Accompanied by the formation, breakage, and reconstruction of the C–O phase key bond structure, the bonding stability of the strong Si–C covalent bonds on the surface layer of single-crystal silicon carbide is weakened. Under the action of interfacial shear, dislocation slip and plastic removal of the surface material are promoted, realizing the thermochemical-mechanical synergistic removal of single-crystal silicon carbide material.
[0063] like Figure 3 As shown, taking the end face grinding mode as an example, the quartz glass grinding wheel 18 and the single crystal silicon carbide workpiece 7 form a solid-solid contact interface. Under the action of thermal energy and interfacial mechanical action, the Si-O structure on the surface of the quartz glass participates in the interfacial thermochemical reaction of the single crystal silicon carbide surface layer, forming a C-O-Si bridging structure and causing changes in the bonding state of the surface layer. As the quartz glass grinding wheel 18 and the single crystal silicon carbide workpiece 7 continue to move relative to each other, the interface-related chemical bonds are continuously formed, broken and reconstructed, making the silicon carbide surface material easier to detach from the matrix under mechanical shearing action, realizing thermochemical-mechanical synergistic removal. Figure 3 Used to illustrate typical solid-solid interface reactions and material removal processes, its left and right positions do not constitute a limitation on the actual equipment installation orientation.
[0064] S9. After processing continues until the preset processing time, material removal amount, processing size, or surface quality is achieved, the corresponding quartz glass processing tool is driven to retract along the Z-axis from the single-crystal silicon carbide workpiece 7 via the corresponding standard air static pressure guide rail 11. After the solid-solid contact interface is completely separated, the rotation or linear movement of the silicon carbide workpiece 7 is stopped. Then, the corresponding rotating components are stopped according to the processing mode adopted: in the surface grinding mode, the high-speed air static pressure spindle 16 is stopped; in the end face grinding mode, the high-speed air static pressure spindle 16 and the high-precision air static pressure rotary table 3 are stopped; in the turning mode, the high-precision air static pressure rotary table 3 is stopped, and the corresponding precision heating device is turned off. The gas chip removal device 10 continues to work until the interface reaction products, grinding chips, or cutting chips in the processing area are discharged. Finally, the gas chip removal device 10 is turned off, and the processed single-crystal silicon carbide workpiece 7 is removed.
[0065] Furthermore, in the surface grinding mode, the high-speed air static pressure spindle 16 drives the quartz glass surface grinding wheel to rotate at a speed of 10~10000 rpm. The feed speed of the quartz glass surface grinding wheel along the Z-axis is 0.1~100 μm / s. The high-precision air static pressure turntable 3 remains stationary. The single crystal silicon carbide workpiece 7 moves along the X-axis or Y-axis according to the preset surface grinding trajectory. The off-axis laser generator 19 continuously preheats the area to be processed in front of the grinding contact area.
[0066] Furthermore, in the end face grinding mode, the high-precision air static pressure turntable 3 drives the single crystal silicon carbide workpiece 7 to rotate around the rotation center axis at a speed of 50~500 rpm, the high-speed air static pressure spindle 16 drives the quartz glass end face grinding wheel to rotate at a speed of 10~10000 rpm, the feed speed of the quartz glass end face grinding wheel along the Z axis is 0.1~100 μm / s, and the resistance wire heating device 5 stably maintains the overall temperature of the silicon carbide workpiece 7 within the set value of 25~500 ℃.
[0067] Furthermore, in turning mode, the high-precision air static pressure turntable 3 drives the single-crystal silicon carbide workpiece 7 to rotate around the rotation center axis at a speed of 5~2000 rpm, while the integral quartz glass tool 13 remains stationary and performs position-controlled feeding along the Z-axis at a feed speed of 0.1~200 μm / s; the workpiece rotation moving device drives the silicon carbide workpiece 7 to move linearly according to the preset turning trajectory, and the laser beam output by the coaxial laser generator 14 is guided by the integral quartz glass tool 13 to the contact area between the quartz glass tool 13 and the single-crystal silicon carbide workpiece 7, realizing in-situ stable heating of the processing area.
[0068] In the following two embodiments, both the silicon carbide sample and the quartz glass processing tool were ultrasonically cleaned in anhydrous ethanol for 5 minutes before processing, then removed and dried. The silicon carbide workpiece was fixed on the workpiece clamping table using a vacuum adsorption fixture, and the relative position between the processing tool and the workpiece was adjusted by a workpiece rotation and movement device and a standard air static pressure guide rail. During processing, an infrared thermal imager was used to monitor the temperature of the processing area in real time, and the corresponding heating device was adjusted by a temperature controller. At the same time, dry compressed air was used to promptly blow away interfacial reaction products, grinding debris, or chips. No liquid cutting fluid, grinding fluid, or polishing fluid was introduced during the entire processing. After processing, the silicon carbide sample was ultrasonically cleaned in anhydrous ethanol for 5 minutes and dried. The surface morphology and surface quality were inspected using a laser confocal microscope and a scanning electron microscope. Specific Implementation Example 1 This embodiment uses a single-crystal silicon carbide sample with a planar dimension of 20 mm × 20 mm and a thickness of 1.5 mm, and performs grinding using a metal-bonded quartz glass abrasive wheel. Specifically, a quartz glass end-face grinding wheel with a diameter of 300 mm is used for end-face grinding; a quartz glass surface grinding wheel with a diameter of 250 mm and a width of 10 mm is used for surface grinding. The average particle size of the quartz glass abrasive grains in both types of wheels is approximately 5 μm, the SiO2 content is not less than 99%, and the quartz glass abrasive grains are bonded with a metal binder mainly composed of copper and tin.
[0070] During end-face grinding, the high-speed air-static spindle is adjusted to end-face grinding mode via the spindle indexing rotary table. The resistance wire heating device is activated to heat the single-crystal silicon carbide sample as a whole, and the workpiece temperature is stabilized at 200±2 ℃ through temperature closed-loop control. After the workpiece temperature stabilizes, the high-precision air-static rotary table and the high-speed air-static spindle are activated, driving the single-crystal silicon carbide sample to rotate at 100 r / min and the quartz glass end-face grinding wheel to rotate at 600 r / min, respectively. After the workpiece and grinding wheel speeds stabilize, they are kept running. Subsequently, the quartz glass end-face grinding wheel is driven along the Z-axis to gradually approach the surface of the single-crystal silicon carbide sample via a standard air-static guide rail. Once a stable solid-solid contact is established between the quartz glass abrasive grains on the grinding wheel surface and the sample surface to be processed, a stepwise micro-feed is performed with a nominal feed amount of 0.1 μm per Z-axis increment. After each feed, the corresponding Z-axis position is maintained to ensure that the quartz glass abrasive grains and the single-crystal silicon carbide sample maintain a stable solid-solid contact state. Under the conditions of rotating the single-crystal silicon carbide sample at 100 r / min, rotating the quartz glass end face grinding wheel at 600 r / min, and keeping the processing temperature stable at 200±2 ℃, the end face grinding was continuously performed for 5 min, and the cumulative nominal feed of the Z-axis was 10 μm.
[0071] During surface grinding, the high-speed air-static spindle is adjusted to surface grinding mode via a spindle indexing rotary table, while the high-precision air-static rotary table remains stationary. The off-axis laser generator is activated, and the laser output power is set to 80 W, positioning the laser spot in front of the workpiece feed direction along the grinding contact area. Temperature closed-loop control stabilizes the preheating zone temperature at 200±10℃. The high-speed air-static spindle drives the quartz glass surface grinding wheel to rotate at a linear velocity of 25 m / s, with a single Z-axis feed depth of 0.1 μm. After reaching the preset feed position, the Z-axis position remains unchanged, and the single-crystal silicon carbide sample is linearly fed along the preset grinding direction at a speed of 600 mm / min. This grinding process is repeated according to the processing requirements.
[0072] During the grinding process described above, the quartz glass abrasive grains maintain solid-solid contact with the single-crystal silicon carbide surface. Interfacial thermochemical reactions occur under the combined action of thermal and mechanical energy, and continuous interfacial shearing promotes the removal of surface material. Dry compressed air is continuously used for chip removal during the machining process.
[0073] Depend on Figure 4 As can be seen, the surface of the processed single-crystal silicon carbide is relatively smooth overall, with no obvious brittle spalling or cracks, indicating that the material is removed in a relatively stable manner under the action of quartz glass abrasive particles. The surface roughness of the processed area was measured by laser confocal microscopy. R a The nm value is approximately 5 nm, indicating that this grinding method can achieve a good surface finish. Specific Implementation Example 2 In this embodiment, a single-crystal silicon carbide sample with a planar dimension of 20 mm × 20 mm and a thickness of 1.5 mm is used for single-point turning with an integral quartz glass round bar cutter with a diameter of 6 mm, a length of 14 mm, and a SiO2 content of not less than 99%. The quartz glass cutter is mounted on a micro-motion tool holder, and its axis forms a 45° angle with the surface of the single-crystal silicon carbide sample to be machined. The cutter remains stationary during the turning process.
[0075] Start the coaxial laser generator, set the laser output power to 80 W and the pulse repetition frequency to 1000 Hz, guide the laser beam through the integral quartz glass tool to the contact area between the tool and the single crystal silicon carbide sample, and stabilize the temperature of the processing area at 200 ℃ through temperature closed-loop control.
[0076] The high-precision air-static rotary table is started, rotating the single-crystal silicon carbide sample at 2000 r / min. The integral quartz glass cutter performs position-controlled feeding along the Z-axis at a speed of 10 mm / min, with a single Z-axis feed amount of 1 μm. After completing a single feed and establishing solid-solid contact, the Z-axis position remains unchanged, and the single-crystal silicon carbide sample is fed along the X-axis at a speed of 1 mm / min by the workpiece rotation and movement device, completing one turning stroke. Subsequently, the workpiece returns to the preset starting position, and the quartz glass cutter feeds again along the Z-axis by 1 μm, repeating the above process for a total of 10 Z-axis feeds, with a cumulative nominal feed amount of 10 μm.
[0077] During the processing, the coaxial laser continuously heats the contact area in situ, and dry compressed air is used to promptly blow away the interfacial reaction products and chips. Under the combined action of thermal and mechanical energy, a solid-solid interfacial thermochemical reaction occurs between the quartz glass tool and the single-crystal silicon carbide surface, and the surface material is removed under the interfacial shearing action formed by workpiece rotation and linear feed.
[0078] Figure 5This is a laser confocal C-DIC microstructure image of the surface of a single-crystal silicon carbide workpiece processed in turning mode. Figure 5 As can be seen, the surface of the turning area is relatively smooth overall, the material removal area is continuous, and no obvious defects such as brittle fracture, chipping, or large-scale cracks are observed, indicating that single-crystal silicon carbide mainly exhibits plastic removal characteristics under the action of the integral quartz glass tool. The surface roughness of the machining area was measured by laser confocal microscopy. R a The value is approximately 11 nm, indicating that this turning method can achieve a good surface finish. Figure 6 This image shows the wear morphology of the working end of a solid quartz glass cutting tool after turning. Figure 6 It is evident that the working end of the quartz glass tool only showed slight wear after processing, and the overall morphology remained intact without any obvious cracking or breakage. This indicates that the quartz glass tool has good processing stability under the stated processing conditions, and can maintain a stable solid-solid contact state and achieve continuous plastic removal of single-crystal silicon carbide.
Claims
1. A method for dry thermochemical mechanical processing of silicon carbide crystals driven by quartz glass, characterized in that: A quartz glass processing tool is used to dry process silicon carbide crystals. The quartz glass tool forms a stable solid-solid contact interface with silicon carbide. While bearing mechanical action, the quartz glass processing tool participates in the thermochemical reaction of the processing interface. The Si-O structure on the surface of the quartz glass undergoes an interfacial thermochemical reaction with the surface layer of silicon carbide to form a C-O-Si chemical bridging structure. This induces the dynamic formation, fracture, and reconstruction of the C-O phase key bond structure, weakens the bonding stability of the strong Si-C covalent bonds on the surface layer of silicon carbide, and promotes dislocation slip and plastic removal of the surface material under interfacial shear.
2. The method for dry thermochemical mechanical processing of silicon carbide crystals driven by quartz glass as described in claim 1, characterized in that, This includes surface grinding mode, end face grinding mode, or turning mode.
3. The method for dry thermochemical mechanical processing of silicon carbide crystals driven by quartz glass as described in claim 1, characterized in that, When processing When the method is surface grinding mode, a side-axis laser generator is used to locally preheat the area to be processed in front of the grinding contact area.
4. The method for dry thermochemical mechanical processing of silicon carbide crystals driven by quartz glass as described in claim 1, characterized in that, When processing When the end face grinding mode is used, a resistance wire heating device is used to stably maintain the overall temperature of the silicon carbide workpiece within the set value of 25~500 ℃.
5. The method for dry thermochemical mechanical processing of silicon carbide crystals driven by quartz glass as described in claim 1, characterized in that, When processing When the turning mode is used, the laser beam output by the coaxial laser generator is guided by the integral quartz glass tool to the contact area between the quartz glass tool and the silicon carbide workpiece, so as to perform in-situ stable heating of the processing area.
6. The method for dry thermochemical mechanical processing of silicon carbide crystals driven by quartz glass as described in claim 1, characterized in that, When the quartz glass processing tool is a quartz glass abrasive, the SiO2 content in the quartz glass abrasive grains is not less than 99%, and the abrasive grain size is 1~20 μm.
7. The method for dry thermochemical mechanical processing of silicon carbide crystals driven by quartz glass as described in claim 1, characterized in that, When the quartz glass processing tool is a quartz glass cutter, the initial surface roughness S a The diameter is not greater than 5 nm and the diameter is 3~8 mm; the SiO2 content in the quartz glass cutting tool is not less than 99%.
8. The method for dry thermochemical mechanical processing of silicon carbide crystals driven by quartz glass as described in claim 1, characterized in that, The quartz glass cutter is a monolithic quartz round rod with an initial surface roughness of [missing information]. S a The diameter is not greater than 5 nm and the diameter is 3~8 mm; the SiO2 content in the quartz glass cutting tool is not less than 99%.
9. A system for implementing the dry thermochemical mechanical processing method for silicon carbide crystal driven by quartz glass according to any one of claims 1-8, characterized in that, It includes the machine tool body, workpiece rotation and movement device, quartz glass abrasive grinding unit, quartz glass tool turning unit, heating device and temperature monitoring and control system; The workpiece rotary moving device is mounted on the machine tool body. The rotary moving device is equipped with a workpiece clamping worktable. The rotary moving device is used to drive the silicon carbide workpiece to rotate around the central axis and move along the X-axis and Y-axis. The quartz glass grinding unit includes a quartz glass grinding wheel, a grinding wheel chuck, a high-speed air hydrostatic spindle, and a spindle indexing rotary table. The quartz glass grinding wheel, grinding wheel chuck, and high-speed air hydrostatic spindle are connected in sequence. The high-speed air hydrostatic spindle is mounted on the spindle indexing rotary table. The spindle indexing rotary table is connected to a standard air hydrostatic guide rail to achieve Z-axis movement. The standard air hydrostatic guide rail is connected to a high-precision linear drive motor to adjust the relative position between the silicon carbide workpiece and the quartz glass grinding wheel. The spindle indexing rotary table is used to adjust the spatial posture of the high-speed air hydrostatic spindle, allowing it to switch between surface grinding mode and end face grinding mode to achieve end face grinding or surface grinding of the surface to be processed. The quartz glass tool turning unit includes a micro-motion tool holder and a quartz glass tool; the turning unit is connected to a standard air hydrostatic guide rail to realize Z-axis movement, the quartz glass tool, the micro-motion tool holder and the standard air hydrostatic guide rail are connected in sequence, and the standard air hydrostatic guide rail is connected to a high-precision linear drive motor to adjust the relative position between the silicon carbide workpiece and the quartz glass tool, so as to realize the rotary turning of the surface to be processed and the quartz glass tool; The precision heating device includes a resistance wire heating device, a side-axis laser generator, and a coaxial laser generator. The resistance wire heating device is located inside the workpiece clamping table to achieve efficient and uniform heating of large-sized silicon carbide workpieces. The side-axis laser generator is fixed on a standard air hydrostatic guide rail by a multi-degree-of-freedom fixture to achieve synchronous linear motion with the quartz glass grinding wheel and is used to preheat the area to be processed in front of the grinding contact area. The coaxial laser generator is connected to the micro-motion tool holder and acts directly on the processing area through the quartz glass tool to achieve in-situ heating. The temperature monitoring and control system includes a non-contact temperature measuring device and a temperature controller; the temperature measuring device is used to detect the temperature of the processing area and transmit the temperature detection signal to the temperature controller; the temperature controller is connected to the precision heating device and is used to adjust the parameters of the resistance wire heating device and the laser generator according to the deviation between the detected temperature and the set temperature.
10. The system for realizing the dry thermochemical mechanical processing method of silicon carbide crystal driven by quartz glass as described in claim 9, characterized in that, It also includes a gas chip removal device, which includes a gas source and flow control component and a gas nozzle. The gas source and flow control component is connected to the gas nozzle, and the gas nozzle delivers dry, high-speed, and high-pressure compressed air toward the processing area to quickly remove chips from the surface of the workpiece.
Citation Information
Patent Citations
Chemical mechanical grinding system and method for hard and brittle semiconductor wafers