A fiber-reinforced composite board and its preparation method

By modifying the fiber cloth and resin matrix and using vacuum-assisted processes, a fiber-reinforced composite board with a sandwich structure is formed, which solves the problems of insufficient impact resistance and thermal insulation performance in the existing technology, and achieves efficient energy-saving preparation and excellent mechanical and thermal insulation properties.

CN123104173APending Publication Date: 2026-11-17SHANGHAI ZHIQIAN IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611580826.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing fiber-reinforced composite panels are prone to debonding under impact loads, have insufficient impact resistance and flexural strength, and the insulation core layer is prone to water absorption, affecting thermal insulation performance. Furthermore, the manufacturing process is energy-intensive and complex, making it difficult to meet the application needs of the building and transportation sectors.

Method used

By activating the fiber cloth with organic acid and grafting it with aminosilane coupling agent, combined with the use of terminal amino polyether modified hydrogenated bisphenol A epoxy resin and modified resin matrix, a sandwich structure is formed, and aerogel board or rock wool is used as the insulation core layer. The structure is then cured at room temperature using a vacuum-assisted resin infusion process.

Benefits of technology

It significantly improves the impact resistance, flexural strength, and thermal insulation performance of the board, reduces the thermal conductivity, improves corrosion resistance, and meets the energy-saving and consumption-reducing requirements of green buildings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104173A_ABST
    Figure CN123104173A_ABST
Patent Text Reader

Abstract

This invention relates to the field of composite panel technology, and in particular to a fiber-reinforced composite panel and its preparation method. The panel includes a structural reinforcement layer and an insulating core layer. The structural reinforcement layer covers both sides of the insulating core layer, forming a sandwich structure. The structural reinforcement layer and the insulating core layer are bonded together by a modified resin matrix. The structural reinforcement layer is formed by impregnating modified fiber cloth with the modified resin matrix and then curing it. The modified fiber cloth is a fiber cloth that has been activated by organic acid and grafted with an aminosilane coupling agent. The modified resin matrix includes amino-terminated polyether-modified hydrogenated bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, and a curing agent component. This invention, through the synergistic effect of multiple technical means such as fiber surface chemical modification and resin matrix toughening modification, can simultaneously and significantly improve the impact resistance, flexural strength, thermal insulation performance, corrosion resistance, and electrothermal function of the fiber-reinforced composite panel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of composite board technology, and in particular to a fiber-reinforced composite board and its preparation method. Background Technology

[0002] Fiber-reinforced composite panels are typically composed of a structural reinforcement layer and an insulation core layer. The structural reinforcement layer provides mechanical load-bearing capacity, while the insulation core layer provides thermal insulation performance. The combination of the two forms a composite panel that combines structural strength and thermal insulation functions, and can be applied in fields such as construction and transportation.

[0003] In existing technologies, structural reinforcement layers are mostly made by impregnating fiber cloth with a resin matrix and curing it. The interfacial bonding strength between the fiber cloth and the resin matrix directly affects the overall performance of the board. However, fibers have few surface active groups and poor wettability with resin, resulting in weak interfacial bonding. Under impact loads, the fiber-resin interface is prone to debonding, leading to brittle failure of the board. The impact resistance and flexural strength are difficult to meet application requirements.

[0004] To improve the toughness of the resin matrix, toughening agents are often added to the epoxy resin system. However, traditional toughening agents such as carboxyl-terminated butadiene nitrile rubber and amino-terminated butadiene nitrile rubber have poor compatibility with epoxy resin, are prone to phase separation, and are difficult to disperse uniformly, resulting in a decrease in the uniformity and performance stability of the resin matrix and a limited toughening effect.

[0005] Aerogel boards, rock wool, and other insulation core layers have high porosity and are prone to water absorption. In humid or freeze-thaw environments, moisture can penetrate the core layer, causing an increase in thermal conductivity and a decrease in insulation performance. This results in poor durability over long-term use and affects the thermal insulation lifespan of the composite board.

[0006] In addition, the existing composite panel manufacturing process often relies on high-temperature and high-pressure curing equipment, which has high energy consumption and complex processes, and is not conducive to energy conservation, emission reduction and green building applications.

[0007] Therefore, providing a fiber-reinforced composite board and its preparation method that can balance impact resistance, thermal insulation performance and ease of preparation has significant application value. Summary of the Invention

[0008] The purpose of this invention is to provide a fiber-reinforced composite board and its preparation method. Through the synergistic effect of multiple technical means such as fiber surface chemical modification and resin matrix toughening modification, the impact resistance, flexural strength, thermal insulation performance, corrosion resistance and electrothermal function of the fiber-reinforced composite board can be significantly improved at the same time.

[0009] To achieve the above objectives, the present invention provides a fiber-reinforced composite board, comprising a structural reinforcement layer and an insulation core layer. The structural reinforcement layer covers both sides of the insulation core layer, forming a sandwich structure. The structural reinforcement layer and the insulation core layer are bonded together by a modified resin matrix. The structural reinforcement layer is formed by impregnating modified fiber cloth with a modified resin matrix and then curing it. The modified fiber cloth is a fiber cloth that has been activated by organic acid and grafted with an aminosilane coupling agent. The modified resin matrix includes amino-terminated polyether modified hydrogenated bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, and a curing agent component. The insulation core layer is one or more of aerogel board, rock wool, or an aerogel-rock wool composite layer.

[0010] Preferably, the fiber cloth is selected from one or more of glass fiber cloth, carbon fiber cloth, quartz fiber cloth, basalt fiber cloth or polyimide fiber cloth; Organic acid activation is performed using a mixed solution of citric acid and oxalic acid, where the concentration of citric acid is 0.1~0.2 mol / L and the concentration of oxalic acid is 0.5~1.0 mol / L. The aminosilane coupling agent is selected from one or more of ADMS silane coupling agent, KH550, and KH792.

[0011] Preferably, the amino-terminated polyether modified hydrogenated bisphenol A epoxy resin is prepared by reacting hydrogenated bisphenol A epoxy resin with amino-terminated polyether at a molar ratio of 1:(1.0~1.5); the amino-terminated polyether is selected from one or more of Jeffamine D-400, Jeffamine D-2000, Jeffamine T-403, Jeffamine ED-600, and Jeffamine ED-900.

[0012] Preferably, the mass ratio of the amino-terminated polyether modified hydrogenated bisphenol A epoxy resin to the curing agent is 1:(2~6):(0.7~1.7); the curing agent component includes a curing agent and an accelerator; the curing agent is selected from at least one of diethylenetriamine, triethylenetetramine, and 4,4'-diaminodicyclohexylmethane; the accelerator is 2,4,6-tris(dimethylaminomethyl)phenol; and the mass ratio of the curing agent to the accelerator is (10~15):1.

[0013] Preferably, the modified resin matrix also includes one or more of sodium carboxylate of natural rubber and carbon nanofibers, and the amount of sodium carboxylate of natural rubber added is 3 to 7 wt% and the amount of carbon nanofibers added is 0.5 to 3 wt% based on the mass of the modified resin matrix.

[0014] This invention also provides a method for preparing fiber-reinforced composite panels, comprising the following steps: S1. After the fiber cloth is activated by organic acid, it is grafted with an aminosilane coupling agent to obtain the modified fiber cloth. S2. Prepare amino-terminated polyether modified hydrogenated bisphenol A epoxy resin, mix it with hydrogenated bisphenol A epoxy resin, add curing agent component, and obtain modified resin matrix; S3. The modified fiber cloth obtained by S1 is laid in the mold in a ±45° oblique layup sequence. After vacuuming, the modified resin matrix of S2 is injected to impregnate the fiber cloth with resin. After injection, the vacuum state is maintained and the fiber cloth is cured at room temperature to obtain the structural reinforcement layer. S4. After the thermal insulation core layer is treated to be hydrophobic, it is placed between the two structural reinforcement layers obtained in S3 and bonded together with a modified resin matrix to form a sandwich structure, thus obtaining a fiber-reinforced composite board.

[0015] Preferably, in S1, the organic acid activation is carried out using a mixed solution of citric acid and oxalic acid, wherein the concentration of citric acid in the mixed solution is 0.1~0.2 mol / L, the concentration of oxalic acid is 0.5~1.0 mol / L, the activation temperature is 55~65℃, and the activation time is 3~6h; the grafting reaction is carried out under nitrogen protection and at 110~120℃ with stirring for 12~36h.

[0016] Preferably, in step S2, the preparation of the amino-terminated polyether modified hydrogenated bisphenol A epoxy resin includes the following steps: the hydrogenated bisphenol A epoxy resin and the amino-terminated polyether are vacuum dried to remove moisture; under nitrogen protection, the amino-terminated polyether is slowly added in batches to the hydrogenated bisphenol A epoxy resin, the molar ratio of the amino-terminated polyether to the hydrogenated bisphenol A epoxy resin being (1.0~1.5):1; the reaction temperature is controlled at 80~100℃, and the mixture is stirred at 200~300 rpm for 1~3 hours; heating is stopped, and the mixture is naturally cooled to room temperature under nitrogen protection to obtain the amino-terminated polyether modified hydrogenated bisphenol A epoxy resin.

[0017] Preferably, in S3, the number of layers of modified fiber cloth is 8 to 20; vacuum is applied to 0.090 to 0.098 MPa, and the mixture is cured at room temperature for 24 to 72 hours.

[0018] Preferably, in S4, the hydrophobic treatment involves immersing the thermal insulation core layer in a silane-based hydrophobic agent or a sodium methylsilicate solution, removing it, air-drying it, bonding and compositing it, and then curing it at room temperature for 10-14 hours under a pressure of 0.2-0.8 MPa.

[0019] Therefore, the present invention, employing the aforementioned fiber-reinforced composite board and its preparation method, has the following beneficial effects: (1) The flexible polyether segments in the amino-terminated polyether modified hydrogenated bisphenol A epoxy resin of the present invention can be curled and slipped under impact load, dissipating a large amount of impact energy and avoiding brittle fracture. At the same time, the aminosilane coupling agent grafted on the surface of the modified fiber cloth can bond with the epoxy group to form a strong interfacial bond. The synergistic effect of the two significantly improves the impact resistance and flexural strength of the board. Meanwhile, the amino-terminated polyether modified hydrogenated bisphenol A epoxy resin retains the hydrogenated bisphenol A skeleton and has the same molecular skeleton as the unmodified hydrogenated bisphenol A epoxy resin. The two have excellent compatibility and do not separate after mixing. This overcomes the defects of traditional toughening agents such as carboxyl-terminated butadiene nitrile rubber and amino-terminated butadiene nitrile rubber that are easy to separate, and ensures the uniformity and performance stability of the resin matrix.

[0020] (2) The present invention uses aerogel board, rock wool or aerogel-rock wool composite layer as insulation core layer, and combines it with the sealing protection of structural reinforcement layer to effectively reduce thermal conductivity; after the insulation core layer is treated with water-repellent treatment, the thermal conductivity caused by water intrusion under freeze-thaw environment can be significantly suppressed, and the long-term durability of insulation system can be improved.

[0021] (3) The present invention adopts a vacuum-assisted resin infusion process, which is cured at room temperature and does not require high temperature and high pressure equipment; both fiber cloth modification and resin modification are conventional chemical reactions with mild conditions and easy implementation; it meets the requirements of green building and sustainable development.

[0022] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0023] Figure 1 These are schematic diagrams illustrating the mechanical properties of various embodiments and comparative examples of the present invention. Detailed Implementation

[0024] This invention provides a fiber-reinforced composite board, comprising a structural reinforcement layer and an insulation core layer. The structural reinforcement layer covers both sides of the insulation core layer, forming a sandwich structure. The structural reinforcement layer and the insulation core layer are bonded together by a modified resin matrix. The structural reinforcement layer is formed by impregnating modified fiber cloth with a modified resin matrix and then curing it. The modified fiber cloth is a fiber cloth that has been activated by organic acid and grafted with an aminosilane coupling agent. The modified resin matrix includes amino-terminated polyether modified hydrogenated bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, and a curing agent component. The insulation core layer is one or more of aerogel board, rock wool, or an aerogel-rock wool composite layer.

[0025] The fiber-reinforced composite board of the present invention achieves simultaneous improvement in impact resistance, thermal insulation performance and corrosion resistance by combining modified fiber cloth, modified resin matrix and thermal insulation core layer through the synergistic effect of modified fiber cloth, modified resin matrix and thermal insulation core layer composite structure.

[0026] Preferably, the fiber cloth is selected from one or more of glass fiber cloth, carbon fiber cloth, quartz fiber cloth, basalt fiber cloth or polyimide fiber cloth; Organic acid activation is performed using a mixed solution of citric acid and oxalic acid, where the concentration of citric acid is 0.1~0.2 mol / L and the concentration of oxalic acid is 0.5~1.0 mol / L. The aminosilane coupling agent is selected from one or more of ADMS silane coupling agent, KH550, and KH792.

[0027] Preferably, the fiber cloth is selected from one or more of quartz fiber cloth, basalt fiber cloth or glass fiber cloth; the aminosilane coupling agent is ADMS silane coupling agent.

[0028] The fiber fabric of this invention is activated by organic acids. A mixed solution of citric acid and oxalic acid can gently remove the weak interfacial layer and impurities on the fiber surface, while introducing active carboxyl and hydroxyl groups on the fiber surface, increasing surface roughness and active sites, providing sufficient anchoring points for subsequent grafting of silane coupling agents. The organic acid activation conditions are mild, avoiding excessive damage to the fiber body by strong alkalis or strong acids, and preserving the mechanical strength of the fiber. After grafting treatment with aminosilane coupling agents, the hydrolyzable group (methoxy) at one end of the silane coupling agent hydrolyzes to generate silanol groups, which undergo a condensation reaction with the activated hydroxyl groups on the fiber surface to form stable Si-O-Si covalent bonds; the amino group (-NH2) at the other end can undergo a ring-opening reaction with the epoxy group of the epoxy resin, thereby constructing a chemical bridging structure between the fiber and the resin, significantly improving the interfacial bonding strength, enabling the effective transfer and dispersion of impact loads, and avoiding brittle failure caused by interfacial debonding.

[0029] Preferably, the amino-terminated polyether modified hydrogenated bisphenol A epoxy resin is prepared by reacting hydrogenated bisphenol A epoxy resin with amino-terminated polyether at a molar ratio of 1:(1.0~1.5); the amino-terminated polyether is selected from one or more of Jeffamine D-400, Jeffamine D-2000, Jeffamine T-403, Jeffamine ED-600, and Jeffamine ED-900.

[0030] More preferably, the terminal amino polyether is selected from one or more of Jeffamine D-400 and Jeffamine T-403.

[0031] The present invention relates to an amino-terminated polyether-modified hydrogenated bisphenol A epoxy resin. This modification involves a ring-opening addition reaction between the primary amino groups of the amino-terminated polyether and the epoxy groups of the hydrogenated bisphenol A epoxy resin, chemically bonding flexible polyether segments to the hydrogenated bisphenol A epoxy resin molecular chain. The polyether segments possess excellent chain mobility and flexibility, allowing them to bend, slip, and extend under impact loads. This chain motion dissipates a significant amount of impact energy, preventing brittle fracture of the epoxy resin due to excessive rigidity. Simultaneously, the modified resin molecules retain primary amino groups at both ends, enabling them to participate in subsequent curing and crosslinking reactions, introducing flexible segments into the crosslinking network to form an interpenetrating "rigid skeleton-flexible segment" structure. Furthermore, because the modified resin retains the hydrogenated bisphenol A skeleton, it shares the same molecular skeleton as the unmodified hydrogenated bisphenol A epoxy resin, resulting in excellent compatibility. The mixture does not separate after mixing, avoiding the phase separation problem common with traditional toughening agents (such as CTBN).

[0032] Preferably, the mass ratio of the amino-terminated polyether modified hydrogenated bisphenol A epoxy resin to the curing agent is 1:(2~6):(0.7~1.7); the curing agent component includes a curing agent and an accelerator; the curing agent is selected from at least one of diethylenetriamine, triethylenetetramine, and 4,4'-diaminodicyclohexylmethane; the accelerator is 2,4,6-tris(dimethylaminomethyl)phenol; and the mass ratio of the curing agent to the accelerator is (10~15):1.

[0033] More preferably, the mass ratio of the amino-terminated polyether modified hydrogenated bisphenol A epoxy resin to the curing agent is 1:5:(0.7~1.0); the curing agent is a compound of diethylenetriamine and 2,4,6-tris(dimethylaminomethyl)phenol in a mass ratio of (10~15):1.

[0034] The modified resin matrix of this invention uses amino-terminated polyether-modified hydrogenated bisphenol A epoxy resin as a toughening component, hydrogenated bisphenol A epoxy resin as the matrix resin, and a curing agent as a crosslinking curing component, all blended in a specific ratio. The mass ratio of the toughening component to the matrix resin is controlled at 1:(2~6), which significantly improves toughness while ensuring the rigidity and heat resistance of the matrix. If the toughening component is too small, the impact resistance will not be sufficiently improved; if the toughening component is too large, the crosslinking density will decrease, and the rigidity and heat resistance will be reduced. The blending of the curing agent and accelerator can adjust the curing rate and degree of curing, ensuring the formation of a uniform and dense crosslinked network under room temperature curing conditions.

[0035] Preferably, the modified resin matrix also includes one or more of sodium carboxylate of natural rubber and carbon nanofibers, and the amount of sodium carboxylate of natural rubber added is 3 to 7 wt% and the amount of carbon nanofibers added is 0.5 to 3 wt% based on the mass of the modified resin matrix.

[0036] In this invention, sodium carboxylate from natural rubber is used as an interface compatibilizer and toughening agent. The sodium carboxylate groups introduced into its molecular chain can strongly interact with inorganic fillers such as cement and silica powder, as well as polar groups on the fiber surface, improving the compatibility between organic resin and inorganic fillers. Simultaneously, it acts as a binder in the slurry, forming an organic-inorganic interpenetrating network structure, thus improving the density and corrosion resistance of the board. Natural rubber itself has good adhesion and toughness, which can further absorb impact energy, improving the flexural strength and corrosion resistance of the board. Carbon nanofibers, as functional fillers, can be uniformly dispersed in the resin matrix to form a three-dimensional conductive network, endowing the board with electrothermal functions. This allows the surface temperature of the board to be controlled within the range of 30~260℃, improving electrothermal efficiency and making it suitable for applications such as electric heating floors and wing de-icing. Furthermore, the introduction of carbon nanofibers also provides reinforcement, improving the mechanical properties of the resin matrix.

[0037] A further preferred embodiment is sodium carboxylate of natural rubber, which is prepared by hydrolysis and neutralization following a reaction of epoxy natural rubber with trimellitic anhydride, specifically including the following steps: Add 100 parts by weight of epoxy natural rubber to N,N-dimethylformamide, stir, then add 20-70 parts by weight of trimellitic anhydride, heat to 130-155℃ and stir for 6-12 hours; add water, heat to 80-90℃ and stir for hydrolysis for 4-6 hours; after cooling, add sodium hydroxide solution dropwise to neutralize the pH to 8-9; add ethanol to the solution, filter, wash the precipitate, and dry to obtain sodium natural rubber carboxylate.

[0038] More preferably, the carbon nanofibers are selected from one or more of carbon powder / carbon nanofibers, titanium carbide / carbon nanofibers, or carbon nanotubes / carbon nanofibers.

[0039] This invention also provides a method for preparing fiber-reinforced composite panels, comprising the following steps: S1. After the fiber cloth is activated by organic acid, it is grafted with an aminosilane coupling agent to obtain the modified fiber cloth. S2. Prepare amino-terminated polyether modified hydrogenated bisphenol A epoxy resin, mix it with hydrogenated bisphenol A epoxy resin, add curing agent component, and obtain modified resin matrix; S3. The modified fiber cloth obtained by S1 is laid in the mold in a ±45° oblique layup sequence. After vacuuming, the modified resin matrix of S2 is injected to impregnate the fiber cloth with resin. After injection, the vacuum state is maintained and the fiber cloth is cured at room temperature to obtain the structural reinforcement layer. S4. After the thermal insulation core layer is treated to be hydrophobic, it is placed between the two structural reinforcement layers obtained in S3 and bonded together with a modified resin matrix to form a sandwich structure, thus obtaining a fiber-reinforced composite board.

[0040] Preferably, in S1, the organic acid activation is carried out using a mixed solution of citric acid and oxalic acid, wherein the concentration of citric acid in the mixed solution is 0.1~0.2 mol / L, the concentration of oxalic acid is 0.5~1.0 mol / L, the activation temperature is 55~65℃, and the activation time is 3~6h; the grafting reaction is carried out under nitrogen protection and at 110~120℃ with stirring for 12~36h.

[0041] In a further preferred embodiment, in step S1, after the grafting reaction is completed, the modified fiber cloth is washed sequentially with deionized water, acetone, ethanol, and then deionized water, and then dried. This effectively removes unreacted silane coupling agent, solvent residue, and byproducts, ensuring the surface of the modified fiber cloth is clean and preventing impurities from interfering with subsequent resin wetting and interfacial bonding.

[0042] Preferably, in step S2, the preparation of the amino-terminated polyether modified hydrogenated bisphenol A epoxy resin includes the following steps: the hydrogenated bisphenol A epoxy resin and the amino-terminated polyether are vacuum dried to remove moisture; under nitrogen protection, the amino-terminated polyether is slowly added in batches to the hydrogenated bisphenol A epoxy resin, the molar ratio of the amino-terminated polyether to the hydrogenated bisphenol A epoxy resin being (1.0~1.5):1; the reaction temperature is controlled at 80~100℃, and the mixture is stirred at 200~300 rpm for 1~3 hours; heating is stopped, and the mixture is naturally cooled to room temperature under nitrogen protection to obtain the amino-terminated polyether modified hydrogenated bisphenol A epoxy resin.

[0043] Vacuum drying in S2 removes moisture from the hydrogenated bisphenol A epoxy resin and the amino-terminated polyether, preventing side reactions between moisture and epoxy groups and preventing bubble formation, thus ensuring the purity of the reaction system. Nitrogen protection prevents oxygen and moisture from interfering with the reaction and avoids epoxy group oxidation or amine absorption of carbon dioxide. Slow, batch-wise addition of the amino-terminated polyether controls the exothermic reaction rate, preventing localized overheating that could lead to gelation or explosive polymerization, ensuring a stable reaction. The reaction temperature is 80-100℃: the ring-opening addition reaction between epoxy groups and primary amines has a suitable reaction rate within this temperature range; too low a temperature results in incomplete reaction, while too high a temperature can easily lead to crosslinking side reactions. The reaction time is 1-3 hours: this ensures sufficient reaction between the primary amine group and the epoxy group in the amino-terminated polyether, while avoiding excessively long reaction times that could increase product viscosity or cause gelation.

[0044] The reaction mechanism is as follows: the primary amino group of the terminal amino polyether undergoes a ring-opening addition reaction with the epoxy group of the hydrogenated bisphenol A epoxy resin to generate a β-hydroxy secondary amine structure, which chemically bonds the flexible segment of the polyether to the molecular chain of the hydrogenated bisphenol A epoxy resin.

[0045] The general structural formula of amino-terminated polyether modified hydrogenated bisphenol A epoxy resin is: ; Wherein: PPG is a polypropylene glycol segment with a molecular weight of 400-1000; R' is a hydrogenated bisphenol A backbone (dicyclohexylpropane structure). Each end of the molecule retains a primary amino group (-NH2), which can participate in subsequent curing and crosslinking reactions; Introducing flexible polyether segments into the molecular chain provides excellent flexibility and impact resistance; The rigid cyclohexane backbone and hydroxyl groups (-OH) of hydrogenated bisphenol A epoxy resin are retained in the molecular backbone.

[0046] In this invention, the terminal amino polyether is preferably Jeffamine D-400 or Jeffamine T-403. D-400 has a moderate molecular weight, good flexibility, and excellent compatibility with hydrogenated bisphenol A epoxy resin; T-403 is trifunctional and can participate in cross-linking reactions, improving the toughening effect while maintaining the network structure; both are commercially available products and are easy to industrialize.

[0047] Preferably, in S3, the number of layers of modified fiber cloth is 8 to 20; vacuum is applied to 0.090 to 0.098 MPa, and the mixture is cured at room temperature for 24 to 72 hours.

[0048] In this invention, S3 features a ±45° oblique layup: adjacent fiber layers are arranged alternately at +45° and -45°, allowing the fibers to share the load in multiple directions, improving the isotropy and impact resistance of the composite board. The oblique layup also increases interlaminar shear strength, preventing interlaminar delamination. Vacuuming to 0.090~0.098MPa: Vacuum negative pressure removes air and volatiles from the laminated structure, promoting uniform resin penetration and wetting of the fiber cloth, reducing bubbles and pore defects, and improving the density and mechanical properties of the composite board. Room temperature curing for 24~72h: Room temperature curing avoids thermal stress and fiber damage caused by high-temperature curing, while ensuring full cross-linking and curing of the resin to form a stable three-dimensional network structure.

[0049] In a further preferred embodiment, in S3, the directions of the adjacent layers of modified fiber cloth are alternately arranged at +45° and -45°, respectively, to control the flatness, wrinkle-free surface, and tight adhesion. On the laid modified fiber cloth, the release cloth and the flow guide net are laid in sequence, and the whole is covered by a vacuum bag film. The edges are sealed to the mold with sealing strips. A vacuum pump inlet, a resin pouring port, and an overflow port are set to form a layered structure. After room temperature curing, the vacuum bag film, the flow guide net, and the release cloth are removed. The edges, overflow glue, and surface defects are removed by mechanical grinding, and the grinding depth does not exceed 0.2mm.

[0050] Preferably, in step S4, the hydrophobic treatment involves immersing the insulation core layer in a silane-based hydrophobic agent or a sodium methylsilicate solution, removing it, air-drying it, bonding and laminating it, and then curing it at room temperature for 10-14 hours under a pressure of 0.2-0.8 MPa. This forms a hydrophobic film on the surface of the insulation core layer, reducing its water absorption rate and preventing moisture penetration in humid or freeze-thaw environments, which could lead to a decrease in insulation performance and structural damage.

[0051] The fiber-reinforced composite panels of the present invention can be used for building exterior walls, electric heating floors, automotive interiors, or rail transit interiors.

[0052] The present invention will be further described below with reference to the accompanying drawings and embodiments. Unless otherwise defined, the technical or scientific terms used in this invention should be understood in their ordinary sense by those skilled in the art. The features mentioned above or in the specific examples mentioned in this invention can be combined arbitrarily, and these specific embodiments are only used to illustrate the invention and are not intended to limit the scope of the invention.

[0053] Example 1 A fiber-reinforced composite board is prepared by means of the following steps: S1. Preparation of modified fiber cloth: Prepare a mixed solution of citric acid and oxalic acid, with a citric acid concentration of 0.15 mol / L and an oxalic acid concentration of 0.75 mol / L; precipitate quartz fiber cloth (area density 200 g / m²) 2 Cut the material into 15cm × 15cm pieces, immerse them in the mixed solution, heat to 60℃, and stir for 4 hours. After the reaction, wash three times with deionized water and dry to obtain activated quartz fiber cloth. Add the activated quartz fiber cloth to 5 times its weight of dry toluene, and add 0.1 times its weight of ADMS silane coupling agent. Under nitrogen protection, stir and react at 115℃ for 24 hours. After the reaction, wash successively with deionized water, acetone, ethanol, and deionized water, and dry to obtain modified quartz fiber cloth.

[0054] S2. Preparation of modified resin matrix: Hydrogenated bisphenol A epoxy resin (DGEHBA) and Jeffamine D-400 were vacuum dried to remove moisture. Under nitrogen protection, Jeffamine D-400 was slowly added to DGEHBA in batches at a molar ratio of 1.2:1. The reaction temperature was controlled at 90℃, and the mixture was stirred at 250 rpm for 2 hours. Heating was then stopped, and the mixture was allowed to cool naturally to room temperature under nitrogen protection to obtain amino-terminated polyether modified hydrogenated bisphenol A epoxy resin.

[0055] A amine-terminated polyether-modified hydrogenated bisphenol A epoxy resin and hydrogenated bisphenol A epoxy resin were mixed at a mass ratio of 1:5 and mechanically stirred until no layering occurred, yielding the resin component. Diethylenetriamine and 2,4,6-tris(dimethylaminomethyl)phenol were mixed evenly at a mass ratio of 12:1, yielding the curing agent component. The resin component and the curing agent component were mixed at a mass ratio of 1:0.75, i.e., amine-terminated polyether-modified hydrogenated bisphenol A epoxy resin: hydrogenated bisphenol A epoxy resin: curing agent component = 1:5:0.75, and stirred evenly to obtain the modified resin matrix.

[0056] S3. Preparation of structural reinforcement layer: Thirteen layers of modified quartz fiber cloth obtained from S1 were sequentially laid in the mold in a ±45° oblique layup sequence. The fiber directions of adjacent fiber cloth layers were arranged alternately at +45° and -45°, respectively. During the layup process, the modified quartz fiber cloth was kept flat and wrinkle-free, and the adjacent fiber cloths were tightly bonded together. A release cloth and a flow guide net were then sequentially laid on the laid modified quartz fiber cloth. The release cloth and the flow guide net completely covered the upper surface of the release cloth. A vacuum bag film was used to completely cover the layup structure. The edges of the vacuum bag film were sealed to the edges of the mold with sealing strips. A vacuum pump inlet, a resin pouring port, and an overflow port were set on the vacuum bag film to form a laminated structure.

[0057] The vacuum pump was started to evacuate the laminated structure to 0.095 MPa. The modified resin matrix obtained from S2 was connected to the resin pouring port through the injection tube, allowing the modified resin matrix to evenly penetrate and impregnate the modified quartz fiber cloth along the guide net under vacuum negative pressure. Injection continued until the modified resin matrix flowed steadily from the overflow port without any air bubbles. Then, injection was stopped, and the vacuum pump was kept running for 25 minutes to remove any residual air bubbles in the system. After injection, the system was kept under vacuum and cured at room temperature for 48 hours. After curing, the vacuum bag, guide net, and release cloth were removed. The edges of the composite board were removed by mechanical grinding to remove burrs, excess glue, and surface defects. The grinding depth should not exceed 0.2 mm to ensure a smooth surface of the composite board and obtain the structural reinforcement layer.

[0058] S4, Composite Insulation Core Layer: A 2cm aerogel board was combined with a 3cm rock wool layer to obtain an aerogel-rock wool composite layer. This composite layer was then immersed in a sodium methylsilicate solution, removed, and air-dried to complete the hydrophobic treatment. The hydrophobic-treated aerogel-rock wool composite layer was placed between two structural reinforcement layers obtained from S3, using a modified resin matrix obtained from S2 as a binder. The mixture was cured at room temperature for 12 hours under 0.5MPa pressure to form a sandwich structure. Subsequently, the composite board was dimensionally adjusted to obtain a fiber-reinforced composite board.

[0059] Example 2 It is basically the same as Example 1, except that: In S1, the fiber cloth is replaced with basalt fiber cloth, and the modified fiber cloth has 15 layers.

[0060] In S2, the amino-terminated polyether is replaced with Jeffamine T-403, the molar ratio of amino-terminated polyether to DGEHBA is 1.5:1, the reaction temperature is 100℃, and the reaction is stirred for 1.5h; the ratio of amino-terminated polyether modified hydrogenated bisphenol A epoxy resin: hydrogenated bisphenol A epoxy resin: curing agent component is 1:3:0.8; the curing agent is triethylenetetramine and 2,4,6-tris(dimethylaminomethyl)phenol compounded in a mass ratio of 15:1; sodium carboxylate of natural rubber is also added to the modified resin matrix, and the amount added is 5wt% of the mass of the modified resin matrix.

[0061] In S4, the insulation core layer is a 3 cm aerogel board.

[0062] Example 3 It is basically the same as Example 1, except that: In S2, the terminal amino polyether is replaced with Jeffamine ED-600, the molar ratio of terminal amino polyether to DGEHBA is 1.0:1, the reaction temperature is 80℃, and the reaction is stirred for 3 hours; the ratio of terminal amino polyether modified hydrogenated bisphenol A epoxy resin: hydrogenated bisphenol A epoxy resin: curing agent component is 1:2:0.7; the curing agent is a mixture of 4,4'-diaminodicyclohexylmethane and 2,4,6-tris(dimethylaminomethyl)phenol in a mass ratio of 10:1; carbon nanotubes / carbon nanofibers are also added to the modified resin matrix, with an addition amount of 2wt% of the modified resin matrix.

[0063] In S4, the insulation core layer is 8cm of rock wool, which is treated with sodium methylsilicate for hydrophobicity; the bonding pressure is 0.8MPa, and the curing time is 10 h at room temperature.

[0064] Example 4 It is basically the same as Example 1, except that: In S2, the amino-terminated polyether is replaced with Jeffamine D-2000, and the molar ratio of amino-terminated polyether to DGEHBA is 1.3:1; the ratio of amino-terminated polyether-modified hydrogenated bisphenol A epoxy resin to hydrogenated bisphenol A epoxy resin to curing agent is 1:6:1.0.

[0065] In S3, the modified fiber cloth has 8 layers.

[0066] In S4, the insulation core layer is 3cm rock wool, the bonding composite pressure is 0.2MPa, and the curing time is 14h at room temperature.

[0067] Example 5 It is basically the same as Example 1, except that: In S1, the aminosilane coupling agent is replaced with KH550.

[0068] In S2, sodium carboxylate of natural rubber and titanium carbide / carbon nanofibers are added to the modified resin matrix at the same time. The amount of sodium carboxylate of natural rubber added is 3 wt% of the mass of the modified resin matrix, and the amount of titanium carbide / carbon nanofibers added is 0.5 wt% of the mass of the modified resin matrix.

[0069] In S4, the insulation core layer is a 2cm aerogel board.

[0070] Comparative Example 1 The process is basically the same as in Example 1, except that in S1, the fiber cloth is not activated by organic acid and grafted with ADMS silane coupling agent, and the original quartz fiber cloth is used directly for layup.

[0071] Comparative Example 2 The process is basically the same as in Example 1, except that in S2, no amino-terminated polyether-modified hydrogenated bisphenol A epoxy resin is added; only unmodified hydrogenated bisphenol A epoxy resin is used as the resin component.

[0072] Comparative Example 3 The example is basically the same as in Example 1, except that in S2, the amino-terminated polyether is replaced with an equimolar amount of carboxyl-terminated nitrile butadiene rubber (CTBN).

[0073] Comparative Example 4 It is basically the same as Example 1, except that in S4, the insulation core layer is ordinary rock wool, which has not been treated with water repellency, and the structural reinforcement layer and the insulation core layer are bonded with ordinary epoxy resin.

[0074] Performance testing The fiber-reinforced composite panels prepared in each embodiment and the comparative example were subjected to performance tests. The test results are shown in Table 1 and 2. Figure 1 The testing method is as follows: Impact strength: Tested according to GB / T 1451-2005 "Impact toughness of simply supported beam fiber reinforced plastics"; Flexural strength: Tested according to GB / T 1449-2005 "Test Method for Flexural Properties of Fiber Reinforced Plastics"; Thermal conductivity: Tested according to GB / T 10295-2008 "Determination of steady-state thermal resistance and related properties of thermal insulation materials by heat flow meter method"; Freeze-thaw cycle test: 50 freeze-thaw cycles were conducted according to GB / T 30100-2013 "Test Methods for Building Wall Panels" to test the change in thermal conductivity before and after freeze-thaw. Corrosion resistance: The maximum width of horizontal cryolite erosion was tested according to YB / T 4161-2007 "Test Method for Resistance of Refractory Materials to Cryolite Erosion". Electrothermal performance: The surface temperature and electrothermal efficiency of the plate were tested under a 12V DC voltage.

[0075] Table 1 Performance test results of each embodiment and comparative example

[0076] Note: " / " in the table indicates that no test was conducted. Boards without added carbon nanofibers do not have electrothermal function, so surface temperature and electrothermal efficiency were not tested.

[0077] From Table 1 and Figure 1 It can be known that: (1) In terms of mechanical properties, the impact strength and flexural strength of Examples 1-5 are significantly better than those of Comparative Examples 1-4, indicating that the synergistic effect of fiber surface modification and resin matrix toughening can effectively improve the mechanical properties of the board.

[0078] (2) Regarding thermal conductivity, the thermal conductivity of Examples 1-5 is 0.030~0.038 W / (m•K), which is at a low level and can meet the insulation requirements. The thermal conductivity of Comparative Examples 1-3 is comparable to that of the Examples, while the thermal conductivity of Comparative Example 4 is the highest, at 0.042 W / (m•K). This indicates that the thermal conductivity is mainly determined by the insulation core layer and the bonding interface. In this application, the modified resin matrix is ​​bonded and composited with an aerogel / rock wool composite insulation core layer, which is beneficial to obtaining and maintaining a low thermal conductivity.

[0079] (3) Regarding freeze-thaw durability, the thermal conductivity growth rate of Examples 1 to 5 after 50 freeze-thaw cycles was only 4.8% to 7.8%, which was significantly lower than the 22.5% of Comparative Example 4. This indicates that the application of this application to treat the insulation core layer with water repellency and use modified resin matrix bonding can effectively suppress the increase in thermal conductivity caused by moisture intrusion in the freeze-thaw environment and improve the long-term durability of the insulation system.

[0080] (4) Regarding corrosion resistance, the maximum width of horizontal erosion by cryolite in Examples 1-5 was 2.5-3.5 mm, significantly smaller than the 5.8-6.4 mm of Comparative Examples 1-4. Specifically, the erosion widths of Comparative Examples 1, 2, and 3 were 6.4 mm, 6.3 mm, and 5.8 mm, respectively, all significantly higher than those of the examples. This indicates that the synergistic effect of organic acid activation on the fiber surface, graft modification with aminosilane coupling agent, toughening with hydrogenated bisphenol A epoxy resin modified with terminal amino polyether, and interfacial compatibilization with sodium carboxylate of natural rubber can significantly enhance the interfacial bonding between the fiber and resin, thereby improving the corrosion resistance of the board.

[0081] (5) In terms of electrothermal performance, the surface temperature of Example 3 can reach 180℃ and the electrothermal efficiency is 92.3%, while the surface temperature of Example 5 can reach 135℃ and the electrothermal efficiency is 88.6%. This shows that the introduction of carbon nanofibers gives the board good electrothermal function, which can meet the usage requirements of scenarios such as electric heating floor and wing de-icing.

[0082] In summary, this invention, through the synergistic effect of multiple technical means such as organic acid activation, aminosilane coupling agent modification of fiber cloth, amino-terminated polyether modified hydrogenated bisphenol A epoxy resin toughening of the resin matrix, sodium carboxylate interface compatibilization of natural rubber, functionalization of carbon nanofibers, aerogel / rock wool insulation core layer composite, and hydrophobic treatment, can simultaneously and significantly improve the impact resistance, thermal insulation performance, corrosion resistance, and electrothermal function of fiber-reinforced composite panels. Moreover, the process is simple, easy to implement, and has broad application prospects.

[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the technical solutions of the present invention, and these modifications or equivalent substitutions cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.

Claims

1. A fiber-reinforced composite board, characterized in that: It includes a structural reinforcement layer and an insulation core layer. The structural reinforcement layer covers both sides of the insulation core layer, forming a sandwich structure. The structural reinforcement layer and the insulation core layer are bonded together by a modified resin matrix. The structural reinforcement layer is formed by impregnating modified fiber cloth with a modified resin matrix and then curing it. The modified fiber cloth is a fiber cloth that has been activated by organic acid and grafted with an aminosilane coupling agent. The modified resin matrix includes amino-terminated polyether modified hydrogenated bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin and curing agent components. The insulation core layer is one or more of aerogel board, rock wool or aerogel-rock wool composite layer.

2. The fiber-reinforced composite board according to claim 1, characterized in that: The fiber cloth is selected from one or more of glass fiber cloth, carbon fiber cloth, quartz fiber cloth, basalt fiber cloth or polyimide fiber cloth; Organic acid activation is performed using a mixed solution of citric acid and oxalic acid, where the concentration of citric acid is 0.1~0.2 mol / L and the concentration of oxalic acid is 0.5~1.0 mol / L. The aminosilane coupling agent is selected from one or more of ADMS silane coupling agent, KH550, and KH792.

3. The fiber-reinforced composite board according to claim 1, characterized in that: The amino-terminated polyether modified hydrogenated bisphenol A epoxy resin is prepared by reacting hydrogenated bisphenol A epoxy resin with amino-terminated polyether at a molar ratio of 1:(1.0~1.5); the amino-terminated polyether is selected from one or more of Jeffamine D-400, Jeffamine D-2000, Jeffamine T-403, Jeffamine ED-600, and Jeffamine ED-900.

4. The fiber-reinforced composite board according to claim 1, characterized in that: The hydrogenated bisphenol A epoxy resin modified with amino-terminated polyether has a mass ratio of 1:(2~6):(0.7~1.7) to the curing agent; the curing agent component includes a curing agent and an accelerator; the curing agent is selected from at least one of diethylenetriamine, triethylenetetramine, and 4,4'-diaminodicyclohexylmethane; the accelerator is 2,4,6-tris(dimethylaminomethyl)phenol; and the mass ratio of the curing agent to the accelerator is (10~15):

1.

5. The fiber-reinforced composite board according to claim 1, characterized in that: The modified resin matrix also includes one or more of sodium carboxylate from natural rubber and carbon nanofibers. The amount of sodium carboxylate from natural rubber added is 3-7 wt% and the amount of carbon nanofibers added is 0.5-3 wt% based on the mass of the modified resin matrix.

6. A method for preparing a fiber-reinforced composite board according to any one of claims 1-5, characterized in that: Includes the following steps: S1. After the fiber cloth is activated by organic acid, it is grafted with an aminosilane coupling agent to obtain the modified fiber cloth. S2. Prepare amino-terminated polyether modified hydrogenated bisphenol A epoxy resin, mix it with hydrogenated bisphenol A epoxy resin, add curing agent component, and obtain modified resin matrix. S3. The modified fiber cloth obtained by S1 is laid in the mold in a ±45° oblique layup sequence. After vacuuming, the modified resin matrix of S2 is injected to impregnate the fiber cloth with resin. After injection, the vacuum state is maintained and the fiber cloth is cured at room temperature to obtain the structural reinforcement layer. S4. After the thermal insulation core layer is treated to be hydrophobic, it is placed between the two structural reinforcement layers obtained in S3 and bonded together with a modified resin matrix to form a sandwich structure, thus obtaining a fiber-reinforced composite board.

7. The method for preparing a fiber-reinforced composite board according to claim 6, characterized in that: In S1, the organic acid activation is carried out by using a mixed solution of citric acid and oxalic acid, with the concentration of citric acid in the mixed solution being 0.1~0.2 mol / L and the concentration of oxalic acid being 0.5~1.0 mol / L, the activation temperature being 55~65℃, and the activation time being 3~6h; the grafting reaction is carried out under nitrogen protection at 110~120℃ with stirring for 12~36h.

8. The method for preparing a fiber-reinforced composite board according to claim 6, characterized in that: In S2, the preparation of amino-terminated polyether-modified hydrogenated bisphenol A epoxy resin includes the following steps: hydrogenated bisphenol A epoxy resin and amino-terminated polyether are vacuum dried to remove moisture; under nitrogen protection, the amino-terminated polyether is slowly added to the hydrogenated bisphenol A epoxy resin in batches, with a molar ratio of amino-terminated polyether to hydrogenated bisphenol A epoxy resin of (1.0~1.5):1; the reaction temperature is controlled at 80~100℃, and the mixture is stirred at 200~300 rpm for 1~3 hours; heating is stopped, and the mixture is naturally cooled to room temperature under nitrogen protection to obtain amino-terminated polyether-modified hydrogenated bisphenol A epoxy resin.

9. The method for preparing a fiber-reinforced composite board according to claim 6, characterized in that: In S3, the number of layers of modified fiber cloth is 8 to 20; vacuum is applied to 0.090 to 0.098 MPa, and the mixture is cured at room temperature for 24 to 72 hours.

10. The method for preparing a fiber-reinforced composite board according to claim 6, characterized in that: In S4, the hydrophobic treatment involves immersing the thermal insulation core layer in a silane-based hydrophobic agent or a sodium methylsilicate solution, removing it, air-drying it, bonding and laminating it, and then curing it at room temperature for 10-14 hours under a pressure of 0.2-0.8 MPa.