Thermoplastic composite welded magnetic thin film sensing element, preparation method and application
By using a thermoplastic resin composite film sensing element filled with magnetic particles, the problems of increased component weight and current leakage caused by metal mesh and continuous carbon fiber fabric sensing elements were solved, achieving efficient and stable welding of thermoplastic composite materials and improving interfacial bonding strength and temperature field uniformity.
Patent Information
- Application Number
- CN202611583309.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-13
- Publication Date
- 2026-11-17
AI Technical Summary
Existing metal mesh or continuous carbon fiber fabric sensing elements cause problems such as increased component weight, current leakage, and interface incompatibility when welding thermoplastic composite materials.
The thermoplastic resin composite film sensing element filled with magnetic particles includes a functional heating core layer and a resin skin layer. The magnetic particles generate hysteresis loss under an alternating magnetic field, realizing the melting and cooling solidification of the thermoplastic resin matrix, avoiding continuous conductive networks and carbon fiber conductive networks, and forming a stable joint.
It reduces component weight gain and current leakage risk, improves interfacial resin continuity and welding stability, temperature field uniformity and process controllability, and reduces the adverse effects of heterogeneous phases.
Smart Images

Figure CN123104081A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of resin-based composite material bonding technology, specifically relating to thermoplastic composite material welding magnetic thin film sensing elements, their preparation methods, and applications. Background Technology
[0002] Thermoplastic composites, leveraging the repeated melt-and-cured properties of thermoplastic resins, offer advantages such as lightweight yet high strength, excellent impact resistance, short processing cycles, and recyclability. They are often used in welding to replace some mechanical connections and adhesive bonding. Compared to mechanical connections, welding avoids stress concentration caused by drilling and reduces structural weight increase and potential damage from bolts and rivets. Compared to adhesive bonding, welding does not rely on a long curing process, resulting in higher connection efficiency and better joint stability. Induction welding uses an alternating magnetic field to generate heat in an induction element placed at the welding interface, melting the interface resin and then cooling and curing it under pressure to achieve component connection. It offers advantages such as non-contact heating, rapid temperature rise, controllable heat input, and ease of automation, making it a promising candidate for applications in aerospace, rail transportation, automotive, and high-end equipment manufacturing.
[0003] Induction elements are crucial in induction welding, as their heat generation capacity, temperature field distribution, and interfacial compatibility directly determine the fusion quality of the weld interface and the mechanical properties of the joint. Currently, commonly used induction elements include two types: metal mesh and carbon fiber fabric. Metal mesh, as a heterogeneous phase implanted into the weld, can easily lead to increased component weight, localized stress concentration, and discontinuous interfacial bonding. Carbon fiber fabric induction elements, due to their continuous conductive network, pose a risk of current leakage, and their temperature field uniformity and interfacial fusion with the resin matrix are also limited. Summary of the Invention
[0004] To address the aforementioned shortcomings of existing technologies, this invention provides a thermoplastic composite welded magnetic thin film sensing element, its preparation method, and its application, aiming to solve the problems of increased component weight, current leakage, and interface incompatibility caused by existing metal mesh or continuous carbon fiber fabric sensing elements.
[0005] To achieve the aforementioned main objectives, this invention provides a thin-film induction element for induction welding of thermoplastic composite materials. The thin-film induction element is a thermoplastic resin composite film filled with magnetic particles, comprising a functional heating core layer and a resin skin layer covering at least one surface of the functional heating core layer along its thickness direction. The functional heating core layer comprises a thermoplastic resin matrix and magnetic particles dispersed within the thermoplastic resin matrix. The magnetic particles can generate hysteresis loss and heat the functional heating core layer under the action of an alternating magnetic field. The content of magnetic particles in the resin skin layer is lower than that in the functional heating core layer, and the resin skin layer is integrally bonded to the functional heating core layer. The thin-film induction element as a whole does not contain a continuous metal conductive network or a continuous carbon fiber conductive network. The thin-film induction element is used to be sandwiched between the overlapping interfaces of the thermoplastic composite components to be welded. Under the combined action of an alternating magnetic field and applied pressure, the thermoplastic resin matrix in the thin-film induction element and the resin matrix of the thermoplastic composite components to be welded melt, flow, diffuse, and cool and solidify together, achieving the connection between the thermoplastic composite components to be welded.
[0006] The principle behind the above technical solution is as follows: Magnetic particles are concentrated in the functional heating core layer, so that hysteresis loss under alternating magnetic field mainly occurs inside the core layer, and heat is transferred from the core layer to both sides; the resin skin layer has low or no magnetic particle content, so during welding, it first melts, wets, and diffuses molecular chains with the interface resin of the base material, forming a continuous transition zone dominated by resin. Since the film as a whole does not contain a continuous metal conductive network or a continuous carbon fiber conductive network, it avoids current leakage and significant weight increase caused by macroscopic conductive networks. The functional heating core layer and the resin skin layer are integrally combined, so that the film does not rely on additional adhesives during welding, reducing the introduction of heterogeneous phases. Its beneficial effects are: the heat generation area and the connection area are separated in the thickness direction, reducing the exposure, detachment, and stress concentration of magnetic particles at the welding interface and free surface; the continuity of the interface resin is improved, which is conducive to the formation of a stable joint; the film does not contain a continuous conductive network, reducing the risk of leakage and the weight increase of the component.
[0007] Furthermore, a resin skin layer is disposed on both sides of the functional heating core layer, forming a symmetrical three-layer structure. The thickness of each resin skin layer is 1% to 20% of the total thickness of the thin-film sensing element, and the mass fraction of magnetic particles in the resin skin layer is not higher than 10 wt%, preferably free of magnetic particles.
[0008] The principle behind the above technical solution is as follows: symmetrical skin layers on both sides ensure symmetrical thermal stress on the film during hot pressing and welding, reducing warpage. If the skin layer is too thin, it is difficult to form a continuous, clean resin transition zone at the welding interface; if the thickness is too large, it reduces the efficiency of heat transfer from the core layer to the base material and decreases the heat generation capacity per unit volume. Controlling the magnetic particle content in the skin layer to no more than 10 wt% maintains compatibility between the skin layer and the core layer while preventing a large number of magnetic particles from being exposed at the welding interface. The beneficial effects are improved temperature field uniformity, suppression of film warpage, and enhanced resin continuity at the interface.
[0009] Furthermore, the magnetic particles are Fe3O4 particles, with a mass fraction of 30wt%–80wt%, preferably 50wt%–70wt%, in the functional heating core layer. Fe3O4 has high saturation magnetization and hysteresis loss, making it suitable as a heating filler under alternating magnetic fields. If the mass fraction is too low, the number of heating points per unit volume is insufficient, resulting in a low heating rate and difficulty in reaching the welding temperature within a reasonable time. If the mass fraction is too high, the continuous phase ratio of thermoplastic resin decreases, leading to poor powder formability and film mechanical integrity. Additionally, the close proximity of particles increases the risk of localized conductive paths, even with a coating layer. Controlling the content within the above range achieves a balance between heat generation capacity, dispersibility, and film structural stability. The beneficial effect is improved heating efficiency while maintaining film forming quality.
[0010] Furthermore, the average particle size of the Fe3O4 particles is 50 nm to 5 μm, preferably 100 nm to 1 μm, and the average particle size is less than one-tenth of its skin depth at the alternating magnetic field operating frequency. The technical principle is as follows: the skin depth is related to the material's resistivity, permeability, and angular frequency. When the particle size is much smaller than the skin depth, the magnetic field distribution inside the particle is uniform, the particle as a whole participates in magnetization, and heat generation is mainly due to hysteresis loss, avoiding surface-concentrated heating caused by the skin effect. If the particle size is too small, it is prone to agglomeration; if the particle size is too large, the internal magnetization is uneven, and the number of heating points per unit volume decreases. This limitation clarifies the heat generation mechanism of the functional heating core layer and makes the temperature field more uniform. The beneficial effects are improved heat generation uniformity and process repeatability.
[0011] Furthermore, the magnetic particles undergo surface treatment to form a dense, electrically insulating, and oxidation-resistant coating layer. This coating layer is selected from at least one of the following: a silica coating layer, an alumina coating layer, a silane coupling agent crosslinking layer, a titanate coupling agent crosslinking layer, or an organic polymer coating layer. The magnetic particles are dispersed in a thermoplastic resin matrix as core-shell particles, with adjacent core-shell particles electrically isolated from each other by the coating layer or the thermoplastic resin matrix. The technical principle is as follows: the insulating coating layer, at high filler content, blocks the electronic conduction path between particles, preventing the formation of a continuous conductive path even when particles make geometric contact, thereby suppressing eddy currents and leakage currents. The oxidation-resistant coating layer blocks oxygen diffusion, inhibiting the transformation of Fe3O4 to γ-Fe2O3 or α-Fe2O3 under hot pressing and high welding temperatures, maintaining saturation magnetization and heat generation capacity. The beneficial effect is that heat generation is primarily due to hysteresis loss, improving the consistency of heat generation across multiple welding cycles and batches.
[0012] Furthermore, the thermoplastic resin matrix is the same as or compatible with the matrix resin of the thermoplastic composite component to be welded. The thermoplastic resin can be selected from one or more of polyolefin resins, polyester resins, polyamide resins, polycarbonate resins, polyimide resins, polyphenylene sulfide resins, polyetheretherketone resins, polyetherketoneketone resins, and polyetherimide resins; polyamide resins are preferred, and PA6 resin is even more preferred. The technical principle is that when the matrix resins are the same or compatible, sufficient molecular chain diffusion and entanglement can occur at the interface between the film skin layer and the base material in the molten state, forming a continuous interface after cooling, reducing interface defects caused by resin incompatibility. PA6 has good compatibility with the PA6 matrix in glass fiber reinforced PA6 composites, and its melting temperature is moderate, making it suitable for induction welding. The beneficial effects are improved interfacial bonding strength and joint stability.
[0013] Furthermore, the thin-film sensing element is divided into a magnetic heating zone and a magnetically depleted edge zone within the plane. The magnetic heating zone corresponds to the lap welding area of the component to be welded, while the magnetically depleted edge zone surrounds the magnetic heating zone, with a lower content of magnetic particles compared to the magnetic heating zone. The technical principle is to confine the magnetic particles primarily within the plane corresponding to the lap welding area, ensuring that the effective heat generation area under the alternating magnetic field is geometrically matched with the weld. The low heat generation in the magnetically depleted edge zone suppresses continuous heat generation in the magnetic field on the suspended film and edges outside the lap area, reducing edge overheating, resin degradation, and uncontrolled adhesive overflow. The beneficial effects include improved spatial uniformity of the temperature field and reduced ineffective heating and edge thermal damage.
[0014] The present invention also provides a method for preparing a thin-film sensing element, comprising step one, raw material pretreatment and drying: providing thermoplastic resin powder and magnetic particles, and drying the thermoplastic resin powder and magnetic particles respectively; Step 2, Mixing and Dispersion: The thermoplastic resin powder and magnetic particles are mixed according to the functional heating core layer formula and the resin skin layer formula, respectively, and dispersed by mechanical stirring, ball milling, ultrasonic dispersion or a combination thereof to obtain the mixed powder for the functional heating core layer and the powder for the resin skin layer. Step 3, Layered Powdering and Molding: The mixed powder of the resin skin layer and the functional heating core layer is laid layer by layer in the mold according to a preset sequence, so that the laid powder forms a stacked powder blank containing the resin skin layer blank and the functional heating core layer blank. Step 4: Hot pressing: The stacked powder blank after being molded is placed in a hot pressing equipment and heated to a temperature higher than the melting point or softening point of the thermoplastic resin. It is kept at a temperature under pressure so that the resin of each layer melts and flows, the interlayer interface fuses and coats the magnetic particles, and the composite film with interlayer integral bonding is formed in one hot pressing. Step 5: Cooling and Shaping: After hot pressing, the material is cooled to room temperature or the target temperature under pressure, and then demolded to obtain the thin-film sensing element. The technical principle is as follows: First, mixed powders for the functional heating core layer and powders for the resin skin layer are prepared separately. Then, they are laid layer by layer in a mold according to a preset sequence to form a stacked powder preform. Subsequently, a single hot pressing causes the resin layers to melt and flow, the interlayer interfaces to fuse, and magnetic particles to be coated. After cooling, a composite thin film with integrated interlayer bonding is obtained. The combination of layered powder laying and single hot pressing allows for a continuous transition between the functional heating core layer and the resin skin layer at the interface, eliminating the need for adhesives and avoiding the introduction of new heterogeneous phases. The beneficial effects are a simple process route, reliable interlayer bonding, and a complete thin film structure.
[0015] Furthermore, before hot pressing, pre-dispersion can be performed using one or more of the following methods: dry powder mixing, solvent-assisted dispersion, ball milling dispersion, ultrasonic dispersion, or melt blending. This ensures that the magnetic particles are uniformly attached to or distributed on the surface of the thermoplastic resin powder and in its gaps. Subsequently, the powder is dried, sieved, or granulated, and then layered and hot-pressed. Hot pressing or cooling can be performed in an inert atmosphere or vacuum environment, with the inert atmosphere being nitrogen or argon. The hot pressing temperature is 10°C to 50°C above the melting or softening point of the thermoplastic resin, the hot pressing pressure is 0.5MPa to 15MPa, and the holding time is 1 min to 30 min. The functional heating core layer and the resin skin layer are laid out and formed into a single unit in a single hot pressing. The technical principle is: pre-dispersion improves the uniformity of magnetic particle dispersion and reduces agglomeration; an inert atmosphere or vacuum inhibits Fe3O4 oxidation; and appropriate temperature, pressure, and time ensure sufficient resin melt flow, interlayer fusion, and particle coating, while preventing resin degradation. The beneficial effects are improved film density, dispersion uniformity, and heat generation consistency.
[0016] This invention also provides an application of a thin-film sensing element. The thin-film sensing element is sandwiched between two or more thermoplastic composite material components to be welded, with the extension direction of the functional heating core layer corresponding to the overlapping welding area. Under an alternating magnetic field, induced heat is generated through hysteresis loss, melting the thermoplastic resin at the core layer and the overlapping interface. The connection is completed under applied pressure through heat preservation and pressure-holding cooling. The components to be welded are fiber-reinforced thermoplastic composite materials, preferably glass fiber reinforced PA6 composite materials. The operating frequency of the alternating magnetic field is 50kHz to 500kHz; the target interface temperature is 10°C to 60°C above the melting or softening point of the base resin; the overlapping pressure is 0.05MPa to 2MPa; the welding sequence is to first apply pressure and apply an alternating magnetic field to raise the temperature and hold it, then stop the magnetic field and hold the pressure to cool until the resin is completely cured before releasing the pressure. The magnetic particles can be selected from ferrite materials with a Curie temperature within the range of 10°C to 60°C above the melting or softening point of the base resin, such as manganese-zinc ferrite, nickel-zinc ferrite, or doped and modified Fe3O4. The technical principle is as follows: when the frequency, particle size, and magnetic particle content are matched, hysteresis loss dominates, and the interface temperature rise is controllable; the hysteresis loss of Curie-limited ferrite drops sharply when the temperature approaches the Curie point, achieving temperature self-limitation. The beneficial effects are improved welding process robustness, prevention of overheating degradation, and suitability for joining thermoplastic composites such as GF / PA6.
[0017] Compared with the prior art, the beneficial results of the present invention are as follows: I. The layered structure separates and coordinates heat generation and bonding functions. The functional heating core layer confines hysteresis heat generation to the vicinity of the center plane of the overlap interface. Clean melting and interdiffusion of non-magnetic or low-magnetic particles occurs between the resin skin layers on both sides and the base material interface, improving the continuity of the interfacial resin and reducing the exposure, detachment, and stress concentration of particles on the weld surface and in the adhesive overflow strip. The symmetrical skin layer facilitates the even conduction of heat from the core layer to the base materials on both sides, improving the uniformity of the temperature field and suppressing film warping.
[0018] II. Synergistic effect of insulating and anti-oxidation coating layer and inert atmosphere process. While maintaining a high Fe3O4 filling content, it provides electrical insulation between particles, suppresses conductive paths and leakage current, and makes heat generation mainly due to hysteresis loss and uniform heating; at the same time, it suppresses the oxidation phase transformation of Fe3O4 under hot pressing and high welding temperatures, and improves the consistency of heat generation and the repeatability of temperature rise curves between multiple welding cycles and batches.
[0019] Third, the patterning of the planar magnetic heating zone and the depleted magnetic edge zone locks the effective heat generation area in the weld lap joint area, reduces the overheating and heat damage width of the outer edge of the lap joint area, controls glue overflow and improves the spatial uniformity of the temperature field, while reducing the ineffective heating of the surrounding area by the magnetic field.
[0020] Fourth, the selection criteria of matching magnetic particle content, particle size and working frequency make the heat generation mechanism clear. Combined with welding temperature, pressure and time window, the heating rate, peak temperature and effective heat generation area can be controlled and adjusted. This avoids insufficient interface fusion caused by insufficient heat generation and resin degradation, pores or resin depletion caused by local overheating, thus improving process portability and joint performance stability.
[0021] Fifth, pure resin continuous phase film without continuous metal mesh and continuous carbon fiber conductive network, and without fiber reinforced skeleton, is beneficial to reduce component weight increase and leakage risk; after the film melts, it participates in the interface blending, leaving no heterogeneous mesh or fiber skeleton, which is beneficial to reduce the adverse effects of heterogeneous structures on the welding interface.
[0022] VI. When Curie temperature-limiting ferrite is used as an alternative mechanism, it can self-limit the interface temperature within the processing window under conditions without temperature control feedback, providing overheat protection and improving process robustness. Attached Figure Description
[0023] Figure 1 This is a schematic diagram of the cross-sectional structure of a thin-film sensing element; Figure 2 A schematic diagram showing the dispersion state of magnetic particles coated in the functional heating core layer; Figure 3 A schematic diagram showing the thin-film sensing element clamped at the lap joint interface of the component to be welded and the welding principle. Figure 4 This is a process flow diagram for the fabrication of thin-film sensing elements; Figure 5 A temperature comparison curve between the edge of a patterned zoned sensing element and an unpatterned whole film; Among them, 1. Thin film sensing element; 101. Functional heating core layer; 102. Resin skin layer; 3. Thermoplastic composite material component to be welded; 4. Welding pressure; 5. Alternating magnetic field; 6. Thermoplastic resin matrix; 7. Magnetic particles. Detailed Implementation
[0024] The specific embodiments of the present invention are described below to enable those skilled in the art to understand the present invention. However, it should be understood that the present invention is not limited to the scope of the specific embodiments. For those skilled in the art, various changes are obvious as long as they are within the spirit and scope of the present invention as defined and determined by the appended claims. All inventions utilizing the concept of the present invention are protected.
[0025] Example 1: Thin-film sensing element like Figure 1As shown, this embodiment provides a thin-film induction element 1 for induction welding of thermoplastic composite materials. The thin-film induction element 1 is a thermoplastic resin composite film filled with magnetic particles, comprising a functional heating core layer 101 and a resin skin layer 102 covering at least one side of the functional heating core layer 101 along its thickness direction. The functional heating core layer 101 includes a thermoplastic resin matrix 6 and magnetic particles 7 dispersed in the thermoplastic resin matrix 6. Under the action of an alternating magnetic field 5, the magnetic particles 7 generate hysteresis loss, causing the functional heating core layer 101 to heat up. The resin skin layer 102 is integrally bonded to the functional heating core layer 101. The thin-film induction element 1 as a whole does not contain a continuous metal conductive network or a continuous carbon fiber conductive network. The thin-film induction element 1 is used to be sandwiched between the overlapping interfaces of the thermoplastic composite material components 3 to be welded. Under the alternating magnetic field 5 and applied pressure 4, the thermoplastic resin matrix 6 in the thin-film induction element 1 melts and bonds with the resin matrix of the thermoplastic composite material components 3 to be welded, thereby achieving the connection between the thermoplastic composite material components 3 to be welded.
[0026] In this embodiment, the resin skin layer 102 can cover both surfaces of the functional heating core layer 101, forming a symmetrical three-layer structure consisting of two resin skin layers 102 and the functional heating core layer 101 sandwiched between the two resin skin layers 102. The thickness of each resin skin layer 102 is 1% to 20% of the total thickness of the thin-film sensing element 1, for example, 1%, 5%, 10%, 15%, 20%, etc. The mass fraction of magnetic particles 7 in the resin skin layer 102 is 0 to 10 wt%, that is, the resin skin layer 102 can be completely free of magnetic particles 7, or it can contain a small amount of magnetic particles 7 but not exceeding 10 wt%. The symmetrical skin layers on both sides make the thermal stress of the film symmetrical during hot pressing and welding, reducing warping; when the skin layer thickness is too thin, it is difficult to form a continuous clean resin transition zone at the welding interface; when the thickness is too large, it will reduce the heat transfer efficiency of the core layer to the base material and reduce the heat generation capacity per unit volume. By controlling the content of magnetic particles in the skin layer to no more than 10 wt%, a large number of magnetic particles can be avoided from being exposed at the welding interface while maintaining the compatibility between the skin layer and the core layer.
[0027] The magnetic particles 7 are Fe3O4 particles. Fe3O4 has high saturation magnetization and hysteresis loss, making it suitable as a heating filler under alternating magnetic field 5. The mass fraction of magnetic particles 7 in the functional heating core layer 101 is 30wt% to 80wt%, for example, 30wt%, 40wt%, 50wt%, 60wt%, 70wt%, 80wt%, etc. If the mass fraction is too low, the number of heating points per unit volume is insufficient, the heating rate is low, and it is difficult to reach the welding temperature within a reasonable time. If the mass fraction is too high, the continuous phase ratio of thermoplastic resin decreases, the powder formability and film mechanical integrity deteriorate, and the distance between particles is too close, which increases the risk of local conductive paths even with a coating layer. Controlling the content within the above range can achieve a balance between heat generation capacity, dispersibility, and film structural stability.
[0028] The average particle size of Fe3O4 particles is 50 nm to 5 μm, for example, it can be 50 nm, 100 nm, 300 nm, 500 nm, 1 μm, 3 μm, 5 μm, etc. Furthermore, the average particle size of Fe3O4 particles is less than one-tenth of its skin depth at the operating frequency of the alternating magnetic field 5, ensuring uniform magnetization of the Fe3O4 particles within the volume range. The heat generation of the functional heating core layer 101 is mainly due to hysteresis loss. The skin depth is related to the material's resistivity, permeability, and angular frequency. When the particle size is much smaller than the skin depth, the magnetic field distribution inside the particles is uniform, the particles as a whole participate in magnetization, and the heat generation is mainly due to hysteresis loss, avoiding surface-concentrated heating caused by the skin effect. If the particle size is too small, it is prone to agglomeration; if the particle size is too large, the internal magnetization of the particles is uneven, and the number of heating points per unit volume decreases. This limitation makes the heat generation mechanism of the functional heating core layer 101 clear, and the temperature field more uniform.
[0029] Specifically, the skin depth δ of Fe3O4 particles at its operating frequency can be determined according to... Estimate, among which, ρ For particle resistivity, μ 0 is the permeability of free space. μ r The relative permeability, ω =2π f The angular frequency is used. For Fe3O4 particles with an average particle size in the range of 100 nm to 1 μm, a working frequency of 50 kHz to 500 kHz is selected. This ensures that the particle size is less than one-tenth of the skin depth at this frequency, guaranteeing uniform magnetization within the particle volume and heat generation primarily through hysteresis loss. As an example: for particles with an average particle size of approximately 300 nm, a working frequency of approximately 100 kHz can be used, combined with appropriate clamping and pressure timing; for particles with an average particle size close to 1 μm, the working frequency can be appropriately reduced or the particle size decreased to maintain the hysteresis-dominated heating mechanism. The above correspondence can be calibrated through heating rate and temperature field uniformity tests under different particle size or frequency combinations.
[0030] like Figure 2 As shown, the magnetic particles 7 undergo surface treatment to form a coating layer. This coating layer is an electrically insulating and oxidation-resistant dense coating layer, selected from at least one of silica coating layers, alumina coating layers, silane coupling agent crosslinking layers, titanate coupling agent crosslinking layers, or organic polymer coating layers. The magnetic particles 7 are dispersed in the thermoplastic resin matrix 6 as core-shell particles encapsulated by the coating layer, with adjacent core-shell particles electrically isolated from each other by the coating layer or the thermoplastic resin matrix 6. The insulating coating layer blocks the electronic conduction path between particles at high filler weights, preventing the formation of a continuous conductive path even when particles make geometric contact, thereby suppressing eddy currents and leakage currents. The oxidation-resistant coating layer blocks oxygen diffusion, inhibiting the transformation of Fe3O4 to γ-Fe2O3 or α-Fe2O3 under hot pressing and welding high temperatures, maintaining saturation magnetization and heat generation capacity. This ensures that heat generation is mainly due to hysteresis loss, improving the consistency of heat generation across multiple welding cycles and batches.
[0031] The thermoplastic resin matrix 6 is the same as or compatible with the matrix resin of the thermoplastic composite component 3 to be welded. The thermoplastic resin is one or more of the following: polyolefin resin, polyester resin, polyamide resin, polycarbonate resin, polyimide resin, polyphenylene sulfide resin, polyetheretherketone resin, polyetherketoneketone resin, and polyetherimide resin. When the matrix resins are the same or compatible, sufficient molecular chain diffusion and entanglement can occur at the interface between the film skin layer and the base material in the molten state, forming a continuous interface after cooling, reducing interface defects caused by resin incompatibility. As a preferred example, the thermoplastic resin is a polyamide resin, particularly PA6 resin. PA6 has good compatibility with the PA6 matrix in glass fiber reinforced PA6 composites, and its melting temperature is moderate, making it suitable for induction welding.
[0032] The thin-film sensing element 1 is divided into a magnetic heating zone and a magnetically depleted edge zone in a plane parallel to its surface. The magnetic heating zone corresponds to the lap welding area of the thermoplastic composite component 3 to be welded. The magnetically depleted edge zone surrounds the magnetic heating zone, and the content of magnetic particles 7 in the magnetically depleted edge zone is lower than that in the magnetic heating zone. By confining the magnetic particles 7 mainly within the plane corresponding to the lap welding area, the effective heat generation area under the alternating magnetic field 5 is geometrically matched with the weld. The low heat generation in the magnetically depleted edge zone can suppress the continuous heat generation of the suspended film and edge outside the lap area in the magnetic field, reduce edge overheating, resin degradation and uncontrolled glue overflow, improve the spatial uniformity of the temperature field, and reduce ineffective heating and edge thermal damage.
[0033] The thin-film sensing element 1 can also form a concentration gradient structure in the thickness direction. For example, from one surface to the other, it consists of a resin skin layer 102, a low-magnetic transition layer, a high-magnetic-functional heating core layer 101, another low-magnetic transition layer, and the resin skin layer 102. The content of magnetic particles 7 in the low-magnetic transition layer is lower than that in the high-magnetic-functional heating core layer 101 but higher than that in the resin skin layer 102. The gradient distribution further smooths the abrupt change in magnetic content between the core layer and the skin layer, which is beneficial for mitigating interlayer thermal stress and magnetocaloric mismatch.
[0034] Example 2: Method for fabricating thin-film sensing elements This embodiment provides a method for preparing the thin-film sensing element 1 described above, such as... Figure 4 As shown, it includes the following steps.
[0035] Step 1: Raw Material Pretreatment and Drying: Thermoplastic resin powder and magnetic particles 7 are provided, and both are dried to remove moisture. The thermoplastic resin powder can be PA6 powder with an average particle size of approximately 80 μm, a melting point of approximately 220℃, and a moisture content of less than 0.1% after vacuum drying. The magnetic particles 7 can be Fe3O4 particles with an average particle size of approximately 300 nm, a magnetite phase, and a saturation magnetization of not less than approximately 80 emu / g.
[0036] Step 2, Mixing and Dispersion: The thermoplastic resin powder and magnetic particles 7 are mixed according to the functional heating core layer formulation and the resin skin layer formulation, respectively. Dispersion is achieved using mechanical stirring, ball milling, ultrasonic dispersion, or a combination thereof, to obtain the mixed powder for the functional heating core layer and the powder for the resin skin layer. For example, modified Fe3O4 particles and PA6 powder are mixed at a mass ratio of 60:40 as the core layer material, ball-milled, dispersed, and then sieved; pure PA6 powder is used as the skin layer material. Before mixing and dispersion, the magnetic particles 7 can be surface-treated to form an electrically insulating and antioxidant coating layer. For example, Fe3O4 particles are ultrasonically dispersed in an ethanol-water solution of KH-550 and refluxed, then washed and dried to obtain surface-silanized modified Fe3O4 particles. The silane crosslinking layer forms an electrically insulating and oxygen-diffusion-blocking thin layer on the particle surface, while simultaneously improving the interfacial wetting between the particles and PA6. Before hot pressing, the magnetic particles 7 and the thermoplastic resin powder can be pre-dispersed by one or more of the following methods: dry powder mixing, solvent-assisted dispersion, ball milling dispersion, ultrasonic dispersion, or melt blending, so that the magnetic particles 7 are uniformly attached to or distributed on the surface of the thermoplastic resin powder and in the gaps therebetween; then the resulting mixed powder is dried, sieved or granulated, and then layered powder spreading and hot pressing are carried out.
[0037] Step 3: Layered Powder Laying and Molding: The resin skin layer powder and the functional heating core layer powder are laid layer by layer in the mold according to a preset sequence, forming a laminated powder blank containing both the resin skin layer blank and the functional heating core layer blank. For example, a skin layer material with a thickness of about 40 μm is first laid in the mold, then a core layer material with a thickness of about 220 μm is evenly laid on it, and finally another skin layer material with a thickness of about 40 μm is laid, resulting in a laminated powder blank with a total thickness of about 300 μm, with the skin layers on both sides each accounting for about 13% of the total thickness; the uniformity of the thickness of each layer is controlled during powder laying. The functional heating core layer blank and the resin skin layer blank are laid and formed in one step in step 3.
[0038] Step 4: Hot Pressing: The laminated powder blank after molding is placed in a hot press and heated to a temperature higher than the melting or softening point of the thermoplastic resin. Under pressure, the temperature is maintained, causing the resin layers to melt and flow, the interlayer interfaces to fuse, and the magnetic particles 7 to be coated. This process is repeated once to form a composite film with integrated interlayer bonding. Hot pressing can be performed in an inert atmosphere or vacuum environment, with the inert atmosphere being nitrogen or argon. The heating temperature for hot pressing is 10°C to 50°C above the melting or softening point of the thermoplastic resin; for example, for PA6, it is heated to approximately 240°C, about 20°C above the melting point of PA6. The hot pressing pressure is 0.5MPa to 15MPa, for example, about 3MPa. The holding time is 1min to 30min, for example, about 8min. The functional heating core layer blank and the resin skin layer blank are hot-pressed into a single unit in step 4.
[0039] Step 5, Cooling and Shaping: After hot pressing, cool to room temperature or target temperature under pressure, then demold to obtain thin-film sensing element 1. Cooling and shaping can be carried out in an inert atmosphere or vacuum environment. For example, after cooling to about 60°C under holding pressure, demold to obtain a symmetrical three-layer Fe3O4 / PA6 thin-film sensing element 1. The resulting thin film layers are bonded together without adhesive, and there is no delamination when bent; observation of the film cross-section shows a continuous transition between the resin skin layer 102, which is basically free of magnetic particles 7, and the functional heating core layer 101.
[0040] After obtaining the formed thin-film sensing element 1, at least one post-processing process can be applied to it to adjust the dimensional accuracy, surface condition, and interfacial bonding performance of the thin-film sensing element 1. The post-processing process includes one or a combination of cutting, drying, annealing, surface cleaning, plasma treatment, ozone oxidation treatment, surface roughening treatment, or hot pressing leveling treatment.
[0041] Example 3: Application of Thin-Film Sensing Elements This embodiment provides an application of the aforementioned thin-film sensing element 1. For example... Figure 3As shown, a thin-film sensing element 1 is sandwiched between two or more thermoplastic composite material components 3 to be welded, such that the extension direction of the functional heating core layer 101 corresponds to the overlapping welding area of the thermoplastic composite material components 3 to be welded. The thermoplastic composite material components 3 to be welded are fiber-reinforced thermoplastic composite materials, such as glass fiber reinforced PA6 composite material, with a glass fiber mass fraction of approximately 30%. The assembly is placed in an induction coil, and under the action of an alternating magnetic field 5, induced heat is generated through the hysteresis loss of the magnetic particles 7 in the functional heating core layer 101, causing the functional heating core layer 101 and the thermoplastic resin at the overlapping interface to melt. Under external pressure 4, the fusion connection between the thermoplastic composite material components 3 to be welded is completed through heat preservation and pressure cooling.
[0042] The alternating magnetic field 5 operates at a frequency of 50kHz to 500kHz, for example, approximately 100kHz. During welding, the target temperature at the lap joint is controlled to be 10°C to 60°C above the melting or softening point of the resin matrix of the thermoplastic composite component 3 to be welded; for example, for a PA6 matrix, the target temperature is approximately 245°C. The pressure applied to the lap joint area during welding is 0.05MPa to 2MPa, for example, approximately 0.3MPa. The welding sequence is as follows: first, the alternating magnetic field 5 is applied under pressure to raise the interface temperature to the target temperature and held; then, the application of the alternating magnetic field 5 is stopped, and the interface is cooled until the resin matrix is completely cured while maintaining or increasing the pressure before releasing the pressure. For example, the lap joint temperature is raised to approximately 245°C and held for approximately 30 seconds, while simultaneously applying a welding pressure of approximately 0.3MPa; subsequently, the application of the alternating magnetic field 5 is stopped, and the interface is cooled to below approximately 80°C under pressure before releasing the pressure to complete the welding. During the welding process, the functional heating core layer 101 acts as the main heat source for localized heat generation, while the resin skin layers 102 on both sides and the interface resin of the base material melt together and diffuse into each other. Since the resin skin layer 102 basically does not contain magnetic particles 7, a continuous phase mainly composed of base material resin and component resin is formed in the central area of the welding interface, which helps to reduce the exposure of particles at the interface and in the overflow tape.
[0043] like Figure 5 As shown, the comparative example uses an unpatterned whole-film sensing element. Under the same welding conditions, the outer edge of its overlap area continuously generates heat under the action of the alternating magnetic field 5. The temperature within 0-2 mm from the edge of the film rapidly rises to about 250°C, exceeding the degradation temperature of PA6 resin (about 230°C), forming a significant edge overheating zone, which easily leads to resin thermal degradation and uncontrolled glue overflow. In contrast, this embodiment uses a patterned partitioned sensing element 1 with a magnetic heating zone and a magnetically depleted edge zone. The magnetic particle content 7 in the magnetically depleted edge zone is low, significantly reducing heat generation. Under the same welding conditions, the temperature within 0-2 mm from the edge of the film is only about 150°C, which is lower than the degradation temperature of PA6 resin. This effectively suppresses edge overheating, resin degradation, and uncontrolled glue overflow, improving the spatial uniformity of the temperature field and the joint forming quality.
[0044] The magnetic particles 7 can also be ferrite materials with Curie temperatures ranging from 10°C to 60°C above the melting or softening point of the resin matrix of the thermoplastic composite component 3 to be welded. The ferrite material is at least one of manganese-zinc ferrite, nickel-zinc ferrite, or doped and modified Fe3O4. Replacing the magnetic particles 7 with manganese-zinc or nickel-zinc ferrites with adjustable Curie temperatures allows the Curie temperature to be adjusted within the range of approximately 100°C to 300°C depending on the content of components such as Zn. Ferrites with Curie temperatures ranging from 10°C to 60°C above the melting point of the base resin can be selected; for example, for PA6 with a melting point of approximately 220°C, a ferrite with a Curie temperature of approximately 240°C to 270°C can be selected. When the interface temperature rises to near this Curie temperature, the material's hysteresis loss decreases significantly, and heat generation spontaneously weakens, thus self-limiting the interface temperature within the processing window and preventing overheating degradation without temperature feedback. This solution can serve as a substitute for or supplement to temperature control feedback.
[0045] For the stacked connection of two or more components, a multilayer thin film sensing element 1 containing two or more functional heating core layers 101 and separated by resin layers can be used, or multiple of the above three-layer thin films can be placed on each adjacent interface and the connection of multiple interfaces can be completed simultaneously during a single magnetic field application process; each interface shares the same welding sequence and pressure, which is beneficial to improving the efficiency and consistency of the connection of multilayer components.
[0046] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Those skilled in the art can adjust the material type, layer thickness ratio, particle content, process parameters, and welding sequence without departing from the concept of the present invention, and all such adjustments should fall within the protection scope defined by the claims of the present invention.
Claims
1. A thin-film induction element for induction welding of thermoplastic composite materials, characterized in that, The thin-film sensing element (1) is a magnetic particle-filled thermoplastic resin composite film, comprising along its thickness direction: a functional heating core layer (101), the functional heating core layer (101) comprising a thermoplastic resin matrix (6) and magnetic particles (7) dispersed in the thermoplastic resin matrix (6), the magnetic particles (7) generating hysteresis loss under the action of an alternating magnetic field (5) to heat up the functional heating core layer (101); and a resin skin layer (102) covering at least one side surface of the functional heating core layer (101), and the resin skin layer (102) The skin layer (102) is integrally combined with the functional heating core layer (101); the thin film sensing element (1) does not contain a continuous metal conductive network and a continuous carbon fiber conductive network; the thin film sensing element (1) is used to be sandwiched between the overlapping interfaces of the thermoplastic composite component (3) to be welded, and under the alternating magnetic field (5) and external pressure (4), the thermoplastic resin matrix (6) in the thin film sensing element (1) is melted and bonded with the resin matrix of the thermoplastic composite component (3) to be welded, thereby realizing the connection between the thermoplastic composite components (3) to be welded.
2. The thin-film sensing element according to claim 1, characterized in that, The resin skin layer (102) covers the two surfaces of the functional heating core layer (101) respectively, forming a symmetrical three-layer structure consisting of two resin skin layers (102) and the functional heating core layer (101) sandwiched between the two resin skin layers (102); the thickness of each resin skin layer (102) is 1% to 20% of the total thickness of the thin film sensing element (1); the mass fraction of magnetic particles (7) in the resin skin layer (102) is 0 to 10 wt%.
3. The thin-film sensing element according to claim 1 or 2, characterized in that, The magnetic particles (7) are Fe3O4 particles; the mass fraction of the magnetic particles (7) in the functional heating core layer (101) is 30wt% to 80wt%.
4. The thin-film sensing element according to claim 3, characterized in that, The average particle size of the Fe3O4 particles is 50nm to 5μm; and the average particle size of the Fe3O4 particles is less than one-tenth of its skin depth at the working frequency of the alternating magnetic field (5), so that the Fe3O4 particles are uniformly magnetized within the volume range, and the heat generation of the functional heating core layer (101) is mainly due to hysteresis loss.
5. The thin-film sensing element according to claim 1, characterized in that, The magnetic particles (7) are surface treated to form a coating layer, which is an electrically insulating and oxidation-resistant dense coating layer selected from at least one of silica coating layer, alumina coating layer, silane coupling agent crosslinking layer, titanate coupling agent crosslinking layer or organic polymer coating layer; the magnetic particles (7) are dispersed in the thermoplastic resin matrix (6) in the form of core-shell particles wrapped by the coating layer, and adjacent core-shell particles are electrically isolated from each other by the coating layer or the thermoplastic resin matrix (6).
6. The thin-film sensing element according to claim 1, characterized in that, The thermoplastic resin matrix (6) is the same as or compatible with the matrix resin of the thermoplastic composite component (3) to be welded; the thermoplastic resin is one or more of the following: polyolefin resin, polyester resin, polyamide resin, polycarbonate resin, polyimide resin, polyphenylene sulfide resin, polyether ether ketone resin, polyether ketone ketone resin, and polyetherimide resin.
7. The thin-film sensing element according to claim 1, characterized in that, The thin-film sensing element (1) is divided into a magnetic heating area and a magnetic depletion edge area in a plane parallel to its surface. The magnetic heating area is used to correspond to the lap welding area of the thermoplastic composite component (3) to be welded. The magnetic depletion edge area is arranged around the magnetic heating area, and the content of magnetic particles (7) in the magnetic depletion edge area is lower than the content of magnetic particles (7) in the magnetic heating area.
8. A method for preparing a thin-film sensing element according to any one of claims 1 to 7, characterized in that, Includes the following steps: Step 1, Raw material pretreatment and drying: Provide thermoplastic resin powder and magnetic particles, and dry the thermoplastic resin powder and magnetic particles respectively; Step 2, Mixing and Dispersion: The thermoplastic resin powder and magnetic particles are mixed according to the functional heating core layer formula and the resin skin layer formula, respectively, and dispersed by mechanical stirring, ball milling, ultrasonic dispersion or a combination thereof to obtain the mixed powder for the functional heating core layer and the powder for the resin skin layer. Step 3, Layered Powdering and Molding: The mixed powder of the resin skin layer and the functional heating core layer is laid layer by layer in the mold according to a preset sequence, so that the laid powder forms a stacked powder blank containing the resin skin layer blank and the functional heating core layer blank. Step 4: Hot pressing: The stacked powder blank after being molded is placed in a hot pressing equipment and heated to a temperature higher than the melting point or softening point of the thermoplastic resin. It is kept at a temperature under pressure so that the resin of each layer melts and flows, the interlayer interface fuses and coats the magnetic particles, and the composite film with interlayer integral bonding is formed in one hot pressing. Step 5, Cooling and Shaping: After hot pressing, the material is cooled to room temperature or target temperature under pressure, and then demolded to obtain a thin-film sensing element.
9. The preparation method according to claim 8, characterized in that, Before mixing and dispersing, the magnetic particles are surface-treated to form an electrically insulating and oxidation-resistant coating layer. Before hot pressing, the magnetic particles and thermoplastic resin powder are pre-dispersed using one or more of the following methods: dry powder mixing, solvent-assisted dispersion, ball milling dispersion, ultrasonic dispersion, or melt blending. The resulting mixed powder is then dried, sieved, or granulated before being layered and hot-pressed. The hot pressing or cooling is performed in an inert atmosphere or vacuum environment, wherein the inert atmosphere is nitrogen or argon. The heating temperature for hot pressing is 10°C to 50°C above the melting or softening point of the thermoplastic resin, the hot pressing pressure is 0.5MPa to 15MPa, and the holding time is 1min to 30min. The functional heating core layer blank and the resin skin layer blank are laid and formed in one step in step three, and then hot-pressed into a whole in step four.
10. An application of the thin-film sensing element (10) according to any one of claims 1 to 7, characterized in that, The thin-film sensing element (1) is sandwiched between two or more thermoplastic composite material components (3) to be welded, so that the extension direction of the functional heating core layer (101) corresponds to the overlapping welding area of the thermoplastic composite material components (3) to be welded. Under the action of the alternating magnetic field (5), induced heat is generated through the hysteresis loss of the magnetic particles (7) in the functional heating core layer (101), causing the thermoplastic resin at the overlapping interface of the functional heating core layer (101) to melt, and the fusion connection between the thermoplastic composite material components (3) to be welded is completed under external pressure (4) through heat preservation and pressure cooling; the thermoplastic composite material components (3) to be welded are fiber-reinforced thermoplastic composite materials; the working frequency of the alternating magnetic field (5) is 50kHz to 500kHz; welding During the process, the target temperature at the interface is controlled at 10°C to 60°C above the melting point or softening point of the resin matrix of the thermoplastic composite component (3) to be welded; the pressure applied to the interface during welding is 0.05MPa to 2MPa; the welding sequence is as follows: first, an alternating magnetic field (5) is applied under pressure to raise the interface to the target temperature and keep it at that temperature, then the alternating magnetic field (5) is stopped, and the interface is cooled until the resin matrix is completely cured while maintaining or increasing the pressure before the pressure is released; the magnetic particles (7) are ferrite materials with a Curie temperature in the range of 10°C to 60°C above the melting point or softening point of the resin matrix of the thermoplastic composite component (3) to be welded; the ferrite material is at least one of manganese zinc ferrite, nickel zinc ferrite or Fe3O4 that has been doped and modified.