PTFE membrane stretching and forming method, PTFE membrane, composite separator and secondary battery

By selectively adjusting the thickness of local areas during the lateral stretching process of the PTFE membrane, and combining wind power, traction force, and heating technology, the problems of uneven PTFE membrane thickness and dimensional instability were solved, achieving higher uniformity and stability while reducing energy consumption.

CN123104043APending Publication Date: 2026-11-17SUZHOU QINGTAO NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611454223.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing PTFE membranes suffer from thickness inhomogeneity and dimensional stability issues during transverse stretching, which are difficult to effectively resolve through hot air and steam activation treatments, and also consume a lot of energy.

Method used

By applying auxiliary forces to local areas of the PTFE membrane during the transverse stretching process, including wind, traction, and heating, combined with gradient cooling and rolling technology, the thickness of local areas is adjusted to achieve uniformity and stability.

Benefits of technology

It improves the thickness uniformity and dimensional stability of PTFE membranes, reduces energy consumption, and enhances production controllability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104043A_ABST
    Figure CN123104043A_ABST
Patent Text Reader

Abstract

This invention relates to the field of battery manufacturing technology, and discloses a method for stretching and forming a PTFE film, a PTFE film, a composite separator, and a secondary battery. The method for stretching and forming a PTFE film includes: step S1, longitudinally stretching a PTFE preform film to obtain a primary stretched film; step S2, laterally stretching the primary stretched film to obtain a secondary stretched film; wherein, the lateral stretching includes the following steps: step S21, applying a lateral tension to the entire primary stretched film, causing the primary stretched film to expand laterally; step S2n, applying an auxiliary force to a local area of ​​the primary stretched film to adjust the thickness of the local area of ​​the primary stretched film; wherein, the entire primary stretched film includes multiple local areas; step S3, shaping the secondary stretched film to obtain a PTFE film; wherein, the longitudinal direction is the same as the transport direction of the secondary stretched film, and the lateral direction is perpendicular to the longitudinal direction. The PTFE film prepared by the method for stretching and forming a PTFE film of this invention has high thickness uniformity and good dimensional stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery manufacturing technology, and in particular to a method for stretching and forming a PTFE membrane, a PTFE membrane, a composite separator, and a secondary battery. Background Technology

[0002] PTFE (Polytetrafluoroethylene) is polymerized from tetrafluoroethylene monomers. The carbon-fluorine bonds have high bond energy, and the fluorine atoms have a highly symmetrical and regularly arranged structure, resulting in a resin with high crystallinity. This leads to materials made from PTFE exhibiting outstanding chemical stability, high heat resistance, strong hydrophobicity, and high fracture toughness. PTFE microporous membranes (hereinafter referred to as PTFE membranes) are widely used in battery separators, filter membranes, and other applications.

[0003] Currently, there are several methods for preparing polytetrafluoroethylene (PTFE) microporous membranes, including mechanical biaxial stretching, electrospinning, centrifugal spinning, and casting sintering. Among these, mechanical biaxial stretching is the most widely used and the most mature process. Traditional mechanical biaxial stretching involves steps such as mixing and curing → extrusion → calendering → longitudinal stretching → transverse stretching → heat setting → finished product. During transverse stretching, the PTFE membrane is held at both ends by a chain track, achieving stretching during chain operation. However, transverse stretching often results in a thickness distribution along the width, with the middle being thicker and the ends thinner. Existing technologies introduce hot air blowing and steam activation after longitudinal stretching to improve the uniformity of transverse stretching through temperature homogenization. However, these methods still have significant drawbacks: firstly, the temperature, humidity, flow rate, and uniformity of the hot air and steam are difficult to control precisely, easily leading to localized overstretching, uneven thickness, or micro-wrinkles on the membrane surface; secondly, steam activation may cause unintended molecular chain slippage, affecting membrane dimensional stability (such as increased thermal shrinkage), and the high temperature and humidity environment significantly increases energy consumption and equipment costs. Therefore, the process window for improving stretch uniformity is narrow, the control is difficult, and it is hard to balance uniformity and dimensional stability.

[0004] Therefore, there is an urgent need for a PTFE membrane stretching and forming method, PTFE membrane, composite separator, and secondary battery to solve the above problems. Summary of the Invention

[0005] The first objective of this invention is to provide a stretching and forming method for PTFE membranes, which can improve the uniformity of PTFE membrane thickness and provide good dimensional stability.

[0006] To achieve this objective, the present invention adopts the following technical solution: Methods for stretching and forming PTFE membranes include: Step S1: The PTFE preform membrane is stretched longitudinally to obtain a primary stretched membrane; Step S2, the primary stretched film is laterally stretched to obtain a secondary stretched film; wherein, the laterally stretching includes the following steps: Step S21: Apply a lateral tension to the entire film of the primary stretching film, causing the primary stretching film to expand laterally. Step S2n: Apply an auxiliary action to a local area of ​​the primary stretching film to adjust the thickness of the local area of ​​the primary stretching film; wherein, the entire primary stretching film includes multiple local areas; Step S3: Shape the secondary stretched membrane to obtain the PTFE membrane; The longitudinal direction is the same as the transmission direction of the secondary stretched film, and the transverse direction is perpendicular to the longitudinal direction.

[0007] As an optional solution, the lateral stretching further includes: Step S22: Obtain the thickness of each local region of the primary stretching membrane; Step S23: Determine whether the thickness of each local region is greater than the corresponding preset thickness. If so, proceed to step S24. Step S24: Perform step S2n on the local region whose thickness is greater than the corresponding preset thickness.

[0008] Preferably, the preset thickness is the average thickness of the corresponding local region of the film segment corresponding to the primary stretching film along the conveying direction; Preferably, the preset thickness is the average value of the historical thickness data of the primary stretched film in the corresponding local area under the same stretching process parameters.

[0009] As an optional approach, the method for applying an auxiliary effect to a localized area of ​​the primary stretched membrane in step S2n includes: Apply wind force to the local area; and / or, Apply traction to the local area; and / or, Heating the localized area; Preferably, the direction of action of at least one component of the wind force is consistent with the current lateral stretching direction of the local area; Preferably, the traction force includes the frictional force between the surface of the primary stretched membrane and the traction device; Preferably, the heating temperature during the heating of the local area is higher than the production temperature of the current transverse stretching process, but lower than the melting point of the PTFE material.

[0010] As an optional solution, step S24 includes: Based on the thickness of each local area, adjust one or more of the following parameters corresponding to each local area: wind force, wind direction, heating temperature, and traction force.

[0011] As an optional solution, step S21 further includes the step: While the primary stretching film is being transported along the longitudinal direction, the transverse tensile force is applied to the primary stretching film; The transmission speed of the primary stretched membrane along the longitudinal direction is obtained; Adjust the size and / or number of the local area based on the transmission speed.

[0012] Preferably, the transmission speed is 5m / min to 150m / min.

[0013] As an optional solution, the shaping of the secondary stretching film includes: Step S31: Heat-set the secondary stretched film to obtain a heat-set film; Step S32: The heat-set film is subjected to gradient cooling to obtain a cooling film.

[0014] Preferably, step S32 includes: cooling the heat-setting film under at least two temperature gradients, wherein the highest temperature gradient is lower than the heat-setting temperature of step S31, the lowest temperature gradient is not less than 80°C, and the temperature difference between adjacent temperature gradients is 50°C to 180°C.

[0015] As an optional solution, the shaping of the secondary stretched film further includes the step of: S33, rolling the cooling film to obtain the PTFE film; Preferably, the surface temperature of the cooling film during the rolling process is 40°C to 80°C; Preferably, step S33 is performed at room temperature; Preferably, the cooling film is rolled using at least one set of rollers, the rollers including a first roller and a second roller, at least one of the first roller and the second roller being a flexible roller.

[0016] The second objective of this invention is to provide a PTFE membrane obtained by the above-mentioned PTFE membrane stretching and forming method, which has uniform thickness and good dimensional stability.

[0017] To achieve this objective, the present invention adopts the following technical solution: A PTFE membrane, the PTFE membrane being obtained according to the stretching and forming method of the PTFE membrane.

[0018] The third objective of this invention is to provide a composite membrane that, by using the aforementioned PTFE membrane, exhibits uniform overall thickness and good dimensional stability.

[0019] To achieve this objective, the present invention adopts the following technical solution: A composite membrane includes a base membrane and the PTFE membrane disposed on at least one side of the base membrane.

[0020] The fourth objective of this invention is to provide a secondary battery that, by employing the aforementioned composite separator, achieves high yield and stable performance.

[0021] To achieve this objective, the present invention adopts the following technical solution: A secondary battery includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, wherein the separator is the PTFE membrane described above, or the separator is the composite separator described above.

[0022] The beneficial effects of this invention are: The PTFE membrane stretching and forming method of the present invention includes: step S1, longitudinally stretching a PTFE preform film to obtain a primary stretched film; step S2, laterally stretching the primary stretched film to obtain a secondary stretched film; wherein, the lateral stretching includes the following steps: step S21, applying a lateral tensile force to the entire primary stretched film, causing the primary stretched film to expand laterally; step S2n, applying an auxiliary action to a local area of ​​the primary stretched film to adjust the thickness of the local area of ​​the primary stretched film; wherein, the entire primary stretched film includes multiple local areas; step S3, shaping the secondary stretched film to obtain a PTFE membrane. The PTFE membrane stretching and forming method of the present invention, by applying an auxiliary action to a local area of ​​the primary stretched film during the lateral stretching process, can specifically adjust the thickness of the local area. Furthermore, compared to directly introducing blowing air or water vapor for activation, it offers better overall controllability, resulting in a PTFE membrane with better thickness uniformity and higher dimensional stability. Attached Figure Description

[0023] Figure 1 This is a schematic diagram illustrating the application of wind force to a local area during the lateral stretching process, provided by a specific embodiment of the present invention. Figure 2 yes Figure 1 Sectional view at point AA; Figure 3 This is a schematic diagram illustrating the application of traction force to a local area during lateral stretching, provided by a specific embodiment of the present invention. Figure 4 yes Figure 3 Sectional view at point BB.

[0024] In the picture: 100. One-time stretch film; 200. Chain track; 300. Hair dryer mechanism; 310. Hair dryer unit; 400. Traction device; 410. Conveyor belt unit. Detailed Implementation

[0025] The present invention will now be described in further detail with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be noted that, for ease of description, the accompanying drawings show only the parts relevant to the present invention and not the entire structure.

[0026] In the description of this invention, unless otherwise explicitly specified and limited, the terms "connected," "linked," and "fixed" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0027] In this invention, unless otherwise explicitly specified and limited, "above" or "below" the second feature can include direct contact between the first and second features, or contact between the first and second features through another feature between them. Furthermore, "above," "over," and "on top" of the second feature includes the first feature directly above or diagonally above the second feature, or simply indicates that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature includes the first feature directly below or diagonally below the second feature, or simply indicates that the first feature is at a lower horizontal level than the second feature.

[0028] In the description of this embodiment, the terms "upper," "lower," "right," etc., refer to the orientation or positional relationship shown in the accompanying drawings. They are used only for ease of description and simplification of operation, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the present invention. In addition, the terms "first" and "second" are used only for distinction in description and have no special meaning.

[0029] This embodiment provides a method for stretching and forming a PTFE membrane, the method comprising: Step S1: The PTFE preform film is stretched longitudinally to obtain a single-stretch film 100. Step S2, the primary stretch film 100 is stretched laterally to obtain the secondary stretch film; wherein, the lateral stretching includes the following steps: Step S21: Apply a transverse tensile force to the entire film of the primary stretch film 100, causing the primary stretch film 100 to expand laterally. Step S2n: Apply an auxiliary action to a local area of ​​the primary stretch film 100 to adjust the thickness of the local area of ​​the primary stretch film 100; wherein, the entire film of the primary stretch film 100 includes multiple local areas. Step S3: Shape and stretch the membrane twice to obtain a PTFE membrane; The longitudinal direction is the same as the transport direction of the secondary stretched membrane, and the transverse direction is perpendicular to the longitudinal direction, which is also the width direction of the membrane material.

[0030] The PTFE membrane stretching method of this embodiment can adjust the thickness of local areas by applying an auxiliary effect to a local area of ​​the first-stretch membrane 100 during the transverse stretching process. Moreover, compared with the method of directly introducing blowing air and water vapor to activate the whole, the overall controllability is better, and the obtained PTFE membrane has better thickness uniformity and higher dimensional stability.

[0031] It should be noted that in step S1, a longitudinal stretching mechanism is used to stretch the PTFE preform into a sequentially stretched film. It is understood that, without departing from the inventive concept of this application, the longitudinal stretching mechanism can be any existing type. In step S21, the method of applying a transverse tension to the entire film of the primary stretched film 100, causing the primary stretched film 100 to expand laterally, is existing technology and is accomplished by a transverse stretching mechanism. Some embodiments may refer to… Figure 1 The transverse stretching mechanism includes two sets of chain tracks 200, which are arranged in a figure-eight shape and respectively clamp the two ends of the primary stretching film 100 in the transverse direction. During the operation of the chain tracks 200, the primary stretching film 100 is stretched in the transverse direction.

[0032] In some embodiments, the transverse stretching in step S2 above further includes: Step S22: Obtain the thickness of each local area of ​​the primary stretch membrane 100; Step S23: Determine whether the thickness of each local area is greater than the corresponding preset thickness. If so, proceed to step S24. Step S24: Perform step S2n on local regions where the thickness is greater than the corresponding preset thickness. Optionally, in some embodiments, step S22 is performed simultaneously with step S21. In some embodiments, step S22 is performed after step S21.

[0033] Based on the above steps S22~S24, local areas with large thickness deviations in the primary stretch membrane 100 can be accurately obtained, and local thickness adjustments can be made for these local areas. This not only allows for the acquisition of PTFE membranes with good thickness uniformity, but also helps to improve overall energy efficiency and reduce energy consumption.

[0034] It is understandable that as the transverse stretching continues, the thickness of the single-stretch film 100 gradually decreases, therefore, the preset thickness varies for different local areas.

[0035] In some embodiments, the preset thickness of each local area is the average value of the historical thickness data of the first-stretch film 100 in the corresponding local area under the same stretching process parameters.

[0036] In some embodiments, the preset thickness is the average thickness of the corresponding local area within the film segment of the primary stretched film 100 along the belt-carrying direction. It should be noted that the film segment refers to all film material within a preset distance of the primary stretched film 100 along the belt-carrying direction. See further reference... Figure 1 The local region S1 is located within the corresponding membrane segment S0, and the preset thickness of the local region S1 is the average thickness of the membrane material within the membrane segment S0.

[0037] The thickness of the local region S1 and the average thickness of the membrane segment S0 in the aforementioned stretched membrane 100 are both measured using a thickness gauge. Specifically, when arranging the thickness gauges, the transverse stretching area is divided into multiple sub-regions, which can be arranged in an array or according to a certain pattern. A thickness gauge is installed in each sub-region. A local region can usually cover one or more sub-regions, so the thickness of each local region can be detected and calculated using the thickness gauges in one or more sub-regions corresponding to its location. When calculating the average thickness of the membrane segment where the local region is located, the average of the detection results from multiple thickness gauges in multiple sub-regions corresponding to the location of that membrane segment can be obtained. In this scheme, even when the size and number of local regions change, the thickness detection of each local region can still be satisfied.

[0038] In some embodiments, the method for applying auxiliary action to a local area of ​​the primary stretch film 100 in step S2n includes at least one of three methods: applying wind force to the local area, applying traction force to the local area, and heating the local area. In actual production, only one of the above three methods may be used to apply auxiliary action to the local area of ​​the primary stretch film 100, or two or three of the above three methods may be used simultaneously to apply auxiliary action to the local area of ​​the primary stretch film 100; no specific limitation is made here.

[0039] In some embodiments, when wind is applied to a local area to assist a local area of ​​the primary stretch membrane 100, the direction of action of at least one component of the wind force is consistent with the current lateral stretching direction of the local area, that is, from the middle of the primary stretch membrane 100 in the lateral direction to the lateral end.

[0040] In some embodiments, reference may be made to Figure 1 and Figure 2 A blower mechanism 300 is used to apply an auxiliary force to a localized area of ​​the primary stretch film 100. The blower mechanism 300 blows air onto the surface of the primary stretch film 100, thereby applying a force to the primary stretch film 100 from its transverse middle to its transverse ends. Specifically, the blower mechanism 300 includes multiple blower units 310. When arranging the blower units 310, the transverse stretching area can be divided into multiple sub-regions (the division of these sub-regions can be the same as or different from the sub-regions where the thickness measuring instrument is arranged), and a blower unit 310 is set in each sub-region. When it is necessary to blow air onto a specific localized area, one or more blower units 310 corresponding to that localized area are activated.

[0041] In some embodiments, the blower mechanisms 300 are arranged only on the upper side of the primary stretch membrane 100. In some embodiments, the blower mechanisms 300 are arranged only on the lower side of the primary stretch membrane 100. In some embodiments, blower mechanisms 300 are provided on both the upper and lower sides of the primary stretch membrane 100.

[0042] In some embodiments, when performing step S2n on a local area with a thickness greater than a corresponding preset thickness in step S24, the method includes adjusting the corresponding wind force and direction based on the thickness of each local area. Specifically, adjusting the wind force and direction at the location of the blowing unit 310 corresponding to the local area can adjust the wind force and direction received by that local area. For example, when the thickness of the local area deviates significantly from the preset thickness, the wind force can be increased accordingly; when the thickness of the local area deviates slightly from the preset thickness, the wind force can be decreased accordingly. For example, when the thickness of the local area deviates significantly from the preset thickness, the angle between the wind blown by the corresponding blowing unit 310 and the surface of the primary stretch film 100 can be appropriately decreased; when the thickness of the local area deviates slightly from the preset thickness, the angle between the wind blown by the corresponding blowing unit 310 and the surface of the primary stretch film 100 can be appropriately increased.

[0043] In some embodiments, when an auxiliary action is applied to a local area of ​​the primary stretch membrane 100 by applying a traction force to a local area: the traction force applied to the local area includes the frictional force between the membrane surface of the primary stretch membrane 100 and the traction device 400. See also... Figure 3 and Figure 4The traction device 400 includes multiple conveyor belt units 410, each extending laterally along the primary stretching film 100. The conveying surface of the conveyor belt unit 410 presses against the lower surface of the primary stretching film 100, and the movement direction of the conveying surface is along the lateral direction of the primary stretching film 100, extending from the middle to the end of the lateral direction. With this configuration, when the conveyor belt unit 410 is running, the conveying surface of the conveyor belt unit 410 applies a frictional force along the lateral direction from the middle to the end of the corresponding local area, thereby adjusting the thickness of that local area. Furthermore, this frictional force is continuous, uniformly distributed, and stable, thereby improving the thickness uniformity of the stretched PTFE film. Specifically, when arranging the traction device 400, the transverse stretching area is divided into multiple sub-areas (the division of these sub-areas can be the same as or different from the sub-areas where the thickness measuring instrument is arranged). Each sub-area is equipped with a conveyor belt unit 410. When the thickness of a certain local area needs to be adjusted, one or more conveyor belt units 410 corresponding to the position of that local area can be turned on to adjust the thickness of that local area.

[0044] In some embodiments, when performing step S2n on local areas with a thickness greater than a corresponding preset thickness in step S24, the magnitude of the corresponding traction force is adjusted according to the thickness of each local area. It is understood that the traction force for that local area can be adjusted by adjusting the pressure between the conveyor belt unit 410 corresponding to the position of that local area and the primary stretch film 100. For example, when the difference between the thickness of the local area and the corresponding preset thickness is large, the corresponding conveyor belt unit 410 can be driven to move slightly upward to increase the pressure between the conveying surface of the conveyor belt unit 410 and the film surface of the primary stretch film, thereby increasing the traction force. When the difference between the thickness of the local area and the corresponding preset thickness is small, the corresponding conveyor belt unit 410 can be driven to move slightly downward to appropriately reduce the pressure between the conveying surface of the conveyor belt unit 410 and the film surface of the primary stretch film, thereby reducing the traction force.

[0045] In some embodiments, when an auxiliary effect is applied to a local area of ​​the primary stretched film 100 by heating a local area: the heating temperature is higher than the production temperature of the current transverse stretching process, but lower than the melting point of the PTFE film. The production temperature is the temperature required for the PTFE material to enter a highly elastic state and achieve transverse and longitudinal stretching, typically 260~320°C, which is common knowledge in the art. In practice, the actual production temperature during the transverse stretching process can be determined according to specific process requirements.

[0046] In some embodiments, when performing step S2n on local regions with a thickness greater than a corresponding preset thickness in step S24, the heating temperature is adjusted according to the thickness of each local region. For example, when the difference between the thickness of a local region and the corresponding preset thickness is large, the heating temperature of that local region can be appropriately increased. When the difference between the thickness of a local region and the corresponding preset thickness is small, the heating temperature of that local region can be appropriately decreased.

[0047] In some embodiments, step S21 further includes the step of: While the primary stretching membrane 100 is being transported longitudinally, a transverse tensile force is applied to the primary stretching membrane 100. Obtain the longitudinal transmission speed of the stretch membrane 100; Adjust the size and / or number of local areas based on transmission speed.

[0048] Understandably, the higher the conveyor speed, the worse the thickness uniformity of the membrane surface, and therefore the required thickness adjustment force also varies. When the local area is divided more finely (e.g., smaller area, more number), the adjustment accuracy of the membrane thickness is higher; conversely, when the local area is divided more coarsely (e.g., larger area, fewer number), the adjustment accuracy of the membrane thickness is lower. This embodiment, by adaptively adjusting the size and / or number of local areas based on the transmission speed of the primary stretching membrane, can reduce energy consumption and computing power while ensuring the uniformity of the final PTFE membrane thickness. Specifically, when the detected transmission speed is within a first range (a relatively high speed range), the size of each local area can be divided into smaller parts, or the number of local areas can be increased, thereby improving the accuracy of the thickness adjustment of the primary stretching membrane 100 to ensure the uniformity of the final PTFE membrane thickness. Conversely, when the detected transmission speed is within a second range (a relatively low speed range), the size of the local areas can be divided into larger parts, or the number of local areas can be reduced, etc., to appropriately reduce the accuracy of the thickness adjustment of the primary stretching membrane 100.

[0049] In some embodiments, the longitudinal conveying speed of the stretched membrane 100 is 5 m / min to 150 m / min. The PTFE membrane stretching method of this embodiment is more advantageous for preparation methods with high conveying speeds.

[0050] In some embodiments, step S3, shaping the secondary stretching film, includes: Step S31: Heat-set the film and stretch it twice to obtain a heat-set film; Step S32: The heat-set film is subjected to gradient cooling to obtain a cooling film.

[0051] Preferably, step S32 includes: cooling the heat-setting film under at least two temperature gradients, wherein the highest temperature gradient is lower than the heat-setting temperature of step S31, the lowest temperature gradient is not less than 80°C, and the temperature difference between adjacent temperature gradients is 50°C to 180°C.

[0052] In some embodiments, the shaped secondary stretching film further includes step S33, rolling and cooling the film to obtain a PTFE film. The rolling and cooling step can further improve the thickness uniformity of the finally obtained PTFE film.

[0053] Preferably, the surface temperature of the cooling film during the rolling process is 40℃~80℃.

[0054] Preferably, step S33 is performed at room temperature.

[0055] Preferably, at least one set of rollers is used to roll the cooling film. The rollers include a first roller and a second roller, and at least one of the first roller and the second roller is a flexible roller. Setting one of the first roller and the second roller as a flexible roller has two advantages: firstly, the flexible roller can undergo adaptive deformation during the rolling process, ensuring that the cooling film can be effectively pressed at all positions along its width, thereby improving the thickness uniformity of the rolled PTFE film; secondly, the flexible roller can also prevent damage to the cooling film during the rolling process. It is understood that the number of roller sets can be flexibly set according to requirements and is not specifically limited here.

[0056] After the gradient cooling in step S32 is completed, the cooling film enters the room temperature environment, but the film surface is still maintained at 40℃~80℃. At this time, without heating and consuming additional energy, the film surface can be rolled to improve the thickness uniformity of the PTFE film, and at the same time, the PTFE film with uniform thickness is shaped.

[0057] This embodiment also provides a PTFE membrane, which is obtained according to the above-described PTFE membrane stretching and forming method. The PTFE membrane of this embodiment has uniform thickness and good dimensional stability.

[0058] This embodiment also provides a composite separator, which includes a base membrane and a PTFE membrane disposed on at least one side of the base membrane. It exhibits uniform overall thickness and good dimensional stability. Optionally, the base membrane can be formed by combining one or more of the following: PE base membrane, PP base membrane, PI base membrane, PET base membrane, aramid base membrane, PVDF base membrane, cellulose base membrane, and glass fiber base membrane. This composite separator, by employing the aforementioned PTFE membrane, exhibits uniform thickness and good dimensional stability.

[0059] This embodiment also provides a secondary battery, which includes a positive electrode, a negative electrode, and a separator disposed between the positive and negative electrode. The separator is the PTFE membrane or the composite separator described above. By using the composite separator / PTFE membrane described above, the secondary battery achieves high manufacturing yield and stable performance.

[0060] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. For those skilled in the art, based on the concept of the present invention, there will be changes in specific implementation methods and application scope. The content of this specification should not be construed as a limitation of the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the claims of the present invention.

Claims

1. A method for stretching and forming a PTFE membrane, characterized in that, include: Step S1: The PTFE preform membrane is stretched longitudinally to obtain a primary stretched membrane; Step S2, the primary stretched film is laterally stretched to obtain a secondary stretched film; wherein, the laterally stretching includes the following steps: Step S21: Apply a lateral tension to the entire film of the primary stretching film, causing the primary stretching film to expand laterally. Step S2n: Apply an auxiliary action to a local area of ​​the primary stretching film to adjust the thickness of the local area of ​​the primary stretching film; wherein, the entire primary stretching film includes multiple local areas; Step S3: Shape the secondary stretched membrane to obtain a PTFE membrane; The longitudinal direction is the same as the transmission direction of the secondary stretched film, and the transverse direction is perpendicular to the longitudinal direction.

2. The stretching and forming method of PTFE membrane as described in claim 1, characterized in that, The lateral stretching also includes: Step S22: Obtain the thickness of each local region of the primary stretching membrane; Step S23: Determine whether the thickness of each local region is greater than the corresponding preset thickness. If so, proceed to step S24. Step S24: Perform step S2n on the local region whose thickness is greater than the corresponding preset thickness; Preferably, the preset thickness is the average thickness of the corresponding local region of the film segment corresponding to the primary stretching film along the conveying direction; Preferably, the preset thickness is the average value of the historical thickness data of the primary stretched film in the corresponding local area under the same stretching process parameters.

3. The stretching and forming method for a PTFE membrane as described in claim 1 or 2, characterized in that, The method for applying an auxiliary effect to a local area of ​​the primary stretched membrane in step S2n includes: Apply wind force to the local area; and / or, Apply traction to the local area; and / or, Heating the localized area; Preferably, the direction of action of at least one component of the wind force is consistent with the current lateral stretching direction of the local area; Preferably, the traction force includes the frictional force between the surface of the primary stretched membrane and the traction device; Preferably, the heating temperature of the localized area is higher than the production temperature of the current transverse stretching process, but lower than the melting point of the PTFE material.

4. The stretching and forming method of the PTFE membrane as described in claim 3, characterized in that, Step S24 includes: Based on the thickness of each local area, adjust one or more of the following parameters corresponding to each local area: wind force, wind direction, heating temperature, and traction force.

5. The stretching and forming method of PTFE membrane as described in claim 1, characterized in that, Step S21 further includes the following step: While the primary stretching film is being transported along the longitudinal direction, the transverse tensile force is applied to the primary stretching film; The transmission speed of the primary stretched membrane along the longitudinal direction is obtained; Adjust the size and / or number of the local regions based on the transmission speed; Preferably, the transmission speed is 5m / min to 150m / min.

6. The stretching and forming method of the PTFE membrane as described in claim 1, characterized in that, The shaped secondary stretching film includes: Step S31: Heat-set the secondary stretched film to obtain a heat-set film; Step S32: The heat-set film is subjected to gradient cooling to obtain a cooling film; Preferably, step S32 includes: cooling the heat-setting film under at least two temperature gradients, wherein the highest temperature gradient is lower than the heat-setting temperature of step S31, the lowest temperature gradient is not less than 80°C, and the temperature difference between adjacent temperature gradients is 50°C to 180°C.

7. The stretching and forming method of the PTFE membrane as described in claim 6, characterized in that, The shaping of the secondary stretching film further includes the step: S33, rolling the cooling film to obtain the PTFE film; Preferably, the surface temperature of the cooling film during the rolling process is 40°C to 80°C; Preferably, step S33 is performed at room temperature; Preferably, the cooling film is rolled using at least one set of rollers, the rollers including a first roller and a second roller, at least one of the first roller and the second roller being a flexible roller.

8. A PTFE membrane, characterized in that, The PTFE membrane is obtained according to the stretching and forming method of the PTFE membrane as described in any one of claims 1 to 7.

9. A composite diaphragm, characterized in that, It includes a base film and a PTFE membrane as described in claim 8 disposed on at least one side of the base film.

10. A secondary battery, characterized in that, It includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, wherein the separator is a PTFE membrane as described in claim 8, or a composite separator as described in claim 9.