A method for forming UAV wingtip fairings based on the thermal expansion of a silicone rubber male mold

By using a silicone rubber male mold to lay carbon fiber prepreg and a female mold to lock and fix the mold in an oven for heating and curing, the problems of strong equipment dependence, long cycle and high cost in the molding of UAV wingtip fairings have been solved, and low-cost and high-efficiency molding of complex structural parts has been achieved.

CN123104102APending Publication Date: 2026-11-17BEIJING COMPOSITE MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610964966.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for forming wingtip fairings for drones suffer from problems such as strong equipment dependence, long production cycles, high costs, and high process complexity, which limit the production capacity and efficiency of small and medium-sized enterprises.

Method used

A process that uses a silicone rubber male mold to lay carbon fiber prepreg, combined with a female mold for locking and a heating oven for curing, replaces the traditional autoclave equipment. By applying molding pressure through the expansion characteristics of silicone rubber, the process achieves efficient molding of complex structural parts.

Benefits of technology

It eliminates the need for autoclave equipment, significantly reducing fixed asset investment and operating costs, substantially shortening the production cycle, improving production efficiency, adapting to the mass production needs of different drone models, and ensuring high performance and dimensional accuracy of the products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104102A_ABST
    Figure CN123104102A_ABST
Patent Text Reader

Abstract

This invention discloses a method for molding a drone wingtip fairing based on the thermal expansion of a silicone rubber male mold. The molding method includes: first, designing a female mold and a silicone rubber male mold based on a three-dimensional digital model of the drone wingtip fairing; then, using high-performance carbon fiber / epoxy resin prepreg as raw material, uniformly laying the carbon fiber / epoxy resin prepreg on the surface of the silicone rubber male mold to form a preform; finally, locking the male mold with the female mold and performing heat curing to obtain the drone wingtip fairing. This invention achieves efficient molding of large-size complex structural parts without the need for autoclave equipment by using a silicone rubber male mold to lay carbon fiber prepreg, combined with female mold locking and oven heating curing processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of aerospace composite material manufacturing technology, specifically to a low-cost, high-efficiency molding method for a complex structure UAV wingtip fairing based on the thermal expansion of a silicone rubber male mold. Background Technology

[0002] Currently, UAV wingtip fairings are typically manufactured using traditional autoclave molding processes due to their complex structures (curved shapes, multi-layered composite structures, etc.). This process requires placing molds and pre-made materials in an autoclave for curing under high temperature and pressure. However, traditional processes have the following problems: (1) High equipment dependence: Autoclave equipment is expensive and bulky, and has strict requirements for production conditions, limiting the production capacity of small and medium-sized enterprises. (2) Long production cycle: Autoclaves require a long heating and cooling process, resulting in low overall production efficiency. (3) High cost: The investment and maintenance costs of autoclave equipment are high, and energy consumption is large, increasing production costs. (4) High process complexity: For complex wingtip fairings, traditional processes present significant technical challenges in mold design, material placement, and pressure control. In order to reduce production costs, improve production efficiency, and meet the UAV market's demand for wingtip fairings, it is urgent to develop a method for molding complex structural components without the need for autoclave equipment. Summary of the Invention

[0003] Based on the problems existing in the above-mentioned background technology, the present invention provides a method for forming a drone wingtip fairing based on laying carbon fiber prepreg with a silicone rubber male mold, combined with mold closing and locking of a female mold and oven heating and curing. This method achieves efficient forming of large-size complex structural parts without the need for autoclave equipment by using a silicone rubber male mold to lay carbon fiber prepreg, combined with mold closing and locking of a female mold and oven heating and curing process.

[0004] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: A method for molding a drone wingtip fairing based on the thermal expansion of a silicone rubber male mold is disclosed. The drone wingtip fairing has a streamlined, thin-walled structure and is constructed using a carbon fiber composite laminate. It is formed by laying a silicone rubber core mold and molding with a female mold. The specific molding method is as follows: (1) Mold design and preparation: Based on the three-dimensional digital model of the UAV wingtip fairing, the female mold is made of Q235B carbon structural steel. The inner surface of the female mold matches the shape of the outer aerodynamic surface of the fairing. Positioning pins are set on the edge of the mold cavity for precise alignment between the female mold and the male mold. The male mold (core mold) is designed and made of 635T silicone rubber material. Its outer surface shape matches the inner surface of the fairing, which can meet the requirements of the complex structure of the wingtip fairing. The female mold is designed to work with the male mold to form a complete molding cavity. The weight ratio of component A to component B in the 635T silicone rubber material is 100:1.5~2, wherein component A is addition-cure silicone rubber 635T and component B is a curing agent; (2) Material preparation: High-performance carbon fiber / epoxy resin prepreg is selected as raw material. The carbon fiber / epoxy resin prepreg uses T700 grade unidirectional tape prepreg and T300 grade fabric prepreg to ensure the lightweight and high strength performance of the product. (3) Material laying and mold assembly: Carbon fiber / epoxy resin prepreg is evenly laid on the surface of the silicone rubber male mold to form a preform; the silicone rubber male mold (core mold) after laying is placed into the rigid female mold and precisely aligned by positioning pins; the female mold is closed and locked, and the average gap of the mold gap is required to be <0.2mm to ensure the sealing of the molding cavity; The number of carbon fiber / epoxy resin prepreg layers is designed according to the thickness of the UAV wingtip fairing. Specifically, the layup design is as follows: if all layers use T300 grade fabric prepreg, the layup direction alternates between 0 / 90° and ±45°; if the first and last layers use T300 grade fabric prepreg, and the middle layers use T700 unidirectional tape prepreg, the layup direction alternates between 0°, 90°, and ±45°, with layup direction deviation requirements of ±3° for unidirectional tape and ±5° for fabric. Both layup designs can meet the mechanical requirements of the fairing. For fairings with high radial strength requirements, T300 grade fabric prepreg and T700 unidirectional tape prepreg are used for layup. This layup design makes the fairing appearance smoother and more aesthetically pleasing, and better fits the product. (4) Curing process: The assembled mold is placed in an oven for heating and curing. The silicone rubber positive mold expands after being heated, applying uniform pressure to the carbon fiber prepreg, replacing the high-pressure gas or mechanical pressure source in the traditional autoclave. After curing, the wingtip fairing of the UAV is obtained when the temperature is ≤60℃.

[0005] Further, the curing procedure in step (4) is as follows: First, heat the material to 130~140℃ at a rate of 0.5~1.5℃ / min, and then keep it at that temperature for 140~160min. During this stage, the silicone rubber expands due to heat, and molding pressure is applied to the prepreg. Then, cool the material to ≤60℃ at a cooling rate of ≤2±1℃ / min, remove the mold, and the curing is complete.

[0006] Compared with the prior art, the present invention has the following beneficial effects: (1) No autoclave equipment required: The present invention uses the expansion characteristics of silicone rubber male mold to apply molding pressure, avoiding dependence on expensive autoclave equipment and greatly reducing fixed asset investment and operating costs.

[0007] (2) High production efficiency: The oven curing time is short and the heating and cooling process is fast, which significantly shortens the overall production cycle, improves mold utilization and product production efficiency, and is suitable for the mass production demand of thousands of drones per year.

[0008] (3) Strong adaptability: The method of the present invention is applicable to the molding of complex shaped structural parts, while ensuring the high performance of the product. The mold modification cost is low and the cycle is short. Moreover, the mold design is flexible and can meet the needs of different models of UAV wingtip fairings.

[0009] (4) Excellent product quality: The high performance (lightweight, high strength) and dimensional accuracy of the product are ensured by the laying of carbon fiber prepreg and the pressure application of silicone rubber positive mold. Attached Figure Description

[0010] Figure 1 This is a schematic diagram of the silicone rubber male mold structure described in this invention.

[0011] Figure 2 This is a simplified diagram showing the disassembled structure of the female mold described in this invention.

[0012] Figure 3 This is a schematic diagram of the cross-section of the female mold structure described in this invention.

[0013] The following are labeled in the diagram: 1. Cover plate, 2. Left mold template, 3. Right mold template, 4. Locking screw hole, 5. Positioning pin, 6. Demolding groove, 7. Positioning boss. Detailed Implementation

[0014] The present invention will be further described below with reference to specific embodiments and accompanying drawings.

[0015] The molding die of this invention includes a silicone rubber mold and a female mold. The female mold structure includes 1 cover plate, 2 left mold template, 3 right mold template, 4 locking screw hole, 5 positioning pin, 6 demolding groove, and 7 positioning boss.

[0016] Example 1 The UAV wingtip fairing molding method based on the thermal expansion of a silicone rubber male mold described in Example 1 involves a streamlined, thin-walled structure made of carbon fiber composite laminate, formed by silicone rubber core mold application and female mold molding. The specific molding method is as follows: (1) Mold design and preparation: Based on the three-dimensional digital model of the UAV wingtip fairing, the female mold is made of Q235B carbon structural steel. The inner surface of the female mold matches the shape of the outer aerodynamic surface of the fairing. Positioning pins are set on the edge of the mold cavity for precise alignment between the female mold and the male mold. The male mold (core mold) is designed and made of 635T silicone rubber material. Its outer surface shape matches the inner surface of the fairing, which can meet the requirements of the complex structure of the wingtip fairing. The female mold is designed to work with the male mold to form a complete molding cavity. The weight ratio of component A to component B in the 635T silicone rubber material is 100:1.75, wherein component A is addition-cure silicone rubber 635T and component B is a curing agent. (2) Material preparation: High-performance carbon fiber / epoxy resin prepreg is selected as raw material. The carbon fiber / epoxy resin prepreg uses T300 grade fabric prepreg to ensure the lightweight and high strength performance of the product. (3) Material laying and mold assembly: Carbon fiber / epoxy resin prepreg is evenly laid on the surface of the silicone rubber male mold to form a preform; the silicone rubber male mold (core mold) after laying is placed into the rigid female mold and precisely aligned by positioning pins; the female mold is closed and locked, and the average gap of the mold joint is required to be <0.2mm to ensure the sealing of the molding cavity; the prepreg layer design is shown in Table 1; Table 1. Layer design for Example 1 Note: The total number of layers is 14, the thickness of a single T300 layer is 0.218mm, and the product wall thickness is 3mm.

[0017] (4) Curing process: The assembled mold is placed in an oven for heating and curing. The silicone rubber positive mold expands after being heated, applying uniform pressure to the carbon fiber prepreg, replacing the high-pressure gas or mechanical pressure source in the traditional autoclave. After curing, the wingtip fairing of the UAV is obtained when the temperature is ≤60℃. Step (4) Curing procedure: First, heat up to 135℃ at a rate of 1℃ / min, then keep warm for 150min. During this stage, the silicone rubber expands due to heat, applying molding pressure to the prepreg. Cool down to ≤60℃ at a cooling rate of 2℃ / min, remove the mold, and the curing is complete.

[0018] Example 2 The UAV wingtip fairing molding method based on the thermal expansion of a silicone rubber male mold described in Example 2 involves a streamlined, thin-walled structure made of carbon fiber composite laminate, formed by silicone rubber core mold application and female mold molding. The specific molding method is as follows: (1) Mold design and preparation: Based on the three-dimensional digital model of the UAV wingtip fairing, the female mold is made of Q235B carbon structural steel. The inner surface of the female mold matches the shape of the outer aerodynamic surface of the fairing. Positioning pins are set on the edge of the mold cavity for precise alignment between the female mold and the male mold. The male mold (core mold) is designed and made of 635T silicone rubber material. Its outer surface shape matches the inner surface of the fairing, which can meet the requirements of the complex structure of the wingtip fairing. The female mold is designed to work with the male mold to form a complete molding cavity. The weight ratio of component A to component B in the 635T silicone rubber material is 100:1.75, wherein component A is addition-cure silicone rubber 635T and component B is a curing agent. (2) Material preparation: High-performance carbon fiber / epoxy resin prepreg is selected as raw material. The carbon fiber / epoxy resin prepreg uses T700 grade unidirectional tape prepreg and T300 grade fabric prepreg to ensure the lightweight and high strength performance of the product. (3) Material laying and mold assembly: Carbon fiber / epoxy resin prepreg is evenly laid on the surface of the silicone rubber male mold to form a preform; the silicone rubber male mold (core mold) after laying is placed into the rigid female mold and precisely aligned by positioning pins; the female mold is closed and locked, requiring the average gap of the mold joint to be <0.2mm to ensure the sealing of the molding cavity; the layup design of this embodiment is shown in Table 2.

[0019] Table 2 Ply Design for Example 2 Note: The total number of layers is 22, the thickness of a single T700 layer is 0.128mm, and the product wall thickness is 3mm.

[0020] The T300 fabric layer serves as the reinforcement layer, while the T700 unidirectional tape is the main structural layer. Layup orientation deviation requirements: unidirectional tape ±3°, fabric ±5°.

[0021] (4) Curing process: The assembled mold is placed in an oven for heating and curing. The silicone rubber positive mold expands after being heated, applying uniform pressure to the carbon fiber prepreg, replacing the high-pressure gas or mechanical pressure source in the traditional autoclave. After curing, the wingtip fairing of the UAV is obtained when the temperature is ≤60℃. Step (4) Curing procedure: First, heat up to 135℃ at a rate of 1℃ / min, then keep warm for 150min. During this stage, the silicone rubber expands due to heat, applying molding pressure to the prepreg. Cool down to ≤60℃ at a cooling rate of 2℃ / min, remove the mold, and the curing is complete.

[0022] This invention utilizes the expansion characteristics of a silicone rubber male mold to apply molding pressure, avoiding reliance on expensive autoclave equipment and significantly shortening the overall production cycle. It also improves mold utilization and product production efficiency, making it suitable for mass production demands of thousands of drones annually. This method is applicable to the molding of complex-shaped structural components while ensuring high product performance, meeting the mechanical shape requirements of wingtip fairings for different drone models.

Claims

1. A method for forming a UAV wingtip fairing based on the thermal expansion of a silicone rubber male mold, characterized in that, The wingtip fairing of this UAV features a streamlined, thin-walled structure, constructed from carbon fiber composite laminates, and formed using a silicone rubber core mold and a female mold. The specific molding method is as follows: (1) Mold design and preparation: Based on the three-dimensional digital model of the UAV wingtip fairing, the female mold is made of Q235B carbon structural steel. The inner surface of the female mold matches the shape of the outer aerodynamic surface of the fairing. The male mold is designed and made of 635T silicone rubber material. Its outer surface shape matches the inner surface of the fairing. The female mold is designed to work with the male mold to form a complete molding cavity. (2) Material preparation: High-performance carbon fiber / epoxy resin prepreg is selected as raw material. The carbon fiber / epoxy resin prepreg adopts T700 grade unidirectional tape prepreg and T300 grade fabric prepreg. (3) Material laying and mold assembly: Carbon fiber / epoxy resin prepreg is evenly laid on the surface of the silicone rubber male mold to form a preform; the silicone rubber male mold after laying is placed into the rigid female mold and precisely aligned by positioning pins; the female mold is closed and locked to ensure the sealing of the molding cavity; (4) Curing process: The assembled mold is placed in an oven and heated for curing. After curing, the mold is demolded when the temperature is ≤60℃ to obtain the wingtip fairing of the UAV.

2. The method for forming the wingtip fairing of a UAV according to claim 1, characterized in that, In step (1), a positioning pin is set on the edge of the female mold cavity for precise alignment between the female mold and the male mold.

3. The method for forming a UAV wingtip fairing according to claim 1, characterized in that, In step (1), the weight ratio of component A to component B in the 635T silicone rubber material is 100:1.5~2, where component A is addition-curing silicone rubber 635T and component B is a curing agent.

4. The method for forming a UAV wingtip fairing according to claim 1, characterized in that, In step (3), the average gap between the mold joints is <0.2mm.

5. The method for forming a UAV wingtip fairing according to claim 1, characterized in that, Step (3) The number of carbon fiber / epoxy resin prepreg layers is designed according to the thickness of the UAV wingtip fairing. The specific laying design is as follows: if all actual layers use T300 grade fabric prepreg, the laying direction is 0 / 90° and ±45° alternately laid; if the first and last layers of the actual lay use T300 grade fabric prepreg, and the middle layer uses T700 unidirectional tape prepreg, the laying direction is 0°, 90° and ±45° alternately laid, and the laying direction deviation requirements are: unidirectional tape ±3°, fabric ±5°.

6. The method for forming a UAV wingtip fairing according to claim 1, characterized in that, Step (4) The curing procedure is as follows: First, heat the temperature to 130~140℃ at a rate of 0.5~1.5℃ / min, then keep it at that temperature for 140~160min. After that, cool the temperature to ≤60℃ at a cooling rate of ≤2±1℃ / min, remove the mold, and the curing is complete.