A processing technology for FPC cover film based on modified polyimide

By modifying the processing technology of polyimide precursor resin, high peel strength and low dielectric loss of adhesive-free polyimide cover film were achieved, solving the problems of insufficient dielectric loss and peel strength in high-frequency signal transmission and meeting the requirements of high-frequency FPC for 5G communication.

CN123104094APending Publication Date: 2026-11-17JIANGXI YIDONG ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611455301.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polyimide cover films suffer from high dielectric loss and insufficient peel strength during high-frequency signal transmission, making it difficult to meet the requirements of high-frequency FPCs for 5G communication.

Method used

By using modified polyimide precursor resin through slit extrusion coating, pre-imidization gradient drying, and three-stage programmed temperature rise hot pressing, combined with fluorine-containing surface modification, an integrated system of adhesive-free interface anchoring, self-relieving bulk stress, and low dielectric surface is achieved.

Benefits of technology

This improves the peel strength of the cover film and reduces dielectric loss, meeting the comprehensive requirements of high peel strength, low dielectric loss, and high reliability for high-frequency flexible printed circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to the field of electronic materials technology, specifically to a processing technology for an FPC cover film based on modified polyimide. The processing technology for an FPC cover film based on modified polyimide uses a modified polyimide precursor resin and a release PET film as its bases. The modified polyimide precursor resin is the sole functional medium. Through the synergistic effects of slot extrusion coating, pre-imidization gradient drying, three-stage programmed temperature hot pressing, and fluorine-containing surface modification, an integrated system of adhesive-free interface anchoring, self-elimination of bulk stress, and in-situ generation of a low-dielectric surface is achieved, resulting in an FPC cover film based on modified polyimide. This invention solves the problems of insufficient peel strength and warping deformation caused by internal stress accumulation in existing adhesive-free cover films, and the difficulty in simultaneously meeting the requirements of low-dielectric-loss cover films for high-frequency FPCs. It provides an integrated FPC cover film solution that spontaneously completes interface chemical anchoring, self-elimination of bulk stress, and generation of a low-dielectric surface within the modified polyimide film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electronic materials technology, and more specifically to a processing technology for an FPC cover film based on modified polyimide. Background Technology

[0002] Polyimide cover films are widely used in the protection of flexible printed circuits (FPCs) due to their excellent heat resistance, dimensional stability, and insulation properties. Their core structure consists of a three-layer composite material formed by hot-pressing a polyimide film coated with epoxy resin or acrylate adhesive onto a copper trace. However, in existing three-layer cover films, the dielectric constant and dielectric loss tangent of the adhesive layer are significantly higher than those of the polyimide substrate, leading to severe signal attenuation and heat generation during high-frequency signal transmission. This makes it difficult to meet the low dielectric loss requirements of high-frequency FPCs used in 5G communication. To reduce dielectric loss, the industry has attempted to remove the adhesive layer to achieve adhesive-free integration. However, the bonding between the adhesive-free polyimide film and the copper surface relies solely on physical adsorption, resulting in a peel strength far lower than that of adhesive-based systems. This makes them prone to delamination failure during subsequent processing and use.

[0003] Currently, the main approaches to achieving interface enhancement of adhesive-free polyimide capping films include copper surface roughening and polyimide surface plasma treatment. Copper surface roughening increases the specific surface area of ​​the copper surface through chemical micro-etching to enhance mechanical anchoring, but the roughened copper surface generates a skin effect at high frequencies, increasing conductor losses. Although plasma treatment can introduce polar groups on the polyimide surface to improve interfacial wettability, the treatment effect decays over time, resulting in insufficient long-term reliability. Therefore, there is an urgent need to develop an integrated capping film preparation method that can spontaneously form stable interfacial chemical bonds under adhesive-free conditions, while also possessing internal stress relief capabilities and a low dielectric surface, to simultaneously meet the comprehensive requirements of high-frequency flexible printed circuits for high peel strength, low dielectric loss, and high reliability.

[0004] To address the above problems, the present invention provides a solution. Summary of the Invention

[0005] The purpose of this invention is to provide a processing technology for FPC cover film based on modified polyimide, which can achieve adhesive-free integration of the cover film, synergistic effects of high peel strength and low dielectric loss, and at the same time endow the cover film with a self-stress relief function. To achieve the above objectives, the present invention adopts the following technical solution: a processing technology for an FPC cover film based on modified polyimide, using modified polyimide precursor resin and release PET film as the basis, with modified polyimide precursor resin as the only functional medium, through the synergistic effect of slit extrusion coating, pre-imidization gradient drying, three-stage programmed temperature hot pressing and fluorine-containing surface modification, to achieve the integration of adhesive-free interface anchoring, self-elimination of bulk stress and in-situ generation of low dielectric surface, thus obtaining an FPC cover film based on modified polyimide; Furthermore, the modified polyimide precursor resin is composed of the following components by weight percentage: 52% 4,4'-(hexafluoroisopropene)phthalic anhydride, 12% 3,3'-diamino-N-methyldipropylamine, 6% terephthalaldehyde, 10% tert-butyl 3,5-diaminobenzoate, 5% methoxy polyethylene glycol monoamine, 3.5% phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 1.2% dicumyl peroxide, 4% ethoxylated trimethylolpropane triacrylate, 1.5% polypropylene glycol diglycidyl ether, 2.5% octaphenyl cage-like silsesquioxane, 1.5% nano silica, 0.5% pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and 0.3% tris(2,4-di-tert-butylphenyl) phosphite; Furthermore, the preparation method of the modified polyimide precursor resin includes the following steps: A1: Place terephthalaldehyde in a vacuum drying oven, set the temperature to 50-70℃, and the vacuum degree to -0.08 to -0.10 MPa, and dry for 8-12 hours to obtain dried terephthalaldehyde. Place 3,3'-diamino-N-methyldipropylamine in a vacuum drying oven, set the temperature to 40-60℃, and the vacuum degree to -0.08 to -0.10 MPa, and dry for 6-10 hours to obtain dried 3,3'-diamino-N-methyldipropylamine. A2: Under nitrogen protection, add anhydrous ethanol to a reactor equipped with a mechanical stirrer, a reflux condenser, and a constant-pressure dropping funnel. The mass ratio of anhydrous ethanol to terephthalaldehyde is 10:1. Set the stirrer speed to 400-500 rpm. Add the dried terephthalaldehyde to the reactor and stir for 5-10 minutes. Raise the reactor temperature to 60-70°C to bring the components in the reactor to a reflux state. Add the dried 3,3'-diamino-N-methyldipropylamine to the anhydrous ethanol and mix at 300 rpm for 5 minutes. The mass ratio of dried 3,3'-diamino-N-methyldipropylamine to anhydrous ethanol is 1:1. After mixing, transfer to a constant-pressure reactor. The solution was added dropwise to a dropping funnel, followed by a solution of terephthalaldehyde over a period of 40-60 minutes. After the addition was complete, the reaction was continued under reflux for 3-5 hours. After the reaction was complete, the reaction solution was cooled to room temperature and transferred to a rotary evaporator. The solvent was removed by rotary evaporation at 40-50°C and -0.08 to -0.10 MPa to obtain a crude product. The crude product was then recrystallized twice with anhydrous ethanol to obtain a recrystallized product. The amount of anhydrous ethanol used in each recrystallization was 8 times the mass of the crude product. The recrystallized product was placed in a vacuum drying oven at a temperature of 50-60°C and a vacuum of -0.08 to -0.10 MPa for 8-12 hours to obtain a Schiff base-containing diamine. A3: Place the Schiff base-containing diamine in a vacuum drying oven, set the temperature to 60-80℃, and the vacuum degree to -0.08 to -0.10 MPa, and dry for 8-12 hours to obtain dried Schiff base-containing diamine. Place tert-butyl 3,5-diaminobenzoate in a vacuum drying oven, set the temperature to 50-70℃, and the vacuum degree to -0.08 to -0.10 MPa, and dry for 10-14 hours to obtain dried tert-butyl 3,5-diaminobenzoate. Place methoxy polyethylene glycol monoamine in a vacuum drying oven, set the temperature to 40-60℃, and the vacuum degree to -0.08 to -0.10 MPa, and dry for 6-10 hours to obtain dried methoxy polyethylene glycol monoamine. A4: Add dried Schiff base-containing diamine and dried tert-butyl 3,5-diaminobenzoate into a reaction vessel and stir at 200 rpm for 5 min to obtain a mixed diamine. Then, under nitrogen protection, add N,N-dimethylacetamide to the reaction vessel, wherein the mass ratio of N,N-dimethylacetamide to the mixed diamine is 5:1. Start stirring and control the temperature of the reaction vessel at -5 to 5℃. Stir under nitrogen bubbling conditions until completely dissolved for 30-60 min to obtain a diamine solution. A5: Under nitrogen protection, keep the reactor temperature at -5 to 5℃, add 4,4'-(hexafluoroisopropene)diphthalic anhydride to the diamine solution in 3-5 batches, with an interval of 20-30 minutes between each addition. After the addition is completed, continue stirring and reacting at -5 to 5℃ for 2-4 hours. Then raise the reactor temperature to 20-30℃ and continue stirring and reacting for 2-4 hours to obtain a polyamic acid solution. A6: Add dried methoxy polyethylene glycol monoamine and N,N-dimethylacetamide to a reaction vessel, set the stirrer speed to 200 rpm, and stir for 5 min. The mass ratio of dried methoxy polyethylene glycol monoamine to N,N-dimethylacetamide is 1:1. After mixing, transfer to a constant pressure dropping funnel, and then add dropwise to a polyamic acid solution. The dropwise addition time is 30-60 min. After the dropwise addition is completed, continue stirring the reaction at 20-30℃ for 2-4 h to obtain a capped polyamic acid solution. A7: Place octaphenyl cage-type silsesquioxane in a vacuum drying oven, set the temperature to 100-120℃, and the vacuum degree to -0.08 to -0.10MPa, and dry for 6-10 hours to obtain dried octaphenyl cage-type silsesquioxane. Place nano-silica in a vacuum drying oven, set the temperature to 100-120℃, and the vacuum degree to -0.08 to -0.10MPa, and dry for 6-10 hours to obtain dried nano-silica. Add the dried octaphenyl cage-type silsesquioxane and dried nano-silica to a 10wt% end-capped polyamic acid solution, and use ultrasonic dispersion treatment with an ultrasonic power of 300-500W and an ultrasonic time of 20-40min to form a nano-filler pre-dispersion slurry. Then add the nano-filler pre-dispersion slurry to the remaining end-capped polyamic acid solution, and disperse it using a high-speed disperser at 2000-3000rpm for 30-60min to obtain a nano-filler dispersion. A8: Phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, dicumyl peroxide, ethoxylated trimethylolpropane triacrylate, polypropylene glycol diglycidyl ether, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and tris(2,4-di-tert-butylphenyl)phosphite were added to the nanofiller dispersion and stirred for 30-60 min to obtain a modified polyimide precursor resin solution. The modified polyimide precursor resin solution was transferred to a reactor equipped with a vacuum distillation device, and N,N-dimethylacetamide was removed by vacuum distillation at 40-50℃ and -0.08 to -0.10 MPa for 8-10 h to obtain the modified polyimide precursor resin. Furthermore, the ethoxylated trimethylolpropane triacrylate has a degree of ethoxylation of 3 and a molecular weight of 600 g / mol; the polypropylene glycol diglycidyl ether has a molecular weight of 500 g / mol; the methoxylated polyethylene glycol monoamine has a molecular weight of 1000 g / mol; the octaphenyl cage-type silsesquioxane has an average particle size of 3 μm; and the nano-silica has an average particle size of 20 nm and a specific surface area of ​​200 m². 2 / g.

[0006] Furthermore, a processing method for an FPC cover film based on modified polyimide includes the following steps: S1: Add the modified polyimide precursor resin to N,N-dimethylacetamide, wherein the mass ratio of the modified polyimide precursor resin to N,N-dimethylacetamide is 1:5. Stir until homogeneous to obtain a coating solution. Place the coating solution in a vacuum degassing machine, set the vacuum degree to -0.09 to -0.10 MPa, and the degassing time to 30-60 min. After degassing, uniformly coat the precursor resin onto the surface of the release PET film using a slit extrusion method. The die gap is 150-250 μm, the coating speed is 3-6 m / min, and the wet film thickness is 120-200 μm. After coating, the wet film enters a multi-stage hot air oven for pre-imidization gradient drying. The first stage has a temperature of 80-100℃ and a dwell time of 8-12 min; the second stage has a temperature of 120-140℃ and a dwell time of 6-10 min; the third stage has a temperature of 150-170℃ and a dwell time of 4-8 min; the fourth stage has a temperature of 200-220℃ and a dwell time of 3-5 min; and the fifth stage has a temperature of 260-280℃ and a dwell time of 2-4 min. There is a transition zone between each stage, with a length of 30-50 cm. After drying, the film surface enters the cooling zone and is gradually cooled to 25℃ at a cooling rate of 15-30℃ / s. Then it is wound up, and the winding tension is controlled at 15-25N to obtain a pre-imidized modified polyimide film containing a release film. S2: The pre-imidized modified polyimide film containing the release film is placed flat on the inspection table. Under an inspection light source with an illuminance of 1200lx, the uniformity and surface defects of the film surface are checked. After confirming that there are no defects such as bubbles, pinholes and particulate impurities, the pre-imidized film is cut to the size of the target FPC width. After cutting, the release PET film is removed, and the pre-imidized modified polyimide film is covered on the FPC substrate with the circuit processing completed, with the film side facing the copper circuit side. Pre-lamination is performed using a roll laminator. The roll lamination temperature is set to 40-60℃, the roll lamination line pressure is 10-20N / cm, and the roll lamination speed is 0.5-1.5m / min. After pre-lamination, the component to be pressed is obtained. S3: The component to be pressed is fed into the vacuum press, and the vacuum degree is set to -0.095 to -0.10 MPa. A three-stage temperature and pressure process is used for hot pressing. The first stage is set with a pressing temperature of 160-180℃, a pressing pressure of 0.5-1.5 MPa, and a holding time of 10-15 min. The second stage is set with a pressing temperature of 230-250℃, a pressing pressure of 2.5-3.5 MPa, and a holding time of 25-35 min. The third stage is set with a pressing temperature of 250-270℃, a pressing pressure of 1.5-2.5 MPa, and a holding time of 15-25 min. After the three stages are completed, while maintaining a holding pressure of 0.5-1 MPa, the component is gradually cooled to below 50℃ at a cooling rate of 5-10℃ / min. The pressure is then released and the component is removed to obtain the integrated FPC substrate. S4: Lay the integrated FPC substrate flat on the inspection table and check the surface flatness and interface bonding quality of the cover film under an inspection light source with an illuminance of 1200lx. After confirming that there are no bubbles, delamination and local unbonded defects, send the integrated FPC substrate into the laser processing platform. Use an ultraviolet picosecond laser to perform windowing and shape cutting processing on the cover film. Set the laser wavelength to 355nm, the pulse width to 10-15ps, the repetition frequency to 500-1000kHz, the cutting speed to 200-500mm / s, and the laser focus to the middle plane in the thickness direction of the cover film. After processing, blow the processed surface with compressed air of 0.3-0.5MPa to remove processing debris and obtain a semi-finished FPC cover film. S5: Perfluorodecyltrimethoxysilane was added to anhydrous ethanol and stirred at 300 rpm for 15 min. Then, deionized water was added, and the stirring and hydrolysis were continued for 30 min while maintaining the same speed to obtain a fluorinated surface modification treatment solution. The mass ratio of perfluorodecyltrimethoxysilane, anhydrous ethanol and deionized water was 2:90:8. The semi-finished FPC cover film was sent to a plasma treatment device, and the surface of the cover film was cleaned and activated online using low-pressure plasma in an argon atmosphere. The treatment power was set to 200-400W, the argon flow rate was 50-100sccm, the treatment pressure was 20-50Pa, and the treatment time was 60-120s. After the treatment, the semi-finished FPC cover film was sent to an impregnation device and impregnated with the fluorinated surface modification treatment solution for 30-60s. The liquid retention rate was controlled at 50-70%. After impregnation, the film was dried and cured with hot air at 120-140℃ for 30-45 min to obtain an FPC cover film based on modified polyimide.

[0007] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are as follows: 1. This invention utilizes the synergistic effect of the self-elimination mechanism of dynamic covalent bonds containing Schiff base diamine and the thermally induced deprotection interface anchoring mechanism of tert-butyl 3,5-diaminobenzoate to construct an integrated structure of self-repair of the cover film and chemical bonding at the interface. The dynamic covalent bonds of the Schiff base eliminate the internal stress of the polyimide molecular chain segments through a reversible exchange reaction in the later stage of hot pressing. After the thermal desorption of the tert-butyl ester protecting group, the free carboxyl groups generated in situ form chemical bonds with the copper surface to anchor the film, which significantly improves the peel strength of the cover film and greatly reduces the warpage height. This solves the problems of insufficient peel strength and warpage deformation caused by internal stress accumulation in existing adhesive-free PI cover films. 2: This invention constructs a bulk-surface dual low-dielectric system through the synergistic effect of the low-polarity fluorinated structure of 4,4'-(hexafluoroisopropene)diphthalic anhydride, the filling of low-dielectric fillers such as octaphenyl cage-type silsesquioxane and nano-silica, and the surface modification of perfluorodecyltrimethoxysilane. The fluorinated dianhydride reduces the polarizability at the molecular structure level, the nanofiller migrates and accumulates on the membrane surface to form a low-dielectric ionized interface, and the fluorinated surface modification imparts hydrophobicity and a lower dielectric constant to the membrane surface, which significantly reduces the dielectric constant and dielectric loss tangent of the cover film, thus solving the requirement of low-dielectric loss cover films for high-frequency FPCs. 3. This invention uses pre-iminolation gradient drying to bring the iminolation reaction to the coating and drying stage, reducing the interference of moisture generated during iminolation on interfacial bonding during hot pressing. At the same time, it encodes the three functions of interfacial anchoring, internal stress relief, and deep iminolation into the temperature sequence of a single hot pressing process using a three-stage programmed temperature rise hot pressing. This allows the cover film to spontaneously complete the entire process from interfacial chemical bonding to internal stress relaxation without adhesives, simplifying the traditional multilayer composite process and meeting the comprehensive requirements of flexible printed circuits for high peel strength, low dielectric loss, and high reliability. Detailed Implementation

[0008] To make the technical means, creative features, objectives and effects of this invention easier to understand, the invention will be further described below with reference to specific embodiments.

[0009] Unless otherwise specified, the experimental methods used in the following examples are conventional methods, performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Unless otherwise specified, the materials and reagents used in the following examples are commercially available.

[0010] Example 1 1. Place 600g of terephthalaldehyde in a vacuum drying oven, set the temperature to 50℃ and the vacuum degree to -0.08MPa, and dry for 8h to obtain 598g of dried terephthalaldehyde. Place 1200g of 3,3'-diamino-N-methyldipropylamine in a vacuum drying oven, set the temperature to 40℃ and the vacuum degree to -0.08MPa, and dry for 6h to obtain 1197g of dried 3,3'-diamino-N-methyldipropylamine. 2. Under nitrogen protection, add 5980g of anhydrous ethanol to a reactor equipped with a mechanical stirrer, a reflux condenser, and a constant-pressure dropping funnel. Set the stirrer speed to 400rpm. Add 598g of dried terephthalaldehyde to the reactor and stir for 5 minutes. Raise the reactor temperature to 60℃ to bring the components in the reactor to a reflux state. Add 1197g of dried 3,3'-diamino-N-methyldipropylamine to 1197g of anhydrous ethanol and mix at 300rpm for 5 minutes. After mixing, transfer the mixture to a constant-pressure dropping funnel and then add dropwise... In the reaction vessel, the dropwise addition time was 40 min. After the dropwise addition was completed, the reaction was continued under reflux for 3 h. After the reaction was completed, the reaction solution was cooled to room temperature and transferred to a rotary evaporator. The solvent was removed by rotary evaporation at 40 °C and -0.08 MPa to obtain the crude product. The crude product was then recrystallized twice with anhydrous ethanol to obtain the recrystallized product. The amount of anhydrous ethanol used in each recrystallization was 8 times the mass of the crude product. The recrystallized product was placed in a vacuum drying oven at 50 °C and a vacuum of -0.08 MPa for 8 h to obtain 1678 g of Schiff base diamine. 3: 1678g of Schiff base-containing diamine was placed in a vacuum drying oven at a temperature of 60℃ and a vacuum degree of -0.08MPa for 8 hours to obtain 1673g of dried Schiff base-containing diamine. 1000g of tert-butyl 3,5-diaminobenzoate was placed in a vacuum drying oven at a temperature of 50℃ and a vacuum degree of -0.08MPa for 10 hours to obtain 997g of dried tert-butyl 3,5-diaminobenzoate. 500g of methoxy polyethylene glycol monoamine was placed in a vacuum drying oven at a temperature of 40℃ and a vacuum degree of -0.08MPa for 6 hours to obtain 498g of dried methoxy polyethylene glycol monoamine. 4: 1673g of dried Schiff base-containing diamine and 997g of dried tert-butyl 3,5-diaminobenzoate were added to a reaction vessel and stirred at 200 rpm for 5 min to obtain 2670g of mixed diamine. Then, under nitrogen protection, 13350g of N,N-dimethylacetamide was added to the reaction vessel, and stirring was started. The temperature of the reaction vessel was controlled at -5℃, and under nitrogen bubbling conditions, the mixture was stirred until completely dissolved for 30 min to obtain 16020g of diamine solution. 5: Under nitrogen protection, keep the reactor temperature at -5℃, add 5200g of 4,4'-(hexafluoroisopropene) phthalic anhydride to the diamine solution in 3 batches, with an interval of 20min between each addition. After the addition is completed, continue stirring and reacting at -5℃ for 2h. Then raise the reactor temperature to 20℃ and continue stirring and reacting for 2h to obtain 21220g of polyamic acid solution. 6: Add 498g of dried methoxy polyethylene glycol monoamine and 498g of N,N-dimethylacetamide to the reaction vessel, set the stirrer speed to 200 rpm, and stir for 5 min. After mixing, transfer to a constant pressure dropping funnel, and then add dropwise to the polyamic acid solution over a period of 30 min. After the addition is complete, continue stirring the reaction at 20℃ for 2 h to obtain 22216g of end-capped polyamic acid solution. 7: Place 250g of octaphenyl cage-type silsesquioxane in a vacuum drying oven, set the temperature to 100℃ and the vacuum degree to -0.08MPa, and dry for 6h to obtain 249g of dried octaphenyl cage-type silsesquioxane. Place 150g of nano-silica in a vacuum drying oven, set the temperature to 100℃ and the vacuum degree to -0.08MPa, and dry for 6h to obtain 149g of dried nano-silica. Add 249g of dried octaphenyl cage-type silsesquioxane and 149g of dried nano-silica to 2222g of end-capped polyamic acid solution, and use ultrasonic dispersion treatment with an ultrasonic power of 300W and an ultrasonic time of 20min to form a nano-filler pre-dispersion slurry. Then add the nano-filler pre-dispersion slurry to the remaining 19994g of end-capped polyamic acid solution, and disperse it at 2000rpm for 30min using a high-speed disperser to obtain 22614g of nano-filler dispersion. 8: 350g of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 120g of dicumyl peroxide, 400g of ethoxylated trimethylolpropane triacrylate, 150g of polypropylene glycol diglycidyl ether, 50g of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and 30g of tris(2,4-di-tert-butylphenyl)phosphite were added to the nanofiller dispersion and stirred for 30 min to obtain 23714g of modified polyimide precursor resin solution. The modified polyimide precursor resin solution was transferred to a reactor equipped with a vacuum distillation device, and N,N-dimethylacetamide was removed by vacuum distillation at 40℃ and -0.08MPa for 8 h to obtain 9866g of the modified polyimide precursor resin prepared in Example 1.

[0011] Example 2 1. Place 600g of terephthalaldehyde in a vacuum drying oven, set the temperature to 70℃ and the vacuum degree to -0.10MPa, and dry for 12h to obtain 596g of dried terephthalaldehyde. Place 1200g of 3,3'-diamino-N-methyldipropylamine in a vacuum drying oven, set the temperature to 60℃ and the vacuum degree to -0.10MPa, and dry for 10h to obtain 1194g of dried 3,3'-diamino-N-methyldipropylamine. 2. Under nitrogen protection, add 5960g of anhydrous ethanol to a reactor equipped with a mechanical stirrer, a reflux condenser, and a constant-pressure dropping funnel. Set the stirrer speed to 500rpm. Add 596g of dried terephthalaldehyde to the reactor and stir for 10min. Raise the reactor temperature to 70℃ to bring the components in the reactor to a reflux state. Add 1194g of dried 3,3'-diamino-N-methyldipropylamine to 1194g of anhydrous ethanol and mix at 300rpm for 5min. After mixing, transfer the mixture to a constant-pressure dropping funnel and then add dropwise... In the reaction vessel, the dropwise addition time was 60 min. After the dropwise addition was completed, the reaction was continued under reflux for 5 h. After the reaction was completed, the reaction solution was cooled to room temperature and transferred to a rotary evaporator. The solvent was removed by rotary evaporation at 50 °C and -0.10 MPa to obtain the crude product. The crude product was then recrystallized twice with anhydrous ethanol to obtain the recrystallized product. The amount of anhydrous ethanol used in each recrystallization was 8 times the mass of the crude product. The recrystallized product was placed in a vacuum drying oven at 60 °C and a vacuum of -0.10 MPa for 12 h to obtain 1665 g of Schiff base diamine. 3: 1665g of Schiff base-containing diamine was placed in a vacuum drying oven at 80℃ and a vacuum of -0.10MPa for 12 hours to obtain 1658g of dried Schiff base-containing diamine. 1000g of tert-butyl 3,5-diaminobenzoate was placed in a vacuum drying oven at 70℃ and a vacuum of -0.10MPa for 14 hours to obtain 994g of dried tert-butyl 3,5-diaminobenzoate. 500g of methoxy polyethylene glycol monoamine was placed in a vacuum drying oven at 60℃ and a vacuum of -0.10MPa for 10 hours to obtain 496g of dried methoxy polyethylene glycol monoamine. 4: 1658g of dried Schiff base-containing diamine and 994g of dried tert-butyl 3,5-diaminobenzoate were added to a reaction vessel and stirred at 200 rpm for 5 min to obtain 2652g of mixed diamine. Then, under nitrogen protection, 13260g of N,N-dimethylacetamide was added to the reaction vessel, stirring was started, the temperature of the reaction vessel was controlled at 5℃, and under nitrogen bubbling conditions, stirring was carried out until completely dissolved for 60 min to obtain 15912g of diamine solution. 5: Under nitrogen protection, keep the reactor temperature at 5℃, add 5200g of 4,4'-(hexafluoroisopropene) phthalic anhydride to the diamine solution in 5 batches, with an interval of 30min between each addition. After the addition is completed, continue stirring and reacting at 5℃ for 4h. Then raise the reactor temperature to 30℃ and continue stirring and reacting for 4h to obtain 21112g of polyamic acid solution. 6: Add 496g of dried methoxy polyethylene glycol monoamine and 496g of N,N-dimethylacetamide to the reaction vessel, set the stirrer speed to 200 rpm, and stir for 5 min. After mixing, transfer to a constant pressure dropping funnel, and then add dropwise to the polyamic acid solution over a period of 60 min. After the addition is complete, continue stirring the reaction at 30℃ for 4 h to obtain 22104g of end-capped polyamic acid solution. 7: Place 250g of octaphenyl cage-type silsesquioxane in a vacuum drying oven, set the temperature to 120℃ and the vacuum degree to -0.10MPa, and dry for 10h to obtain 248g of dried octaphenyl cage-type silsesquioxane. Place 150g of nano-silica in a vacuum drying oven, set the temperature to 120℃ and the vacuum degree to -0.10MPa, and dry for 10h to obtain 148g of dried nano-silica. Add 248g of dried octaphenyl cage-type silsesquioxane and 148g of dried nano-silica to 2210g of end-capped polyamic acid solution, and use ultrasonic dispersion treatment with an ultrasonic power of 500W and an ultrasonic time of 40min to form a nano-filler pre-dispersion slurry. Then add the nano-filler pre-dispersion slurry to the remaining 19894g of end-capped polyamic acid solution, and disperse it at 3000rpm for 60min using a high-speed disperser to obtain 22500g of nano-filler dispersion. 8: 350g of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 120g of dicumyl peroxide, 400g of ethoxylated trimethylolpropane triacrylate, 150g of polypropylene glycol diglycidyl ether, 50g of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and 30g of tris(2,4-di-tert-butylphenyl)phosphite were added to the nanofiller dispersion and stirred for 60 min to obtain 23600g of modified polyimide precursor resin solution. The modified polyimide precursor resin solution was transferred to a reactor equipped with a vacuum distillation device, and N,N-dimethylacetamide was removed by vacuum distillation at 50℃ and -0.10MPa for 10 h to obtain 9804g of the modified polyimide precursor resin prepared in Example 2.

[0012] Example 3 1. Add 800g of the modified polyimide precursor resin prepared in Example 1 to 4kg of N,N-dimethylacetamide, stir and dissolve until homogeneous to obtain a coating solution. Place the coating solution in a vacuum degassing machine, set the vacuum degree to -0.09MPa, and the degassing time to 30min. After degassing, uniformly coat the precursor resin onto the surface of the release PET film using a slit extrusion method. The die gap is 150µm, the coating speed is 3m / min, and the wet film thickness is 120µm. After coating, the wet film is placed in a multi-stage hot air oven for pre-imidization gradient drying. The temperature of the first section is 80℃ and the dwell time is 8min; the temperature of the second section is 120℃ and the dwell time is 6min; the temperature of the third section is 150℃ and the dwell time is 4min; the temperature of the fourth section is 200℃ and the dwell time is 3min; and the temperature of the fifth section is 260℃ and the dwell time is 2min. There is a transition zone between each section with a length of 30cm. After drying, the film surface enters the cooling zone and is gradually cooled to 25℃ at a cooling rate of 15℃ / s. Then it is wound up with the winding tension controlled at 15N to obtain a pre-imidized modified polyimide film containing a release film. 2: Place the pre-imidized modified polyimide film containing the release film onto the inspection table. Under an inspection light source with an illuminance of 1200 lx, check the uniformity and surface defects of the film surface. After confirming that there are no bubbles, pinholes, or particulate impurities, cut the pre-imidized film to the size of the target FPC width. After cutting, remove the release PET film and cover the pre-imidized modified polyimide film onto the FPC substrate with the circuit processing completed, with the film side facing the copper circuit side. Use a roll laminator for pre-lamination, setting the roll temperature to 40℃, the roll pressure to 10 N / cm, and the roll speed to 0.5 m / min. After pre-lamination, the component to be pressed is obtained. 3. The components to be pressed are fed into a vacuum press, and the vacuum degree is set to -0.095MPa. A three-stage temperature and pressure process is used for hot pressing. The first stage is set with a pressing temperature of 160℃, a pressing pressure of 0.5MPa, and a holding time of 10min. The second stage is set with a pressing temperature of 230℃, a pressing pressure of 2.5MPa, and a holding time of 25min. The third stage is set with a pressing temperature of 250℃, a pressing pressure of 1.5MPa, and a holding time of 15min. After the three stages are completed, while maintaining a holding pressure of 0.5MPa, the components are gradually cooled to below 50℃ at a cooling rate of 5℃ / min. The pressure is then released and the components are removed to obtain an integrated FPC substrate. 4. Lay the integrated FPC substrate flat on the inspection table and check the surface flatness and interface bonding quality of the cover film under an inspection light source with an illuminance of 1200lx. After confirming that there are no bubbles, delamination and local unbonded defects, send the integrated FPC substrate into the laser processing platform. Use an ultraviolet picosecond laser to perform windowing and shape cutting of the cover film. Set the laser wavelength to 355nm, the pulse width to 10ps, the repetition frequency to 500kHz, the cutting speed to 200mm / s, and the laser focus to the middle plane in the thickness direction of the cover film. After processing, blow the processed surface with 0.3MPa compressed air to remove processing debris and obtain a semi-finished FPC cover film. 5. Add 200g of perfluorodecyltrimethoxysilane to 9kg of anhydrous ethanol and stir at 300rpm for 15min. Then add 800g of deionized water and continue stirring and hydrolyzing for 30min while maintaining the same speed to obtain a fluorine-containing surface modification treatment solution. Send the semi-finished FPC cover film into a plasma treatment device and use low-pressure plasma in an argon atmosphere to perform online cleaning and activation treatment on the surface of the cover film. Set the treatment power to 200W, the argon flow rate to 50sccm, the treatment pressure to 20Pa, and the treatment time to 60s. After the treatment, send the semi-finished FPC cover film flat into an impregnation device and impregnate it with the fluorine-containing surface modification treatment solution for 30s. The liquid content is controlled at 50%. After impregnation, dry and cure it with hot air at 120℃ for 30min to obtain the FPC cover film based on modified polyimide prepared in Example 3.

[0013] Example 4 1. Add 800g of the modified polyimide precursor resin prepared in Example 2 to 4kg of N,N-dimethylacetamide, wherein the mass ratio of the modified polyimide precursor resin to N,N-dimethylacetamide is 1:5. Stir until homogeneous to obtain a coating solution. Place the coating solution in a vacuum degassing machine, set the vacuum degree to -0.10MPa, and the degassing time to 60min. After degassing, uniformly coat the precursor resin onto the surface of the release PET film using a slit extrusion method. The die gap is 250µm, the coating speed is 6m / min, and the wet film thickness is 200µm. After coating, the wet film enters a multi-stage heat treatment process. The pre-imidized gradient drying was performed in an air-drying oven. The temperature of the first stage was 100℃ and the residence time was 12 min; the temperature of the second stage was 140℃ and the residence time was 10 min; the temperature of the third stage was 170℃ and the residence time was 8 min; the temperature of the fourth stage was 220℃ and the residence time was 5 min; and the temperature of the fifth stage was 280℃ and the residence time was 4 min. A transition zone with a length of 50 cm was set between each stage. After drying, the film surface entered the cooling zone and was gradually cooled to 25℃ at a cooling rate of 30℃ / s. Then it was wound up with the winding tension controlled at 25N to obtain a pre-imidized modified polyimide film containing a release film. 2: Place the pre-imidized modified polyimide film containing the release film onto the inspection table. Under an inspection light source with an illuminance of 1200 lx, check the uniformity and surface defects of the film surface. After confirming that there are no bubbles, pinholes, or particulate impurities, cut the pre-imidized film to the size of the target FPC width. After cutting, remove the release PET film and cover the pre-imidized modified polyimide film onto the FPC substrate with the circuit processing completed, with the film side facing the copper circuit side. Use a roll laminator for pre-lamination, setting the roll temperature to 60℃, the roll pressure to 20 N / cm, and the roll speed to 1.5 m / min. After pre-lamination, the component to be pressed is obtained. 3. The components to be pressed are fed into the vacuum press, and the vacuum degree is set to -0.10MPa. A three-stage temperature and pressure process is used for hot pressing. The first stage is set with a pressing temperature of 180℃, a pressing pressure of 1.5MPa, and a holding time of 15min. The second stage is set with a pressing temperature of 250℃, a pressing pressure of 3.5MPa, and a holding time of 35min. The third stage is set with a pressing temperature of 270℃, a pressing pressure of 2.5MPa, and a holding time of 25min. After the three stages are completed, while maintaining a holding pressure of 1MPa, the temperature is gradually cooled to below 50℃ at a cooling rate of 10℃ / min. The pressure is then released and the components are removed to obtain the integrated FPC substrate. 4. Lay the integrated FPC substrate flat on the inspection table and check the surface flatness and interface bonding quality of the cover film under an inspection light source with an illuminance of 1200lx. After confirming that there are no bubbles, delamination and local unbonded defects, send the integrated FPC substrate into the laser processing platform. Use an ultraviolet picosecond laser to perform windowing and shape cutting of the cover film. Set the laser wavelength to 355nm, the pulse width to 15ps, the repetition frequency to 1000kHz, the cutting speed to 500mm / s, and the laser focus to the middle plane in the thickness direction of the cover film. After processing, blow the processed surface with 0.5MPa compressed air to remove processing debris and obtain a semi-finished FPC cover film. 5: Add 200g of perfluorodecyltrimethoxysilane to 9kg of anhydrous ethanol and stir at 300rpm for 15min. Then add 800g of deionized water and continue stirring and hydrolyzing for 30min while maintaining the same speed to obtain a fluorine-containing surface modification treatment solution. Send the semi-finished FPC cover film to a plasma treatment device and use low-pressure plasma in an argon atmosphere to perform online cleaning and activation treatment on the surface of the cover film. Set the treatment power to 400W, the argon flow rate to 100sccm, the treatment pressure to 50Pa, and the treatment time to 120s. After the treatment, send the semi-finished FPC cover film flat into an impregnation device and impregnate it with the fluorine-containing surface modification treatment solution for 60s. The liquid retention rate is controlled at 70%. After impregnation, dry and cure with hot air at 140℃ for 45min to obtain the FPC cover film based on modified polyimide prepared in Example 4.

[0014] Comparative Example 1 The difference between this comparative example and Example 3 is that the modified polyimide precursor resin prepared in Example 1 is replaced with a commercially available ordinary polyimide precursor resin, while the other components and processes remain unchanged. The commercially available common polyimide precursor resin is a polyamic acid solution obtained by condensation of 4,4'-(hexafluoroisopropylene) phthalic anhydride and 4,4'-diaminodiphenyl ether, with a solid content of 18%, a rotational viscosity of 4000 mPa·s at 25°C, and N,N-dimethylacetamide as the solvent. The specific preparation method is as follows: 1. Place 4.8 kg of commercially available ordinary polyimide precursor resin in a vacuum degassing machine, set the vacuum level to -0.09 MPa, and the degassing time to 30 min. After degassing, uniformly coat the precursor resin onto the surface of the release PET film using a slit extrusion method. The die gap is 150 μm, the coating speed is 3 m / min, and the wet film thickness is 120 μm. After coating, the wet film is placed in a multi-stage hot air oven for gradient drying. The first stage temperature is set to 80℃, and the residence time is 8 min. The film is dried in five stages: the second stage is at 120℃ with a dwell time of 6 minutes; the third stage is at 150℃ with a dwell time of 4 minutes; the fourth stage is at 200℃ with a dwell time of 3 minutes; and the fifth stage is at 260℃ with a dwell time of 2 minutes. A transition zone with a length of 30 cm is provided between each stage. After drying, the film surface enters the cooling zone and is gradually cooled to 25℃ at a cooling rate of 15℃ / s. Then, it is wound up with a winding tension controlled at 15N to obtain a polyimide film containing a release film. 2: Place the polyimide film containing the release film onto the inspection table. Under an inspection light source with an illuminance of 1200 lx, check the uniformity and surface defects of the film surface. After confirming that there are no bubbles, pinholes, or particulate impurities, cut the polyimide film to the size of the target FPC width. After cutting, remove the release PET film and cover the polyimide film onto the FPC substrate with the circuit processing completed, with the film side facing the copper circuit side. Use a roll laminator for pre-lamination, setting the roll temperature to 40℃, the roll pressure to 10 N / cm, and the roll speed to 0.5 m / min. After pre-lamination, the component to be pressed is obtained. 3. The components to be pressed are fed into a vacuum press, and the vacuum degree is set to -0.095MPa. A three-stage temperature and pressure process is used for hot pressing. The first stage is set with a pressing temperature of 160℃, a pressing pressure of 0.5MPa, and a holding time of 10min. The second stage is set with a pressing temperature of 230℃, a pressing pressure of 2.5MPa, and a holding time of 25min. The third stage is set with a pressing temperature of 250℃, a pressing pressure of 1.5MPa, and a holding time of 15min. After the three stages are completed, while maintaining a holding pressure of 0.5MPa, the components are gradually cooled to below 50℃ at a cooling rate of 5℃ / min. The pressure is then released and the components are removed to obtain an integrated FPC substrate. 4. Lay the integrated FPC substrate flat on the inspection table and check the surface flatness and interface bonding quality of the cover film under an inspection light source with an illuminance of 1200lx. After confirming that there are no bubbles, delamination and local unbonded defects, send the integrated FPC substrate into the laser processing platform. Use an ultraviolet picosecond laser to perform windowing and shape cutting of the cover film. Set the laser wavelength to 355nm, the pulse width to 10ps, the repetition frequency to 500kHz, the cutting speed to 200mm / s, and the laser focus to the middle plane in the thickness direction of the cover film. After processing, blow the processed surface with 0.3MPa compressed air to remove processing debris and obtain a semi-finished FPC cover film. 5: 200g of perfluorodecyltrimethoxysilane was added to 9kg of anhydrous ethanol and stirred at 300rpm for 15min. Then, 800g of deionized water was added, and the stirring and hydrolysis were continued for 30min while maintaining the same speed to obtain a fluorine-containing surface modification treatment solution. The semi-finished FPC cover film was sent to a plasma treatment device, and the surface of the cover film was cleaned and activated online using low-pressure plasma in an argon atmosphere. The treatment power was set to 200W, the argon flow rate to 50sccm, the treatment pressure to 20Pa, and the treatment time to 60s. After the treatment, the semi-finished FPC cover film was sent to an impregnation device and impregnated with the fluorine-containing surface modification treatment solution for 30s. The liquid content was controlled at 50%. After impregnation, the film was dried and cured with hot air at 120℃ for 30min to obtain the FPC cover film prepared in Comparative Example 1.

[0015] Comparative Example 2 The difference between this comparative example and Example 3 is that the modified polyimide precursor resin used does not contain terephthalaldehyde during the preparation process, that is, it only relies on the thermal deprotection of tert-butyl 3,5-diaminobenzoate to provide the interface anchoring function, without the function of dynamic covalent bond internal stress relief. The specific preparation method is as follows: 1. Place 1800g of 3,3'-diamino-N-methyldipropylamine in a vacuum drying oven, set the temperature to 60℃ and the vacuum degree to -0.08MPa, and dry for 8h to obtain 1795g of dried 3,3'-diamino-N-methyldipropylamine. Place 1000g of tert-butyl 3,5-diaminobenzoate in a vacuum drying oven, set the temperature to 50℃ and the vacuum degree to -0.08MPa, and dry for 10h to obtain 997g of dried tert-butyl 3,5-diaminobenzoate. Place 500g of methoxy polyethylene glycol monoamine in a vacuum drying oven, set the temperature to 40℃ and the vacuum degree to -0.08MPa, and dry for 6h to obtain 498g of dried methoxy polyethylene glycol monoamine. 2: 1795g of dried 3,3'-diamino-N-methyldipropylamine and 997g of dried tert-butyl 3,5-diaminobenzoate were added to a reaction vessel and stirred at 200 rpm for 5 min to obtain 2792g of mixed diamine. Then, under nitrogen protection, 13960g of N,N-dimethylacetamide was added to the reaction vessel, and stirring was started. The temperature of the reaction vessel was controlled at -5℃, and under nitrogen bubbling conditions, the mixture was stirred until completely dissolved for 30 min to obtain a diamine solution. 3: Under nitrogen protection, keep the reactor temperature at -5℃, add 5200g of 4,4'-(hexafluoroisopropene) phthalic anhydride to the diamine solution in 3 batches, with an interval of 20min between each addition. After the addition is completed, continue stirring and reacting at -5℃ for 2h. Then raise the reactor temperature to 20℃ and continue stirring and reacting for 2h to obtain a polyamic acid solution. 4: Add 498g of dried methoxy polyethylene glycol monoamine and 498g of N,N-dimethylacetamide to the reaction vessel, set the stirrer speed to 200 rpm, and stir for 5 min. After mixing, transfer to a constant pressure dropping funnel, and then add dropwise to the polyamic acid solution over a period of 30 min. After the addition is complete, continue stirring and reacting at 20℃ for 2 h to obtain the end-capped polyamic acid solution. 5: Place 250g of octaphenyl cage-type silsesquioxane in a vacuum drying oven, set the temperature to 100℃ and the vacuum degree to -0.08MPa, and dry for 6h to obtain 249g of dried octaphenyl cage-type silsesquioxane. Place 150g of nano-silica in a vacuum drying oven, set the temperature to 100℃ and the vacuum degree to -0.08MPa, and dry for 6h to obtain 149g of dried nano-silica. Add 249g of dried octaphenyl cage-type silsesquioxane and 149g of dried nano-silica to a 10% (w / w) end-capped polyamic acid solution and perform ultrasonic dispersion treatment with an ultrasonic power of 300W and an ultrasonic time of 20min to form a nano-filler pre-dispersion slurry. Then add the nano-filler pre-dispersion slurry to the remaining end-capped polyamic acid solution and disperse it at 2000rpm for 30min using a high-speed disperser to obtain a nano-filler dispersion. 6: 350g of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 120g of dicumyl peroxide, 400g of ethoxylated trimethylolpropane triacrylate, 150g of polypropylene glycol diglycidyl ether, 50g of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and 30g of tris(2,4-di-tert-butylphenyl)phosphite were added to the nanofiller dispersion and stirred for 30 min to obtain a modified polyimide precursor resin solution. The modified polyimide precursor resin solution was transferred to a reactor equipped with a vacuum distillation device, and N,N-dimethylacetamide was removed by vacuum distillation at 40℃ and -0.08MPa for 8 h to obtain the modified polyimide precursor resin prepared in Comparative Example 2. 7: Add 800g of the modified polyimide precursor resin prepared in Comparative Example 2 to 4kg of N,N-dimethylacetamide, stir until homogeneous to obtain a coating solution. Place the coating solution in a vacuum degassing machine, set the vacuum degree to -0.09MPa, and the degassing time to 30min. After degassing, uniformly coat the coating solution onto the surface of the release PET film using a slit extrusion method. The die gap is 150μm, the coating speed is 3m / min, and the wet film thickness is 120μm. After coating, the wet film enters a multi-stage hot air oven for pre-imidization gradient drying. The first stage temperature is set to 80℃, and the residence time is [not specified]. The drying process is as follows: 8 minutes for the first stage, 6 minutes for the second stage at 120℃, 4 minutes for the third stage at 150℃, 3 minutes for the fourth stage at 200℃, and 2 minutes for the fifth stage at 260℃. A transition zone with a length of 30 cm is provided between each stage. After drying, the film surface enters the cooling zone and is gradually cooled to 25℃ at a cooling rate of 15℃ / s. Then, it is wound up with the winding tension controlled at 15N to obtain a pre-imidized modified polyimide film containing a release film. 8: Place the pre-imidized modified polyimide film containing the release film onto the inspection table. Under an inspection light source with an illuminance of 1200 lx, check the uniformity and surface defects of the film surface. After confirming that there are no bubbles, pinholes, or particulate impurities, cut the pre-imidized film to the size of the target FPC width. After cutting, remove the release PET film and cover the pre-imidized modified polyimide film onto the FPC substrate with the circuit processing completed, with the film side facing the copper circuit side. Use a roll laminator for pre-lamination, setting the roll temperature to 40℃, the roll pressure to 10 N / cm, and the roll speed to 0.5 m / min. After pre-lamination, the component to be pressed is obtained. 9. The components to be pressed are fed into the vacuum press, and the vacuum degree is set to -0.095MPa. A three-stage temperature and pressure process is used for hot pressing. The first stage is set with a pressing temperature of 160℃, a pressing pressure of 0.5MPa, and a holding time of 10min. The second stage is set with a pressing temperature of 230℃, a pressing pressure of 2.5MPa, and a holding time of 25min. The third stage is set with a pressing temperature of 250℃, a pressing pressure of 1.5MPa, and a holding time of 15min. After the three stages are completed, while maintaining a holding pressure of 0.5MPa, the components are gradually cooled to below 50℃ at a cooling rate of 5℃ / min. The pressure is then released and the components are removed to obtain the integrated FPC substrate. 10: Lay the integrated FPC substrate flat on the inspection table and check the surface flatness and interface bonding quality of the cover film under an inspection light source with an illuminance of 1200lx. After confirming that there are no bubbles, delamination and local unbonded defects, send the integrated FPC substrate into the laser processing platform. Use an ultraviolet picosecond laser to perform windowing and shape cutting processing on the cover film. Set the laser wavelength to 355nm, the pulse width to 10ps, the repetition frequency to 500kHz, the cutting speed to 200mm / s, and the laser focus to the middle plane in the thickness direction of the cover film. After processing, blow the processed surface with compressed air of 0.3MPa to remove processing debris and obtain a semi-finished FPC cover film. 11: 200g of perfluorodecyltrimethoxysilane was added to 9kg of anhydrous ethanol and stirred at 300rpm for 15min. Then, 800g of deionized water was added, and the stirring and hydrolysis were continued for 30min while maintaining the same speed to obtain a fluorine-containing surface modification treatment solution. The semi-finished FPC cover film was sent to a plasma treatment device, and the surface of the cover film was cleaned and activated online using low-pressure plasma in an argon atmosphere. The treatment power was set to 200W, the argon flow rate to 50sccm, the treatment pressure to 20Pa, and the treatment time to 60s. After the treatment, the semi-finished FPC cover film was sent to an impregnation device and impregnated with the fluorine-containing surface modification treatment solution for 30s. The liquid content was controlled at 50%. After impregnation, the film was dried and cured with hot air at 120℃ for 30min to obtain the FPC cover film prepared in Comparative Example 2.

[0016] Peel strength test Samples with dimensions of 100 mm × 25 mm were cut from the FPC cover films prepared in Examples 3, 4, Comparative Example 1, and Comparative Example 2. After being placed under standard conditions for 24 hours, the peel strength between the cover film and the copper surface was tested according to IPC-TM-650 2.4.9 "Peel Strength, Flexible Printed Wiring Materials". The test angle was 90° and the peel speed was 50 mm / min. Each group of samples was tested in parallel 3 times, and the average value was taken. The test results were recorded. Table 1. Peel strength test results As shown in Table 1, the peel strengths of Examples 3 and 4 reached 12.5 N / cm and 14.2 N / cm, respectively, while the peel strength of Comparative Example 1 was only 3.8 N / cm, a decrease of 69.6% compared to Example 3. The reason for this is that Comparative Example 1 used commercially available ordinary polyimide precursor resin, which did not contain tert-butyl 3,5-diaminobenzoate. Therefore, it could not remove the in-situ free carboxyl groups generated by the thermal desorption of the tert-butyl ester protective group during the hot pressing process to form a chemical bond anchoring with the copper surface. The coating film and the copper surface relied only on physical adsorption, and the interfacial bonding force was significantly insufficient. This verifies the key role of the thermally induced deprotection interfacial anchoring mechanism in achieving high peel strength without adhesives. The peel strength of Comparative Example 2 was 11.8 N / cm, which is close to 12.5 N / cm of Example 3. The reason for this is that although Comparative Example 2 does not contain dynamic covalent bonds, it retains the thermally induced deprotection interface anchoring function of tert-butyl 3,5-diaminobenzoate. This indicates that interface anchoring is the dominant contributing factor to peel strength, while dynamic covalent bonds mainly play a role in stress relief within the matrix rather than interface bonding.

[0017] Dielectric performance testing The FPC cover films prepared in Examples 3, 4, Comparative Example 1, and Comparative Example 2 were cut into 50mm × 50mm samples. After being placed under standard conditions for 24 hours, the dielectric constant and dielectric loss tangent at 10GHz were tested according to ASTM D150-18 "Standard Test Methods for AC Loss Characteristics and Permittivity of Solid Electrical Insulation". Each group of samples was tested in parallel three times, and the average value was taken and the test results were recorded. Table 2, Dielectric property test results Analysis of Table 2 shows that the dielectric constants of Examples 3 and 4 are 2.72 and 2.65, respectively, and the dielectric loss tangents are 0.0042 and 0.0038, respectively. The dielectric constant of Comparative Example 1 is 3.15, and the dielectric loss tangent is 0.0085, which are 15.8% and 102.4% higher than those of Example 3, respectively. The reason for this is that Comparative Example 1 uses commercially available ordinary polyimide precursor resin, which does not contain low dielectric fillers such as octaphenyl cage-type silsesquioxane and nano silica, and does not have a low dielectric surface layer formed by fluorine-containing surface modification treatment. At the same time, the commercially available polyimide molecular chain does not contain -CF3 groups, and has a high polarizability. This verifies the synergistic effect of fluorine-containing dianhydride, POSS / nano silica filler and fluorine-containing surface modification in reducing dielectric constant and dielectric loss. The dielectric constant and dielectric loss tangent of Example 4 were reduced by 2.6% and 9.5% respectively compared with Example 3. The reason for this is that Example 4 used the maximum value of process parameters, with a higher pre-imidization gradient drying temperature and a longer time, which allowed for more complete migration and enrichment of nano-silica to the upper surface of the film, resulting in a more perfect low-dielectric-ionized interface. The dielectric constant and dielectric loss tangent of Comparative Example 2 are basically the same as those of Example 3, indicating that the presence or absence of dynamic covalent bonds has no significant effect on dielectric properties.

[0018] Internal stress relief effect test Samples with dimensions of 100mm × 100mm were cut from the integrated FPC substrates prepared in Examples 3, 4, Comparative Example 1, and Comparative Example 2. After being placed under standard conditions for 24 hours, the warpage height after hot-pressing the cover film was measured. The samples were then placed in a constant temperature and humidity chamber with a temperature of 85℃ and a relative humidity of 85% for 168 hours of aging treatment. After being removed, the samples were allowed to recover under standard conditions for 2 hours, and the warpage height was measured again. The rate of change of warpage height before and after aging was calculated. Each group of samples was tested in parallel three times, and the average value was taken and the test results were recorded. Table 3. Test results of internal stress relief effect Analysis of Table 3 shows that the warpage heights before aging in Examples 3 and 4 were only 0.8 mm and 0.5 mm, respectively, while the warpage heights before aging in Comparative Examples 1 and 2 reached 3.2 mm and 2.1 mm, respectively. The reason for this is that the precursor resins in Examples 3 and 4 contain Schiff base dynamic covalent bonds formed by the condensation of terephthalaldehyde and 3,3'-diamino-N-methyldipropylamine. During the 250°C holding stage of the third stage of hot pressing in S3, the Schiff base bonds undergo a reversible exchange reaction, causing the polyimide molecular chain segments to undergo topological rearrangement under stress, effectively relaxing the interfacial thermal stress caused by the difference in thermal expansion coefficients during hot pressing. However, Comparative Examples 1 and 2 did not have this mechanism, and the thermal stress was released in the form of warpage. Comparative Example 1 showed the greatest warping height before aging. The reason for this was that Comparative Example 1 not only lacked a dynamic covalent bond stress relief mechanism, but also used a commercially available ordinary polyimide precursor resin, which had a greater difference in thermal expansion coefficient with the copper surface than the modified system, resulting in more severe thermal stress accumulation. The warpage height change rate of Comparative Example 2 after aging was as high as 114.3%, while that of Example 3 was only 37.5%. The reason for this is that although Comparative Example 2 retained the interface anchoring function, it lacked Schiff base dynamic covalent bonds. It could not continuously dissipate the additional stress caused by the humid and hot environment through the dynamic exchange of molecular chain segments during the aging process. The stress continued to accumulate, leading to increased warpage. In contrast, the Schiff base bonds in Example 3 could still be exchanged to a limited extent during the high temperature and high humidity aging process, gradually releasing the accumulated stress. This verified the key role of dynamic covalent bonds in eliminating internal stress in long-term reliability. The warpage height before aging in Example 4 was only 0.5 mm, which was lower than the 0.8 mm in Example 3. The reason for this is that Example 4 used the maximum value of the process parameters, with the hot pressing temperature of the third stage of S3 being 270°C and the holding time being 25 min. This resulted in a more complete exchange reaction of the Schiff base dynamic covalent bonds and a more thorough stress relaxation effect.

[0019] Surface hydrophobicity test Samples with a size of 50 mm × 50 mm were cut from the FPC cover films prepared in Examples 3, 4, Comparative Example 1 and Comparative Example 2. After being placed under standard conditions for 24 h, the water contact angle was tested according to GB / T 30447-2013 "Method for Measurement of Contact Angle of Nanofilms". Each group of samples was tested in parallel 3 times, and the average value was taken and the test results were recorded. Table 4. Surface hydrophobicity test results Analysis of Table 4 shows that the water contact angles of Examples 3 and 4 reached 115° and 118°, respectively, while the water contact angle of Comparative Example 1 was only 78°. The reason for this is that Examples 3 and 4 were impregnated with perfluorodecyltrimethoxysilane hydrolysate. The fluorinated silane underwent a hydrolysis and condensation reaction on the surface of the plasma-activated cover film, and the -CF3 groups were arranged in an orderly manner on the film surface to form a low surface energy monolayer, which endowed the cover film with excellent hydrophobic properties. Although Comparative Example 1 was also treated with fluorinated surface modification, the surface of the commercially available ordinary polyimide film lacked the micro-nano rough structure formed by the migration and enrichment of nano silica, which was not conducive to the construction of a hydrophobic surface. This verifies the synergistic enhancement effect of the release interface formed by the migration and enrichment of nano silica on the film surface during the pre-imidization gradient drying process on the fluorinated surface modification.

[0020] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of this invention is defined by the appended claims and their equivalents.

Claims

1. A processing technology for an FPC cover film based on modified polyimide, characterized in that, Based on modified polyimide precursor resin and release PET film, and with modified polyimide precursor resin as the sole functional medium, through the synergistic effect of slit extrusion coating, pre-imidization gradient drying, three-stage programmed temperature hot pressing and fluorine-containing surface modification, an integrated system of adhesive-free interface anchoring, self-elimination of bulk stress and in-situ generation of low dielectric surface is achieved, resulting in an FPC cover film based on modified polyimide.

2. The processing technology for an FPC cover film based on modified polyimide according to claim 1, characterized in that, The modified polyimide precursor resin is composed of the following components by weight percentage: 52% 4,4'-(hexafluoroisopropene)phthalic anhydride, 12% 3,3'-diamino-N-methyldipropylamine, 6% terephthalaldehyde, 10% tert-butyl 3,5-diaminobenzoate, 5% methoxy polyethylene glycol monoamine, 3.5% phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 1.2% dicumyl peroxide, 4% ethoxylated trimethylolpropane triacrylate, 1.5% polypropylene glycol diglycidyl ether, 2.5% octaphenyl cage-like silsesquioxane, 1.5% nano silica, 0.5% pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and 0.3% tris(2,4-di-tert-butylphenyl) phosphite.

3. The processing technology for an FPC cover film based on modified polyimide according to claim 1, characterized in that, The preparation method of the modified polyimide precursor resin includes the following steps: A1: Place terephthalaldehyde in a vacuum drying oven, set the temperature to 50-70℃, and the vacuum degree to -0.08 to -0.10 MPa, and dry for 8-12 hours to obtain dried terephthalaldehyde. Place 3,3'-diamino-N-methyldipropylamine in a vacuum drying oven, set the temperature to 40-60℃, and the vacuum degree to -0.08 to -0.10 MPa, and dry for 6-10 hours to obtain dried 3,3'-diamino-N-methyldipropylamine. A2: Under nitrogen protection, add anhydrous ethanol to a reactor equipped with a mechanical stirrer, a reflux condenser, and a constant-pressure dropping funnel. The mass ratio of anhydrous ethanol to terephthalaldehyde is 10:

1. Set the stirrer speed to 400-500 rpm. Add the dried terephthalaldehyde to the reactor and stir for 5-10 minutes. Raise the reactor temperature to 60-70°C to bring the components in the reactor to a reflux state. Add the dried 3,3'-diamino-N-methyldipropylamine to the anhydrous ethanol and mix at 300 rpm for 5 minutes. The mass ratio of dried 3,3'-diamino-N-methyldipropylamine to anhydrous ethanol is 1:

1. After mixing, transfer to a constant-pressure reactor. The solution was added dropwise to a dropping funnel, followed by a solution of terephthalaldehyde over a period of 40-60 minutes. After the addition was complete, the reaction was continued under reflux for 3-5 hours. After the reaction was complete, the reaction solution was cooled to room temperature and transferred to a rotary evaporator. The solvent was removed by rotary evaporation at 40-50°C and -0.08 to -0.10 MPa to obtain a crude product. The crude product was then recrystallized twice with anhydrous ethanol to obtain a recrystallized product. The amount of anhydrous ethanol used in each recrystallization was 8 times the mass of the crude product. The recrystallized product was placed in a vacuum drying oven at a temperature of 50-60°C and a vacuum of -0.08 to -0.10 MPa for 8-12 hours to obtain a Schiff base-containing diamine. A3: Place the Schiff base-containing diamine in a vacuum drying oven, set the temperature to 60-80℃, and the vacuum degree to -0.08 to -0.10 MPa, and dry for 8-12 hours to obtain dried Schiff base-containing diamine. Place tert-butyl 3,5-diaminobenzoate in a vacuum drying oven, set the temperature to 50-70℃, and the vacuum degree to -0.08 to -0.10 MPa, and dry for 10-14 hours to obtain dried tert-butyl 3,5-diaminobenzoate. Place methoxy polyethylene glycol monoamine in a vacuum drying oven, set the temperature to 40-60℃, and the vacuum degree to -0.08 to -0.10 MPa, and dry for 6-10 hours to obtain dried methoxy polyethylene glycol monoamine. A4: Add dried Schiff base-containing diamine and dried tert-butyl 3,5-diaminobenzoate into a reaction vessel and stir at 200 rpm for 5 min to obtain a mixed diamine. Then, under nitrogen protection, add N,N-dimethylacetamide to the reaction vessel, wherein the mass ratio of N,N-dimethylacetamide to the mixed diamine is 5:

1. Start stirring and control the temperature of the reaction vessel at -5 to 5℃. Stir under nitrogen bubbling conditions until completely dissolved for 30-60 min to obtain a diamine solution. A5: Under nitrogen protection, maintain the reactor temperature at -5 to 5℃, add 4,4'-(hexafluoroisopropene)diphthalic anhydride to the diamine solution in 3-5 batches, with an interval of 20-30 minutes between each addition. After the addition is completed, continue stirring and reacting at -5 to 5℃ for 2-4 hours. Then raise the reactor temperature to 20-30℃ and continue stirring and reacting for 2-4 hours to obtain a polyamic acid solution. A6: Add dried methoxy polyethylene glycol monoamine and N,N-dimethylacetamide to a reaction vessel, set the stirrer speed to 200 rpm, and stir for 5 min. The mass ratio of dried methoxy polyethylene glycol monoamine to N,N-dimethylacetamide is 1:

1. After mixing, transfer to a constant pressure dropping funnel, and then add dropwise to a polyamic acid solution. The dropwise addition time is 30-60 min. After the dropwise addition is completed, continue stirring the reaction at 20-30℃ for 2-4 h to obtain a capped polyamic acid solution. A7: Place octaphenyl cage-type silsesquioxane in a vacuum drying oven, set the temperature to 100-120℃, and the vacuum degree to -0.08 to -0.10MPa, and dry for 6-10 hours to obtain dried octaphenyl cage-type silsesquioxane. Place nano-silica in a vacuum drying oven, set the temperature to 100-120℃, and the vacuum degree to -0.08 to -0.10MPa, and dry for 6-10 hours to obtain dried nano-silica. Add the dried octaphenyl cage-type silsesquioxane and dried nano-silica to a 10wt% end-capped polyamic acid solution, and use ultrasonic dispersion treatment with an ultrasonic power of 300-500W and an ultrasonic time of 20-40min to form a nano-filler pre-dispersion slurry. Then add the nano-filler pre-dispersion slurry to the remaining end-capped polyamic acid solution, and disperse it using a high-speed disperser at 2000-3000rpm for 30-60min to obtain a nano-filler dispersion. A8: Phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, dicumyl peroxide, ethoxylated trimethylolpropane triacrylate, polypropylene glycol diglycidyl ether, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and tris(2,4-di-tert-butylphenyl)phosphite were added to the nanofiller dispersion and stirred for 30-60 min to obtain a modified polyimide precursor resin solution. The modified polyimide precursor resin solution was transferred to a reactor equipped with a vacuum distillation device, and N,N-dimethylacetamide was removed by vacuum distillation at 40-50℃ and -0.08 to -0.10 MPa for 8-10 h to obtain the modified polyimide precursor resin.

4. The processing technology for an FPC cover film based on modified polyimide according to claim 1, characterized in that, Includes the following steps: S1: Add the modified polyimide precursor resin to N,N-dimethylacetamide, wherein the mass ratio of the modified polyimide precursor resin to N,N-dimethylacetamide is 1:

5. Stir until homogeneous to obtain a coating solution. Place the coating solution in a vacuum degassing machine, set the vacuum degree to -0.09 to -0.10 MPa, and the degassing time to 30-60 min. After degassing, uniformly coat the precursor resin onto the surface of the release PET film using a slit extrusion method. The die gap is 150-250 μm, the coating speed is 3-6 m / min, and the wet film thickness is 120-200 μm. After coating, the wet film enters a multi-stage hot air oven for pre-imidization gradient drying. The first stage has a temperature of 80-100℃ and a dwell time of 8-12 min; the second stage has a temperature of 120-140℃ and a dwell time of 6-10 min; the third stage has a temperature of 150-170℃ and a dwell time of 4-8 min; the fourth stage has a temperature of 200-220℃ and a dwell time of 3-5 min; and the fifth stage has a temperature of 260-280℃ and a dwell time of 2-4 min. There is a transition zone between each stage, with a length of 30-50 cm. After drying, the film surface enters the cooling zone and is gradually cooled to 25℃ at a cooling rate of 15-30℃ / s. Then it is wound up, and the winding tension is controlled at 15-25N to obtain a pre-imidized modified polyimide film containing a release film. S2: The pre-imidized modified polyimide film containing the release film is placed flat on the inspection table. Under an inspection light source with an illuminance of 1200lx, the uniformity and surface defects of the film surface are checked. After confirming that there are no defects such as bubbles, pinholes and particulate impurities, the pre-imidized film is cut to the size of the target FPC width. After cutting, the release PET film is removed, and the pre-imidized modified polyimide film is covered on the FPC substrate with the circuit processing completed, with the film side facing the copper circuit side. Pre-lamination is performed using a roll laminator. The roll lamination temperature is set to 40-60℃, the roll lamination line pressure is 10-20N / cm, and the roll lamination speed is 0.5-1.5m / min. After pre-lamination, the component to be pressed is obtained. S3: The component to be pressed is fed into the vacuum press, and the vacuum degree is set to -0.095 to -0.10 MPa. A three-stage temperature and pressure process is used for hot pressing. The first stage is set with a pressing temperature of 160-180℃, a pressing pressure of 0.5-1.5 MPa, and a holding time of 10-15 min. The second stage is set with a pressing temperature of 230-250℃, a pressing pressure of 2.5-3.5 MPa, and a holding time of 25-35 min. The third stage is set with a pressing temperature of 250-270℃, a pressing pressure of 1.5-2.5 MPa, and a holding time of 15-25 min. After the three stages are completed, while maintaining a holding pressure of 0.5-1 MPa, the component is gradually cooled to below 50℃ at a cooling rate of 5-10℃ / min. The pressure is then released and the component is removed to obtain the integrated FPC substrate. S4: Lay the integrated FPC substrate flat on the inspection table and check the surface flatness and interface bonding quality of the cover film under an inspection light source with an illuminance of 1200lx. After confirming that there are no bubbles, delamination and local unbonded defects, send the integrated FPC substrate into the laser processing platform. Use an ultraviolet picosecond laser to perform windowing and shape cutting processing on the cover film. Set the laser wavelength to 355nm, the pulse width to 10-15ps, the repetition frequency to 500-1000kHz, the cutting speed to 200-500mm / s, and the laser focus to the middle plane in the thickness direction of the cover film. After processing, blow the processed surface with compressed air of 0.3-0.5MPa to remove processing debris and obtain a semi-finished FPC cover film. S5: Perfluorodecyltrimethoxysilane was added to anhydrous ethanol and stirred at 300 rpm for 15 min. Then, deionized water was added, and the stirring and hydrolysis were continued for 30 min while maintaining the same speed to obtain a fluorinated surface modification treatment solution. The mass ratio of perfluorodecyltrimethoxysilane, anhydrous ethanol and deionized water was 2:90:

8. The semi-finished FPC cover film was sent to a plasma treatment device, and the surface of the cover film was cleaned and activated online using low-pressure plasma in an argon atmosphere. The treatment power was set to 200-400W, the argon flow rate was 50-100sccm, the treatment pressure was 20-50Pa, and the treatment time was 60-120s. After the treatment, the semi-finished FPC cover film was sent to an impregnation device and impregnated with the fluorinated surface modification treatment solution for 30-60s. The liquid retention rate was controlled at 50-70%. After impregnation, the film was dried and cured with hot air at 120-140℃ for 30-45 min to obtain an FPC cover film based on modified polyimide.

5. The processing technology for an FPC cover film based on modified polyimide according to claim 2, characterized in that, The ethoxylated trimethylolpropane triacrylate has a degree of ethoxylation of 3 and a molecular weight of 600 g / mol.

6. The processing technology for an FPC cover film based on modified polyimide according to claim 2, characterized in that, The molecular weight of the polypropylene glycol diglycidyl ether is 500 g / mol.

7. The processing technology for an FPC cover film based on modified polyimide according to claim 2, characterized in that, The molecular weight of the methoxy polyethylene glycol monoamine is 1000 g / mol.

8. The processing technology for an FPC cover film based on modified polyimide according to claim 2, characterized in that, The average particle size of the octaphenyl cage-type silsesquioxane is 3 μm.

9. The processing technology for an FPC cover film based on modified polyimide according to claim 2, characterized in that, The average particle size of the nano-silica is 20 nm, and the specific surface area is 200 m 2 / g.