A multilayer physically foamed co-extruded material and its preparation process

By combining a ternary cross-linked branched system and a specific filling system with an integrated mold composite process, the problems of poor cell formation and interlayer delamination in multilayer foamed materials have been solved. Stable formation and high-strength bonding of micron-level closed micropores have been achieved, improving the overall performance and production efficiency of the material.

CN123104200APending Publication Date: 2026-11-17JIANGXI FANSHENG TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611202114.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing multilayer foamed materials suffer from problems such as poor cell formation between the foaming layer and the surface layer, easy delamination between layers, warping and deformation of finished products, and easy degradation during high-temperature processing, which are difficult to solve simultaneously with existing technologies.

Method used

By employing a ternary cross-linking branching system and a specific filling system, combined with an integrated mold composite process, a molecular network is formed through organic peroxide cross-linking agents, multifunctional acrylate branching monomers, and cross-linking activators. In conjunction with interlayer compatibility aids and molding control aids, high-strength bonding and stable microporous molding between the foamed and non-foamed layers are achieved.

Benefits of technology

It achieves stable molding of micron-level closed micropores, widens the processing window, avoids cell rupture and interlayer delamination, improves the tensile toughness and processing fluidity of materials, and reduces production costs and equipment complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention relates to a multilayer physically foamed co-extruded material, comprising at least one foamed layer and at least one non-foamed layer. The matrix resin of the foamed layer includes at least one of PE, EVA, and GPPS, and the matrix resin of the non-foamed layer includes PP or PE. The raw materials of the foamed layer include the matrix resin and functional additives. The functional additives include melt strength modifiers, interlayer compatibility additives, filler modifiers, foaming additives, and molding control additives. Based on 100 parts by weight of the matrix resin of the foamed layer, the melt strength modifiers include: 0.2-1 parts of organic peroxide crosslinking agent, 0.3-2 parts of multifunctional acrylate branched monomers, and 1-3 parts of co-crosslinking activator. This invention solves the defects of incompatibility of multiphase materials and easy delamination at multilayer interfaces in the foamed layer by using two independent compatibility systems within and between the layers. The specific ternary crosslinking system balances melt strength and processing fluidity, resulting in a finished product with fine and uniform cells, no warping or delamination, and a wide processing window. It can be used in rigid sound insulation and buffer sheets, industrial protective pads, and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of foamed composite materials technology, specifically relating to a multilayer physically foamed co-extruded material and its preparation process. Background Technology

[0002] Polyolefin microporous foam composites are widely used in automotive interiors, packaging cushioning, building insulation, and electronic padding due to their advantages such as lightweight cushioning, thermal and sound insulation, and low cost. Currently, the mainstream foaming processes are divided into chemical foaming and supercritical CO2 / butane physical microporous foaming. Physical foaming can achieve micron-level fine closed pores, leaving no chemical foaming agent residue, resulting in superior product texture and mechanical properties, and represents the mainstream development direction for high-end foam materials.

[0003] Multilayer foamed materials are typically composed of a polyolefin (PE / EVA / GPPS) foamed core layer and a dense, non-foamed PP / PE surface layer, combining the cushioning function of the foamed layer with the wear resistance, printability, and barrier properties of the surface layer. However, due to significant differences in the molecular structure, polarity, and crystallinity of the resins in the foamed and surface layers, they are naturally incompatible, leading to a series of long-standing problems such as poor cell formation, easy delamination between layers, warping and deformation of finished products, and easy degradation during high-temperature processing. Current technologies mainly focus on improving these issues through foam modification formulations and multilayer composite processes, but both have limitations and cannot completely solve the defects in production and the final product.

[0004] Therefore, it is urgent to simultaneously optimize the formulation system and preparation process to address the aforementioned industry pain points. Summary of the Invention

[0005] To overcome the shortcomings of the prior art, the present invention solves the problems of insufficient melt strength, poor filler dispersion, interlayer delamination and narrow processing window by using a ternary cross-linked branched system and a specific filling system, combined with an integrated mold composite process.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: The present invention provides a multilayer physically foamed co-extruded material, comprising at least one foamed layer and at least one non-foamed layer, wherein the matrix resin of the foamed layer comprises at least one of PE, PET, EVA, and GPPS, and the matrix resin of the non-foamed layer comprises PP or PE. The raw materials for the foamed layer include a matrix resin and functional additives, wherein the functional additives include melt strength modifiers, filler modifiers, foaming aids, and molding control aids. Based on 100 parts by weight of the foaming layer matrix resin, the melt strength modifying agent includes: 0.2-1 parts of organic peroxide crosslinking agent, 0.3-2 parts of polyfunctional acrylate branched monomer, and 1-3 parts of crosslinking activator.

[0007] In some embodiments, the organic peroxide crosslinking agent includes at least one of dicumyl peroxide, di-tert-butyl peroxide, and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.

[0008] In some embodiments, the multifunctional acrylate branched monomer is selected from at least one of trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and ethylene glycol dimethacrylate.

[0009] In some embodiments, the crosslinking activator includes triallyl isocyanurate and / or diallyl phthalate.

[0010] The present invention modifies the melt strength of the foam layer using a ternary compound system of organic peroxide crosslinking agent, multifunctional acrylate branched monomer, and co-crosslinking activator. Within the extrusion crosslinking temperature range, the organic peroxide decomposes upon heating to generate free radicals, forming macromolecular active sites on the PE / EVA / GPPS matrix. The multifunctional acrylate monomer is grafted onto the polyolefin backbone to introduce a large number of flexible long branches, improving the degree of molecular chain entanglement and melt elasticity. The co-crosslinking activator prolongs the effective reaction time of free radicals, constructing controllable sparse micro-crosslinking nodes between long branches, and consuming free radicals that easily cause resin chain breakage, thus inhibiting high-temperature degradation of the substrate. The ternary components synergistically form a molecular network where long branch entanglement and mild covalent crosslinking coexist, simultaneously solving the defects of poor flowability of single peroxide crosslinking and insufficient high-temperature melt strength of simple branching modification. This gives the foamed melt both excellent tensile toughness and processing flowability, effectively supporting the bubble wall during the physical foaming decompression and stretching stage, preventing bubble rupture and merging, and achieving stable micron-level micropore formation throughout the entire range.

[0011] In some embodiments, the raw materials of the co-extruded material also include an interlayer compatibility agent, which is maleic anhydride-grafted polyolefin. The interlayer compatibility agent is pre-mixed into the non-foamed layer, and the amount of interlayer compatibility agent added is 3-5 wt% based on the total mass of the foamed layer and the non-foamed layer.

[0012] In some embodiments, the maleic anhydride-grafted polyolefin compatibility agent can be adaptively adjusted according to different foamed and non-foamed layers, as follows: 1) Maleic anhydride grafted polyethylene: suitable for PEPET / / GPPS / EVA foamed layer + PE non-foamed layer; 2) Maleic anhydride grafted polypropylene: suitable for PE / PET / EVA / GPPS foamed layer + PP non-foamed layer.

[0013] In some embodiments, the foaming agent includes a lubricant and / or an antioxidant; the lubricant includes at least one of stearic acid, zinc stearate, polyethylene wax, and oxidized polyethylene wax; the antioxidant includes hindered phenolic primary antioxidant and phosphite secondary antioxidant.

[0014] Preferably, the foaming agent comprises 0.3-2 parts of lubricant and 0.3-5 parts of antioxidant, wherein the hindered phenolic primary antioxidant comprises 0.1-2 parts and the phosphite secondary antioxidant comprises 0.2-3 parts.

[0015] The system employs a combination of hindered phenol as the primary antioxidant and phosphite as the secondary antioxidant, which effectively captures free radicals generated by cross-linking reactions, preventing the degradation of polyolefin molecular chains and resulting in finished products free from yellowing and tensile strength reduction.

[0016] The lubrication system is reasonably controlled at 0.3 to 2.0 parts, which has both internal and external lubrication effects: reducing the frictional resistance of the screw and die head and reducing material accumulation; at the same time, a small amount of lubricant migrates to the cell wall, improving the toughness of the cell wall, preventing micropore shrinkage and collapse during the cooling stage, and making the sheet surface flat and smooth.

[0017] In some embodiments, the filler modifier includes inorganic fillers, polymeric reinforcing phases, and intralayer compatibilizers; the inorganic fillers include at least one of talc, calcium carbonate, silica, and mica powder; the polymeric reinforcing phase includes at least one of PA6, PA12, and EMA.

[0018] In some embodiments, the intralayer compatibilizer is EVA-g-MAH.

[0019] Preferably, the filler modifier comprises 2-6 parts of inorganic filler, 3-5 parts of polymeric reinforcing phase, and 2-3 parts of intralayer compatibilizer, based on 100 parts by weight of the foaming layer matrix resin.

[0020] This invention solves the problem of filler agglomeration defects in the foam layer by using intralayer EVA-g-MAH. The foam layer is compounded with nano-silica, montmorillonite inorganic filler, and PA6 / PA12 polar polymer. The filler surface is rich in hydroxyl groups, and nylon has a large number of amide polar groups, resulting in extremely high interfacial tension with the non-polar matrix. After adding EVA-g-MAH, its EVA main chain segment is compatible with the foam matrix, and the maleic anhydride branched on the side can covalently bond with the terminal amino groups of PA, while forming hydrogen bonds with the hydroxyl groups of the inorganic filler, thus building a multi-level bridging structure of "matrix-EVA-g-MAH-nylon / inorganic filler", which completely eliminates filler white spots and two-phase grooves. In addition, PA can synergistically improve the foam wall modulus with the cross-linking network, and has multiple functions such as heterogeneous nucleation, enhanced heat resistance, wear resistance and resilience.

[0021] In some embodiments, the molding control aid comprises 0.2 to 1.5 parts of a viscosity modifier; the viscosity modifier includes one or more of low melt index LDPE, PP wax, hydrogenated petroleum resin, and terpene resin.

[0022] In some embodiments, 0 to 1.0 parts by weight of a retarding crystallization aid are added based on 100 parts by weight of the non-foamed matrix resin; the retarding crystallization aid is an aliphatic amide or a random polyα-olefin.

[0023] When the non-foamed layer is PP, it is necessary to add a slow crystallization aid to delay the growth rate of PP spherulites and match the cooling rhythm of the PE / PETEVA / GPPS foamed layer; a viscosity modifier balances the melt flow rate of the two layers, reduces extrusion flow fluctuations, reduces internal stress in the product from the source of the formulation, and improves warping and uneven thickness problems.

[0024] A second aspect of the present invention provides a process for preparing a multilayer physically foamed co-extruded material, comprising the following steps: S1 Material Premixing: Mix melt strength modifier, filler modifier, foaming agent, and molding control agent according to 100 parts by weight of foaming layer matrix resin; mix interlayer compatibility agent into non-foaming layer raw material and stir evenly. S2 layered melt extrusion: foamed layer extrusion with segmented temperature control: low temperature plasticizing 150-170℃, side feeding of all modified auxiliary materials 155-175℃, medium temperature crosslinking 170-190℃, auxiliary material blending 200-230℃, melt homogenization 170-190℃; non-foamed layer screw independent melting. S3 high-pressure injection of physical foaming agent, followed by static mixing to obtain gas-containing melt; S4 In-mold Composite: Each layer of melt is fed into a multi-layer independent temperature-controlled coat hanger mold for melt composite; mold temperature 110~130℃; S5 Cooling and Shaping: After exiting the die head, the material is cooled, shaped, and wound up by a pressure roller at 110-160℃ and 60-80℃.

[0025] The multi-layer coat hanger mold of the present invention includes multiple sets of independent feeding channels and a die head discharge section; the mold is equipped with ≥3 sets of independent temperature-controlled feeding channels, and a semi-tube-shaped confluence groove is provided at the bottom, where the material flow of each layer converges into the groove to complete the melting and composite; the slope and turning angle R of the coat hanger channel are adjustable, and the mold can be expanded to have multiple feeding channels.

[0026] In this invention, an interlayer compatibility additive is pre-mixed into the non-foamed layer raw material. After the surface layer melts, it enters a multi-layer hanger mold. During the high-temperature melting and blending stage in the semi-pipe manifold groove, the molecular chains of the compatibility additive migrate to the interface between the two phases. The polyolefin segments of the compatibility additive are compatible with the foamed layer PE / PET / EVA / GPPS, and the acid anhydride active groups react with the hydroxyl groups at the resin end of the foamed layer to form interfacial bonding forces. The applicant found that the amount of interlayer compatibility additive added in this system needs to be strictly controlled at 3-5 wt% of the total composite material mass: below 3 wt%, the interfacial compatibility component is insufficient, resulting in low interlayer peel strength and easy delamination; above 5 wt%, it will cause an excessive difference in melt viscosity between the foamed layer and the non-foamed layer, resulting in wavy lines, warping, and uneven layer thickness in the sheet. This process premixes the compatibility agent in the surface layer and co-extrudes it simultaneously, without the need for an additional coating process. The interface compatibility is completed in situ by in-mold melting, and the interlayer bonding strength is much higher than that of the subsequent cold coating process.

[0027] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention constructs a synergistic system from the formulation stage, consisting of an organic peroxide-polyfunctional acrylate monomer-co-crosslinking agent ternary crosslinking branching system, a filler modifier, a foaming agent, a molding regulator, and an interlayer compatibilizer. This system significantly improves the high-temperature tensile strength of the melt at the microscopic level. During the physical foaming and depressurization process of CO2 / butane, the bubble walls are less prone to tearing and bubbles do not merge, resulting in stable micron-sized closed micropores with uniform pore size, free from visible large voids and pinhole defects. It also significantly widens the processing window, avoiding the problems of extrusion breakage and die carbon buildup associated with single peroxide systems. The foaming ratio is adjustable over a wider range, adapting to the needs of different cushioning and insulation products.

[0028] 2. The preparation process of this invention involves two independently premixed systems: the foamed layer is uniformly mixed with crosslinking, fillers, intralayer compatibility agents, and antioxidant lubricants; the interlayer compatibility agents are pre-uniformly mixed into the non-foamed surface layer to ensure uniform dispersion of the compatibility agents and provide sufficient active components for the intramold interface reaction. Five-stage gradient temperature control precisely controls the reaction sequence: low-temperature plasticizing avoids premature decomposition of peroxides; side feeding simultaneously adds all modified excipients, ensuring thorough shear mixing; the medium-temperature crosslinking stage precisely controls the degree of free radical crosslinking and branching reaction; high-temperature homogenization eliminates uneven component concentrations, allowing the ternary modified system and the filler compatibility system to react fully, significantly improving batch performance consistency.

[0029] 3. In-situ compatibilization in the mold replaces the traditional cold lamination process: In the molten state, the compatibilizer spontaneously migrates to the interface between the two phases and undergoes interfacial bonding, eliminating the need for secondary lamination equipment, shortening the production line, reducing labor and equipment costs, and the interlayer bonding strength is much higher than that of the solid cold lamination process. Detailed Implementation

[0030] The present invention will be described below with reference to specific implementation schemes. It should be noted that the following embodiments are examples of the present invention and are used only to illustrate the invention, not to limit it. Other combinations and various modifications within the scope of the present invention can be made without departing from its spirit or scope. It is worth noting that, unless otherwise specified, the raw materials used in the following preparation examples and embodiments are all from any commercially available manufacturer.

[0031] The specific manufacturers and models of the raw materials used in the following examples and comparative examples are as follows: PE: Dow LLDPE 2045G (extrusion grade) PP: Sinopec Zhenhai Refining & Chemical, PP T30S general-purpose grade for fiber drawing / co-extrusion EVA: Formosa Plastics EVA UE3330 (VA content 18%) GPPS: Formosa Plastics GPPS GP535N PE-g-MAH: Dow Fusabond, Model MN493D PP-g-MAH: Arkema Orevac RV418 EVA-g-MAH: Ningbo Nengguang CMG202 PA6: BASF B3S extrusion modified general grade PA12: Arkema Rilsamid AESNO TL EMA: Arkema Lotryl AC 1225 Nano-silica: Wacker HDK N20 fumed silica Montmorillonite: Zhejiang Fenghong Organic Modified Montmorillonite DK2 Polyethylene wax: Clariant Licowax PE520 Hydrogenated petroleum resin: Eastman C80 The above raw material models are for illustrative purposes only. Those skilled in the art can select similar products from other manufacturers based on actual performance requirements.

[0032] Example 1 A multilayer physically foamed co-extruded material, comprising a PE foam layer and a PP non-foamed layer; The raw material for the PE foam layer is: 100 parts by weight of PE. Melt strength modifier: 0.5 parts dicumyl peroxide, 1 part trimethylolpropane triacrylate, 2 parts triallyl isocyanurate; Filler and modifier: 1.5 parts nano silica, 1.5 parts montmorillonite, 4 parts PA6, 2.5 parts EVA-g-MAH; Foaming aids: 0.3 parts zinc stearate, 0.8 parts polyethylene wax; 0.3 parts antioxidant 1010, 0.6 parts antioxidant 168; Molding control agent: 0.8 parts of hydrogenated petroleum resin.

[0033] Raw materials for the non-foamed PP layer: by weight, 100 parts PP, 0.6 parts oleamide; The interlayer compatibility additive is PP-g-MAH, and the amount added is 4wt% of the total mass of the foamed layer and the non-foamed layer.

[0034] The preparation process of the multilayer physically foamed co-extruded material in this embodiment includes the following steps: S1 Material Premixing: Mix all the raw materials for the foaming layer at 500 rpm for 10 minutes according to the above ratio; mix the non-foaming layer raw materials PP, PP-g-MAH, and oleic acid amide evenly. S2 layered melt extrusion: Foamed layer extrusion with segmented temperature control: low temperature plasticizing 160℃, side feeding of all modified auxiliary materials 170℃, medium temperature crosslinking 180℃ (hold for 60s), auxiliary material blending 210℃ (hold for 30s), melt homogenization 180℃; screw speed 60rpm; non-foamed layer melt extrusion 190℃. S3 high pressure (12MPa) injection of physical foaming agent CO2, the injection amount is 3wt% of the melt mass, and gas-containing melt is obtained by static mixing; S4 In-mold Composite: Each layer of melt is fed into its own flow channel in a multi-layer independent temperature-controlled coat hanger mold, and the two-phase interface in-situ compatibilization composite is completed in the molten state; mold temperature 120℃; S5 Cooling and Shaping: After the material exits from the die head, it is cooled, shaped, and wound up by a 130°C die section and a 70°C pressure roller.

[0035] Example 2 A multilayer physically foamed co-extruded material, comprising an EVA foam layer and a PE non-foamed layer; The raw material for the EVA foam layer is: 100 parts by weight of EVA. Melt strength modifier: 0.4 parts dicumyl peroxide, 0.9 parts trimethylolpropane triacrylate, and 1.8 parts triallyl isocyanurate; Filler and modifier: 1.2 parts nano silica, 1.2 parts montmorillonite, 4 parts PA12, 2.2 parts EVA-g-MAH; Foaming aids: 0.25 parts zinc stearate, 0.7 parts polyethylene wax; 0.25 parts antioxidant 1010, 0.5 parts antioxidant 168; Molding control agent: 0.7 parts of hydrogenated petroleum resin.

[0036] Raw material for the non-foamed PE layer: 100 parts by weight of PE; The interlayer compatibility additive is PE-g-MAH, and the addition amount is 3.5wt% of the total mass of the foamed layer and the non-foamed layer.

[0037] The preparation process of the multilayer physically foamed co-extruded material in this embodiment includes the following steps: S1 Material Premixing: Mix and stir all raw materials for the foaming layer according to the above ratio for 10 minutes; mix and stir the non-foaming layer raw materials PE and PE-g-MAH evenly. S2 layered melt extrusion: Foamed layer extrusion with segmented temperature control: low temperature plasticizing 155℃, side feeding of all modified auxiliary materials 165℃, medium temperature crosslinking 175℃ (hold for 60s), auxiliary material blending 205℃ (hold for 30s), melt homogenization 180℃; screw speed 60rpm; non-foamed layer melt extrusion 190℃. S3 high pressure (10MPa) injection of physical foaming agent CO2, the injection amount is 2.5wt% of the melt mass, and the gas-containing melt is obtained by static mixing; S4 In-mold Composite: Each layer of melt is fed into its own flow channel in a multi-layer independent temperature-controlled coat hanger mold, and the two-phase interface in-situ compatibilization composite is completed in the molten state; mold temperature 120℃; S5 Cooling and Shaping: After exiting the die head, the material is cooled, shaped, and wound up by a 130℃ die back section and a 65℃ pressure roller.

[0038] Example 3 A multilayer physical foam co-extruded material includes two non-foamed PE layers and a middle foamed PE core layer; the thickness of a single non-foamed PE layer is 0.8 mm, and the thickness of the middle foamed PE core layer is 8.4 mm.

[0039] The raw material for the PE foam layer is: 100 parts by weight of PE. Melt strength modifier: 0.6 parts dicumyl peroxide, 1.2 parts trimethylolpropane triacrylate, and 2.2 parts triallyl isocyanurate; Filler and modifier: 1.5 parts nano silica, 1.5 parts montmorillonite, 4 parts PA6, 2.5 parts EVA-g-MAH; Foaming aids: 0.4 parts zinc stearate, 0.9 parts polyethylene wax; 0.35 parts antioxidant 1010, 0.7 parts antioxidant 168; Molding control agent: 0.9 parts of hydrogenated petroleum resin.

[0040] Raw material for the non-foamed PE layer: 100 parts by weight of PE; The interlayer compatibility additive is PE-g-MAH, and the addition amount is 3.5wt% of the total mass of the three-layer composite material. It is uniformly mixed into the two non-foamed PE layers. The preparation process of the multilayer physically foamed co-extruded material in this embodiment includes the following steps: S1 Material Premixing: Mix and stir all raw materials for the foaming layer according to the above ratio for 10 minutes; mix and stir the non-foaming layer raw materials PE and PE-g-MAH evenly. S2 layered melt extrusion: Foamed layer extrusion with segmented temperature control: low temperature plasticizing 160℃, side feeding of all modified auxiliary materials 170℃, medium temperature crosslinking 185℃ (residence time 60s), auxiliary material blending 210℃ (residence time 30s), melt homogenization 185℃; screw speed 60rpm; non-foamed layer melt extrusion 190℃. S3 high pressure (13MPa) injection of physical foaming agent CO2, the injection amount is 3.5wt% of the melt mass, and the gas-containing melt is obtained by static mixing; S4 In-mold Composite: The melt of the non-foamed layer is divided into two equal parts, which are used as the upper and lower surface melts respectively. They are simultaneously fed into a three-layer independent temperature-controlled coat hanger mold along with the gas-containing melt. The three-phase interface in-situ compatibilization composite is completed in the molten state; the mold temperature is 130℃. S5 Cooling and Shaping: After exiting the die head, the material is cooled, shaped, and wound up by a 130℃ die back section and a 65℃ pressure roller.

[0041] Example 4 This embodiment provides a multilayer physical foaming co-extrusion material and its preparation process. The specific implementation method is roughly the same as that in Embodiment 1, except that PA6 is replaced by an equal mass fraction of EMA.

[0042] Example 5 This embodiment provides a multilayer physical foaming co-extrusion material and its preparation process. The specific implementation method is roughly the same as that in Embodiment 1, except that EVA-g-MAH is not added.

[0043] Example 6 This embodiment provides a multilayer physical foaming co-extrusion material and its preparation process. The specific implementation method is roughly the same as that in Embodiment 1, except that the amount of interlayer compatibility additive added is 2wt% of the total mass of the foamed layer and the non-foamed layer.

[0044] Example 7 This embodiment provides a multilayer physical foaming co-extrusion material and its preparation process. The specific implementation method is roughly the same as that in Embodiment 1, except that the amount of interlayer compatibility additive added is 6wt% of the total mass of the foamed layer and the non-foamed layer.

[0045] Comparative Example 1 The specific implementation method of this comparative example is roughly the same as that of Example 1, except that no filler or modifying agent is added.

[0046] Comparative Example 2 The specific implementation method of this comparative example is roughly the same as that of Example 1, except that the melt strength modifier is 0.5 parts of dicumyl peroxide.

[0047] Performance testing The composite materials obtained in each embodiment and comparative example were tested as follows, and the results are shown in Table 1: 1. Foam quality Test method: The foamed layer cross section was cut using a cryostat and observed by SEM. The diameter of 200 cells was counted from 5 randomly selected fields of view and the average value was calculated. The presence of connected broken cells and large collapsed cavities was determined by visual inspection and electron microscopy.

[0048] Judgment criteria: No broken bubbles = no interconnected pores in the field of view, no super-large pores >10μm; a small number / large number of broken bubbles are marked with visual observations.

[0049] 2. Interlayer peel strength (N / 15mm) Implementation standard: GB / T 2790-2017 Adhesives 180° peel strength test Sample: Cut a 15mm wide composite sheet, stretch it at a universal tensile testing machine at a rate of 50mm / min, and record the average force value during the stable peeling stage.

[0050] 3. Sheet warpage Test method: Take a 300mm×300mm flat sample and place it flat on a standard glass plate, then measure the maximum height of the four corners that warp up. Grading: No warping (warping < 0.5 mm), slight warping (0.5–2 mm), severe wavy warping (> 2 mm).

[0051] 4. Surface defect judgment Visual inspection + 40x magnification: Check for white spots, streaks, pits, and blooming on the mold head.

[0052] 5. Compression rebound rate (%) Standard: GB / T 6669-2001 Modified Test for Compression Permanent Deformation of Flexible Foam The sample thickness is 10mm. It is compressed by 50%, held for 30 minutes, and then allowed to stand for 30 minutes after decompression. The thickness is measured, and the rebound rate is calculated as: (thickness after rebound / original thickness) × 100%.

[0053] 6. Stability during extrusion processing Extrude continuously for 30 minutes and record whether there is strip breakage, carbon buildup on the die head, or drastic torque fluctuations.

[0054] Table 1

[0055] As can be seen from the data in Table 1, the composite material of Example 1 has excellent comprehensive performance, with regular and uniform cell structure; high interlayer peel strength; no warping; no filler agglomeration white spots or longitudinal stripes on the surface of the product, and a smooth surface; compression rebound rate of up to 86%; and uniform and stable continuous extrusion output with no broken strips or obvious die head accumulation.

[0056] Example 2 showed only a few tiny irregular bubbles, with no broken bubbles or collapse; the interlayer peel strength was 12.9 N / 15 mm; there was a slight difference in the shrinkage rate between PE and EVA, and the sample was slightly warped; there were no white spots, only slight haze caused by a small amount of lubricant migration, and no surface blooming; the compression rebound rate was 83%; the extrusion process was stable, with only a small amount of material accumulation at the die head.

[0057] Example 3 showed no large-area collapse or interconnected large air bubbles; the peel strength values ​​of the upper and lower layers were basically the same, proving that PE-g-MAH was uniformly dispersed on both sides of the PE surface layer and the bonding effect of the upper and lower interfaces was balanced; the sample had no warping; no white spots or streaks; the compression rebound rate was 82%; the extrusion was continuous without broken strips and there was a small amount of material accumulation at the die head.

[0058] Compared to Example 1, Example 4, which replaced PA6 with EMA, showed lower peel strength and resilience than Example 1 due to the lack of rigid support from hydrogen bonds in nylon molecules. EMA and EVA-g-MAH also showed good compatibility, and the filler did not agglomerate, proving that the polar reinforcing phase is replaceable.

[0059] Compared to Example 1, Example 5 did not include an intralayer compatibilizer, resulting in an increased average cell diameter, numerous large cells, and localized collapse; the interlayer peel strength was only 8.3 N / 15 mm; the sheet was covered with white filler agglomeration streaks and localized unevenness; the compression rebound rate was 62%; and the screw torque fluctuated drastically, with inconsistent discharge speeds. The possible reasons are that the nano-silica, montmorillonite, and PA6 in the foaming layer are all highly polar components, resulting in extremely high interfacial tension with the non-polar PE matrix. Without EVA-g-MAH bridging, the filler agglomerates severely, forming visible white spots; a large amount of foaming gas escapes from the interphase interface gaps, leading to significant differences in cell size and a decline in mechanical properties.

[0060] Compared to Example 1, Examples 6-7 all showed varying degrees of performance degradation. The possible reasons are: insufficient addition of interlayer compatibilizer, limited number of active anhydride groups enriched at the interface between the two phases, inability to form a stable intermolecular bonding layer, and a significant decrease in interlayer peel strength, which cannot meet the requirements for use in multilayer composite products; while excessive PP-g-MAH significantly widened the melt viscosity difference between the PP non-foamed layer and the PE foamed layer, resulting in asynchronous flow rates of the two layers during in-mold co-extrusion, generating huge internal stress after cooling, forming wavy warping and thickness fluctuation defects; although the interfacial bonding strength was acceptable, the appearance was substandard and could not be mass-produced.

[0061] Comparative Example 1 showed that the absence of filler modifiers resulted in a deterioration in appearance, mechanical properties, and processing performance. This was because the absence of PA6 and nanofillers led to a lack of heterogeneous nucleation sites and rigid microphase support, resulting in larger cell size and a significant decrease in resilience. While the absence of fillers did not cause agglomeration defects, the heat resistance, wear resistance, and cushioning performance of the foamed layer were greatly reduced, failing to meet the requirements of high-end applications.

[0062] Comparative Example 2, using only a single DCP, resulted in larger average cell size, bubble breakage and collapse, reduced interlayer peel strength, severe carbon buildup on the die, decreased compression rebound rate, and frequent breakage during continuous extrusion, leading to poor processing performance. This may be due to the single peroxide crosslinking, which easily leads to severe crosslinking, causing a sharp drop in melt flowability and an extremely narrow extrusion processing window; the lack of TMPTA long-chain entanglement and TAIC crosslinking synergists resulted in insufficient melt strain hardening capacity, and the bubble walls could not be supported during CO2 foaming and depressurization, leading to extensive tearing and merging to form ultra-large pores; at the same time, free radicals easily cause molecular chain breakage and degradation, resulting in simultaneous deterioration of mechanical and processing properties.

[0063] The embodiments and comparative examples described above do not limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A multi-layer physically foamed co-extruded material, characterized in that, It includes at least one foamed layer and at least one non-foamed layer, wherein the base resin of the foamed layer includes at least one of PE, PET, EVA, and GPPS, and the base resin of the non-foamed layer includes PP or PE. The raw materials for the foamed layer include a matrix resin and functional additives, wherein the functional additives include melt strength modifiers, filler modifiers, foaming aids, and molding control aids. Based on 100 parts by weight of the foaming layer matrix resin, the melt strength modifying agent includes: 0.2-1 parts of organic peroxide crosslinking agent, 0.3-2 parts of polyfunctional acrylate branched monomer, and 1-3 parts of crosslinking activator.

2. The multi-layer physically foamed co-extruded material according to claim 1, characterized in that, The organic peroxide crosslinking agent includes at least one of dicumyl peroxide, di-tert-butyl peroxide, and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.

3. The multi-layer physically foamed co-extruded material according to claim 1, characterized in that, The multifunctional acrylate branched monomer is selected from at least one of trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and ethylene glycol dimethacrylate.

4. The multi-layer physically foamed co-extruded material according to claim 1, characterized in that, The crosslinking activator includes triallyl isocyanurate and / or diallyl phthalate.

5. The multi-layer physically foamed co-extruded material according to claim 1, characterized in that, The raw materials of the co-extruded material also include an interlayer compatibility agent, which is maleic anhydride-grafted polyolefin. The interlayer compatibility agent is pre-mixed into the non-foamed layer, and the amount of interlayer compatibility agent added is 3-5 wt% based on the total mass of the foamed layer and the non-foamed layer.

6. The multi-layer physically foamed co-extruded material according to claim 1, characterized in that, The foaming agent includes a lubricant and / or an antioxidant; the lubricant includes at least one of stearic acid, zinc stearate, polyethylene wax, and oxidized polyethylene wax; the antioxidant includes hindered phenolic primary antioxidant and phosphite secondary antioxidant.

7. The multilayer physically foamed co-extruded material according to claim 1, characterized in that, The filler modification agent includes inorganic fillers, polymeric reinforcing phases, and intralayer compatibilizers; the inorganic fillers include at least one of talc, calcium carbonate, silica, and mica powder; the polymeric reinforcing phase includes at least one of PA6, PA12, and EMA.

8. The multilayer physically foamed co-extruded material according to claim 1, characterized in that, The molding control aid contains 0.2 to 1.5 parts of viscosity modifier; the viscosity modifier includes one or more of low melt index LDPE, PP wax, hydrogenated petroleum resin, and terpene resin.

9. The multilayer physically foamed co-extruded material according to claim 1, characterized in that, 0 to 1.0 parts by weight of a retarding crystallization aid are added to 100 parts of the non-foamed matrix resin; the retarding crystallization aid is an aliphatic amide or random polyα-olefin.

10. A preparation process for a multilayer physically foamed co-extruded material according to any one of claims 1-9, characterized in that, Includes the following steps: S1 Material Premixing: Mix melt strength modifier, filler modifier, foaming agent, and molding control agent according to 100 parts by weight of foaming layer matrix resin; mix interlayer compatibility agent into non-foaming layer raw material and stir evenly. S2 layered melt extrusion: foamed layer extrusion with segmented temperature control: low temperature plasticizing 150-170℃, side feeding of all modified auxiliary materials 155-175℃, medium temperature crosslinking 170-190℃, auxiliary material blending 200-230℃, melt homogenization 170-190℃; non-foamed layer screw independent melting. S3 high-pressure injection of physical foaming agent, followed by static mixing to obtain gas-containing melt; S4 In-mold Composite: Each layer of melt is fed into a multi-layer independent temperature-controlled coat hanger mold for melt composite; mold temperature 110~130℃; S5 Cooling and Shaping: After exiting the die head, the material is cooled, shaped, and wound up by a pressure roller at 110-160℃ and 60-80℃.