A method for preparing a metal-ceramic composite craft and the craft itself.
By pre-reserving process gaps in ceramic-metal composites and filling them with molten metal for welding, combined with additive manufacturing and multiple filling and sintering of low-temperature glazes, the problem of thermal stress concentration caused by the difference in thermal expansion coefficients during high-temperature sintering of metal-ceramic composites is solved. This achieves efficient and reliable connection and integrated decoration, improving yield and appearance quality.
Patent Information
- Application Number
- CN202611590125.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-14
- Publication Date
- 2026-11-17
AI Technical Summary
During the high-temperature sintering process of metal-ceramic composite materials, the difference in thermal expansion coefficients leads to thermal stress concentration, which causes ceramic cracking or connection and sealing failure. At the same time, traditional surface decoration processes are inefficient and the substrate is prone to oxidation and deformation, affecting the yield and appearance quality.
By reserving process gaps and filling them with molten metal for welding and sealing, combined with additive manufacturing and multiple filling and sintering of low-temperature glaze, a stress-buffered connection and an integrally formed decorative skeleton are formed to avoid high-temperature oxidation deformation.
It effectively releases thermal stress, ensures connection reliability, reduces costs, improves yield and decorative quality, and achieves reliable composite of heterogeneous materials and integrated surface decoration.
Smart Images

Figure CN123104272A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of craft preparation technology, and in particular to a method for preparing a metal-ceramic composite craft and the craft itself. Background Technology
[0002] In the field of craft manufacturing, metal-ceramic composites combine the strength of metal with the corrosion resistance and easy cleaning properties of ceramics. However, due to the significant difference in the coefficients of thermal expansion between metal and ceramic, the interface between the two is prone to generating enormous thermal stress during high-temperature sintering in the manufacturing process or under temperature changes in the subsequent use environment, leading to ceramic cracking or failure of the connection seal. Furthermore, to enhance the surface decoration effect of crafts, traditional techniques often employ manual filigree to construct the surface texture framework and fill it with glaze. This method not only relies on manual experience, has low production efficiency, and is costly, but also, during the high-temperature firing process after glazing, the metal substrate is prone to oxidation or thermal deformation due to prolonged exposure to high temperatures, severely affecting the yield and appearance quality. Therefore, there is an urgent need to develop a manufacturing method that can effectively release the thermal stress of dissimilar materials, ensure connection reliability, and simultaneously achieve low-cost, one-piece molding of the surface decoration framework while avoiding thermal deformation of the substrate. Summary of the Invention
[0003] The technical problem to be solved by the present invention is to overcome the defects of the existing technology. The present invention proposes a method for preparing metal and ceramic composite crafts and the crafts themselves.
[0004] To solve the aforementioned technical problems, the technical solution adopted by the present invention is as follows: A method for preparing a metal-ceramic composite craft includes: placing a ceramic inner liner into the inner cavity of a metal outer shell, leaving a process gap at the mating part between the ceramic inner liner and the metal outer shell, filling the process gap with molten metal and welding it to seal it; integrally forming a metal decorative skeleton on the surface of the metal outer shell; filling the gaps in the metal decorative skeleton with a low-temperature glaze, and subjecting the low-temperature glaze to multiple filling and sintering processes.
[0005] In one embodiment, the mating part between the ceramic inner liner and the metal outer shell adopts a mechanical interlocking structure; the molten metal is a copper-based molten metal.
[0006] In one embodiment, the mechanical interlocking structure is a dovetail-shaped fit structure, and the outer wall of the ceramic inner liner is provided with an outwardly protruding tooth structure to form the dovetail-shaped fit structure; the top inner wall of the ceramic inner liner is provided with an anti-overflow protrusion, and the height of the anti-overflow protrusion is 1-1.5mm.
[0007] In one embodiment, a metal decorative skeleton is integrally formed on the surface of the metal shell, including: integrally forming the metal decorative skeleton on the surface of the metal shell by using an additive manufacturing sacrificial mold combined with a lost-wax casting process; and performing multiple filling and sintering treatments on the low-temperature glaze, including: filling the low-temperature glaze in stages and performing secondary sintering at corresponding temperatures in a low-temperature range lower than the oxidation deformation temperature of the metal shell.
[0008] In one embodiment, the additive manufacturing sacrificial mold is a 3D printed wax film; the temperature of the low-temperature range is 720-780℃, and the holding time for each sintering is 3-5 minutes; the number of filling operations is 2-4 times.
[0009] In one embodiment, the low-temperature glaze is mainly composed of quartz, borax and feldspar, with zinc oxide or borate added as flux, and is combined with metal oxide colorants. The low-temperature glaze has no high-melting-point hard components.
[0010] In one embodiment, the ceramic inner liner is placed into the inner cavity of the metal outer shell, including: finely adjusting the height of the ceramic inner liner by passing a bottom fixing post through the central hole at the bottom of the metal outer shell and abutting against the bottom surface of the ceramic inner liner.
[0011] In one embodiment, the bottom fixing post is threadedly connected to the metal shell, and threadlocker is applied to the threads; a silicone gasket is installed between the head of the bottom fixing post and the bottom surface of the metal shell, and one side of the silicone gasket is provided with an adhesive layer.
[0012] As one implementation method, after obtaining the metal and ceramic composite craft, the process further includes: sequentially performing degreasing and dust removal, low-temperature baking and dehumidification, surface activation and wiping, high-temperature firing and hot coloring, and pigment painting; and spraying the entire surface with colorless, transparent, high-hardness, wear-resistant nano paint for surface sealing treatment.
[0013] This application also provides a metal and ceramic composite craft, comprising: a metal shell; a ceramic inner liner housed in the inner cavity of the metal shell, wherein a process gap is reserved at the mating part between the ceramic inner liner and the metal shell, and the process gap is filled with a weld formed by molten metal; a metal decorative frame integrally formed on the surface of the metal shell; and a low-temperature glaze sintering layer filling the gap of the metal decorative frame.
[0014] Compared with the prior art, the beneficial effects of the present invention are: This invention utilizes a pre-existing process gap at the interface between the ceramic inner liner and the metal outer shell, filled with molten metal during welding. This pre-existing process gap acts as a buffer space for thermal expansion stress, effectively absorbing the deformation and displacement caused by the difference in thermal expansion coefficients between the two dissimilar materials. This avoids ceramic cracking or sealing failure caused by direct rigid connection. At the same time, the weld formed by the molten metal ensures an airtight connection between the ceramic inner liner and the metal outer shell, guaranteeing the water-holding function and structural stability of the container-type crafts.
[0015] Furthermore, this invention integrates a metal decorative skeleton onto the surface of a metal shell by using additive manufacturing sacrificial molds combined with lost-wax casting, replacing the traditional hand-wired process. This significantly reduces the molding cost and production cycle of complex texture structures and improves product consistency. In addition, multiple filling and sintering processes are performed in a low-temperature range below the oxidation and deformation temperature of the metal shell, which ensures the full melting, leveling and densification of the low-temperature glaze, while avoiding oxidation, deformation or coarse grain problems caused by prolonged high-temperature heating of the metal substrate, thus improving the yield and surface decoration quality. Attached Figure Description
[0016] The disclosure of this invention is illustrated with reference to the accompanying drawings. It should be understood that the drawings are for illustrative purposes only and are not intended to limit the scope of protection of this invention. In the drawings, the same reference numerals are used to refer to the same parts. Wherein: Figure 1 These are top and cross-sectional schematic diagrams of metal and ceramic composite handicrafts according to embodiments of this application; Figure 2 This is a detailed drawing of the ceramic inner liner structure and dovetail joint of an embodiment of this application; Figure 3 This is a top view and cross-sectional detail diagram of the metal decorative frame according to an embodiment of this application; Figure 4 This is an exploded view of the ceramic inner liner and metal outer shell assembly according to an embodiment of this application; Figure 5 This is a schematic diagram of the tenon and mortise fit and copper fusion welding sealing structure according to an embodiment of this application; Figure 6 This is a schematic diagram of the welding and texture layout of the metal decorative skeleton according to an embodiment of this application.
[0017] Reference numerals: 1. Metal decorative frame; 2. Ceramic inner liner; 3. Metal outer shell; 4. Bottom fixing post; 5. Silicone gasket. Detailed Implementation
[0018] It is readily understood that, based on the technical solution of this invention, those skilled in the art can propose various interchangeable structural methods and implementations without altering the essential spirit of the invention. Therefore, the following detailed embodiments and accompanying drawings are merely illustrative examples of the technical solution of this invention and should not be considered as the entirety of the invention or as limitations or restrictions on the technical solution of this invention.
[0019] Specific embodiments of the present invention are described below with reference to the accompanying drawings.
[0020] Example 1
[0021] like Figure 1 and Figure 5 As shown, this embodiment provides a method for preparing metal-ceramic composite handicrafts. This method aims to solve the problems of thermal stress concentration at the interface of heterogeneous materials, complex surface decoration processes, and easy thermal deformation of the substrate. The preparation method mainly includes the following steps: Step S100: Place the ceramic inner liner 2 into the inner cavity of the metal outer shell 3, leave a process gap at the mating part between the ceramic inner liner 2 and the metal outer shell 3, and fill the process gap with molten metal for welding and sealing.
[0022] Specifically, due to the significant difference in the coefficients of thermal expansion between ceramic and metal materials, if rigid direct contact or interference fit is used, the interface is prone to generating huge thermal stress due to deformation mismatch during subsequent high-temperature processing or changes in ambient temperature, leading to ceramic cracking or connection failure. Therefore, the process gap reserved in this step is not simply an assembly tolerance clearance, but is configured as a thermal expansion stress buffer cavity to accommodate and release the relative displacement generated by the two materials during heating. After reserving this buffer space, a highly fluid molten metal is used to fill the process gap. After the molten metal cools and solidifies, it forms a dense weld, which not only achieves structural fixation between the ceramic inner liner 2 and the metal outer shell 3, but also ensures the airtightness and watertightness required for container-type crafts. It should be understood that although this embodiment uses a vase-type container as an example, this connection method is also applicable to other composite craft structures that require sealing or load-bearing, such as tea sets and incense burners.
[0023] Step S200: The metal decorative frame 1 is integrally formed on the surface of the metal shell 3.
[0024] Specifically, the metal decorative skeleton 1 constitutes the texture base and glaze support structure of the product surface. Unlike traditional processes that construct surface textures through manual wire cutting and welding, this embodiment uses a one-piece molding method to directly generate the metal decorative skeleton 1 on the surface of the metal shell 3. This integral structure eliminates the numerous weld points and seams present in traditional splicing processes, not only improving the overall strength and dimensional accuracy of the structure but also avoiding the degradation of substrate performance or appearance defects caused by localized heat-affected zones from welding. Simultaneously, the one-piece molded metal decorative skeleton 1 can form a continuous material bonding interface with the metal shell 3, providing a reliable physical basis for the stable adhesion of the subsequent glaze.
[0025] In step S300, low-temperature glaze is filled into the gaps of the metal decorative frame 1, and the low-temperature glaze is subjected to multiple filling and sintering processes.
[0026] Specifically, to ensure glaze quality while avoiding damage to the metal substrate, this step employs a unique process strategy that differs from traditional single-stage high-temperature firing. Firstly, a low-temperature glaze with a lower melting temperature is selected, allowing it to melt and flow below the oxidation deformation temperature of the metal outer shell. This avoids the oxidation, grain coarsening, or plastic deformation problems that can occur in the metal substrate due to prolonged exposure to high temperatures. Secondly, to address the potential volume shrinkage and surface collapse that may occur during the sintering process of the low-temperature glaze, a cyclical treatment method combining layer-by-layer filling and corresponding sintering is adopted. By repeatedly filling the glaze layer by layer and performing heat treatment, defects such as bubbles, pinholes, and unevenness caused by a single thick coating are gradually eliminated, ultimately resulting in a dense and smooth glaze layer flush with the top of the metal decorative framework 1. This process design balances the need for glaze densification with the thermal sensitivity of the metal substrate, improving the product's yield and appearance quality.
[0027] Through the coordinated operation of steps S100 to S300 above, this embodiment constructs a complete framework for the preparation of metal and ceramic composite crafts. Without relying on specific material types or specific microstructures, it establishes a general process route with stress buffer connection, integral skeleton structure and low-temperature cyclic glazing as the core, providing higher-level support for the refinement of subsequent specific implementation methods.
[0028] Example 2
[0029] Based on Example 1, this example further specifies the structure and filling material of the mating part between the ceramic inner liner 2 and the metal outer shell 3. As one embodiment, the mating part between the ceramic inner liner 2 and the metal outer shell 3 adopts a mechanical interlocking structure, and the molten metal is a copper-based molten metal.
[0030] Specifically, such as Figure 2 and Figure 5As shown, the aforementioned mechanical interlocking structure is preferably a dovetail-shaped fit structure. A toothed structure protruding outwards is provided on the circumferential outer wall of the ceramic inner liner 2. This toothed structure engages with a corresponding groove pre-set on the inner wall of the metal outer shell 3, together forming a dovetail-shaped fit interface. This non-planar geometric interlocking design has dual technical benefits: firstly, axially, the sidewall of the toothed structure and the inner wall of the groove form an abutment surface, effectively limiting axial movement or dislodgement of the ceramic inner liner 2 relative to the metal outer shell 3, ensuring the accuracy and stability of the assembly position; secondly, radially, the inclined fit of the dovetail structure allows for slight relative slippage along the inclined direction during thermal expansion, thereby converting the originally destructive tensile stress perpendicular to the interface into a shear component along the inclined surface. Combined with the process gap reserved in Example 1, this further releases the interface stress caused by the difference in thermal expansion coefficients between ceramic and metal, reducing the risk of ceramic cracking. It should be understood that although this embodiment uses a dovetail structure as an example, in other embodiments, T-slots, sawtooth shapes, or other irregular cross-sectional structures that can achieve bidirectional limiting can also be used, as long as they can provide the degree of freedom to adapt to thermal deformation and maintain the structural connection strength.
[0031] Furthermore, to prevent molten metal from overflowing and contaminating the product appearance or affecting assembly accuracy in subsequent processes, the top inner wall of the ceramic inner liner 2 is provided with an anti-overflow protrusion, the height of which is 1-1.5mm. For example... Figure 2 As shown in the enlarged view of detail B, the anti-overflow protrusion extends continuously along the edge of the top opening of the ceramic inner liner 2, forming a ring-shaped physical barrier. During the process of filling the gaps in the molten metal filling process, the liquid metal may rise or flow upwards due to capillary action or gravity. When the liquid level rises to the position of the anti-overflow protrusion, the sidewall of the protrusion will block the further spread of the liquid, confining it within the predetermined welding area. Limiting the height to the range of 1-1.5mm is an optimized value derived from process verification: if the height is less than 1mm, it is difficult to effectively block the copper-based molten metal with high surface tension, and overflow is likely to occur; if the height exceeds 1.5mm, it will excessively occupy the effective volume of the inner liner and may cause interference when installing the subsequent metal decorative frame 1. In addition, the corners of the anti-overflow protrusion preferably adopt a rounded transition to avoid stress concentration that could lead to chipping of the ceramic edge.
[0032] Regarding the selection of filler material, in this embodiment, the preferred metal melt is a copper-based melt. Compared to pure copper or other metal solders, copper-based melts (such as copper-phosphorus brazing filler metal or copper-zinc alloy) exhibit excellent wettability and spreading ability on both the metallization layer on the ceramic surface and the metal outer shell substrate 3. This allows for thorough filling within narrow process gaps, forming a dense, non-porous weld. Simultaneously, the moderate melting point of copper-based melts ensures fluidity during welding while avoiding thermal shock damage to the ceramic inner liner caused by excessively high heating temperatures. The cooled and solidified copper-based weld also possesses good ductility, serving as a flexible connecting layer to further absorb the thermal deformation differences between dissimilar materials, thereby improving the overall structural reliability and sealing performance of the composite product.
[0033] Example 3
[0034] Based on Example 1, this example further specifies the forming method of the metal decorative skeleton 1 and the sintering process of the low-temperature glaze. As one implementation method, the metal decorative skeleton 1 is integrally formed on the surface of the metal shell 3, including: integrally forming the metal decorative skeleton 1 on the surface of the metal shell 3 using an additive manufacturing sacrificial mold combined with a lost-wax casting process; and performing multiple filling and sintering treatments on the low-temperature glaze, including: filling the low-temperature glaze in stages and performing secondary sintering at corresponding temperatures within a low-temperature range below the oxidation deformation temperature of the metal shell 3.
[0035] Specifically, such as Figure 3 and Figure 6 As shown, the metal decorative skeleton 1 typically contains complex continuous geometric textures (such as meander patterns, lotus scroll patterns, etc.). If traditional manual wire cutting or segmented welding is used for splicing, it is not only inefficient but also prone to stress concentration and appearance defects at the weld points. This embodiment employs an additive manufacturing sacrificial mold combined with lost-wax casting. First, additive manufacturing technology is used to quickly construct a sacrificial mold that perfectly matches the target texture in negative shape. Then, this mold is wrapped around the surface of the metal shell 3 or used as an independent cavity for precision casting, allowing the molten metal to directly fill and form a metal decorative skeleton 1 that is metallurgically bonded to the base material or integrally cast. This integrated molding method completely eliminates splicing seams, ensures the continuity of texture lines and dimensional accuracy, and shortens the manufacturing cycle of complex decorative structures. It should be understood that although this embodiment preferably uses lost-wax casting as the molding method, in other embodiments, other processes that can achieve integrated or quasi-integrated connection between the texture skeleton and the base material, such as electroforming, precision stamping, or laser selective melting, can be selected depending on the complexity of the product structure, as long as they can achieve the purpose of eliminating splicing defects and improving structural integrity.
[0036] Regarding the sintering treatment of low-temperature glazes, this embodiment specifically emphasizes staged filling and secondary sintering within a low-temperature range below the oxidation deformation temperature of the metal outer shell. This is because metal substrates (especially precious metals such as copper and silver) are prone to grain growth, softening deformation, or severe surface oxidation at high temperatures, while traditional high-temperature glazes often require firing temperatures above 900°C, which fundamentally contradicts the thermal stability of the metal substrate. By strictly controlling the sintering temperature below the metal oxidation deformation threshold and adopting a staged thin-layer filling and corresponding temperature cyclic sintering strategy, the problems of bubbles, pinholes, and glaze collapse caused by single thick coating are avoided. Furthermore, it ensures that each layer of glaze can fully melt and level at a suitable temperature and form a stable physicochemical bond with the metal skeleton, thereby maximizing the protection of the structural integrity and surface condition of the metal substrate while ensuring decorative quality.
[0037] Furthermore, as a preferred embodiment, the additive manufacturing sacrificial mold is a 3D printed wax film; the temperature in the low-temperature range is 720-780℃, the holding time for each sintering is 3-5 minutes, and the number of filling operations is 2-4 times.
[0038] Specifically, 3D printed wax films are used as sacrificial molds. Compared with traditional hand-carved wax models or silicone molds, they have extremely high dimensional accuracy and detail reproduction capabilities, and can directly output complex texture structures with micron-level resolution. Moreover, the wax film has very low residual ash content during the degreasing process, effectively avoiding sand holes and inclusion defects on the surface of the casting. Regarding the setting of the sintering process window, the temperature range of 720-780℃ is a critical equilibrium point determined through extensive process verification: when the temperature is below 720℃, the viscosity of the low-temperature glaze is too high and the fluidity is insufficient, making it difficult to completely fill the gaps in the skeleton and achieve densification within a short holding time of 3-5 minutes, which easily leads to a matte glaze surface, orange peel, or poor adhesion to the metal; while when the temperature is above 780℃, although the fluidity of the glaze improves, it is close to or exceeds the recrystallization temperature or oxidation acceleration inflection point of some copper alloy matrices. Under the cumulative effect of long-term or repeated heat treatment, the metal shell 3 may show visible deformation, darkening of color, or decline in mechanical properties. Therefore, 720-780℃ is the optimal operating window that balances the maturity of the glaze and the safety of the matrix.
[0039] Equally crucial is the limitation of 2-4 filling cycles. Low-temperature glazes inevitably shrink in volume during melting and cooling. Attempting to achieve the final thickness with a single filling would result in sink marks far exceeding acceptable depths, easily trapping gas and creating defects. Through 2-4 layer-by-layer filling and sintering, each new layer of glaze covers only minor sink marks on the previous layer's surface. After repeated accumulation and compensation, the final glaze surface can be perfectly flush with the top of the metal decorative frame 1. If fewer than 2 filling cycles are used, the compensation is insufficient to eliminate sink marks, and the flatness cannot meet subsequent polishing requirements. If more than 4 cycles are used, while flatness is further improved, each additional sintering cycle means the metal substrate endures an additional thermal cycle impact, reducing production efficiency and increasing the risk of thermal fatigue damage to the substrate and glaze color deviation. Therefore, 2-4 cycles represent the optimal combination of process parameters that achieves the best balance between quality, efficiency, and substrate protection. It should be understood that the above-mentioned temperature, time and number of times parameters are mainly for copper-based shells and specific low-temperature glaze systems. If aluminum-based or silver-based metals are used or the glaze formula is adjusted, the process window can be shifted accordingly, but the core process concept of being below the oxidation deformation temperature of the substrate and compensating for collapse in stages remains unchanged.
[0040] In addition, as one implementation method, the low-temperature glaze is mainly composed of quartz, borax and feldspar, with zinc oxide or borate added as flux, and combined with metal oxide colorants. The low-temperature glaze has no high melting point hard components.
[0041] Specifically, the core design principle of this glaze formulation lies in achieving a balance between low-temperature rapid firing and excellent wettability. Quartz provides the skeletal structure and hardness of the glaze layer, while borax and feldspar, as the main glass-forming agents, can form a low-viscosity glass phase within the 720-780℃ range, giving the glaze excellent flow and spreading ability, allowing it to spontaneously penetrate into the fine gaps of the metal decorative skeleton 1 and form a smooth mirror surface. The addition of zinc oxide or borate flux further lowers the eutectic temperature of the system and widens the melting temperature range, improving the tolerance of the firing process and avoiding underfiring or overfiring due to furnace temperature fluctuations. Metal oxide colorants (such as copper oxide, iron oxide, cobalt oxide, etc.) can stably develop color in this low-temperature system, and due to the low firing temperature, they are not prone to volatilization or valence change reactions, ensuring the purity of the color and batch consistency. It is particularly important to emphasize that this formulation deliberately excludes high-melting-point hard components such as alumina and zirconium oxide. These components cannot completely dissolve at low temperatures and will remain suspended in the glaze layer as unmelted particles. This not only damages the glaze's gloss and transparency but also causes scratches or chips during the polishing process due to differences in hardness, severely affecting the finished product's appearance. This pure low-temperature glass phase formulation design ensures the compatibility and decorative effect of the glaze and metal framework under low-temperature sintering conditions from the material source.
[0042] Example 4
[0043] Based on Example 1, this example further specifies the assembly, positioning, and fixing method of the ceramic inner liner 2 within the metal outer shell 3. As one implementation method, placing the ceramic inner liner 2 into the inner cavity of the metal outer shell 3 includes: finely adjusting the height of the ceramic inner liner 2 by passing a bottom fixing post 4 through the central hole at the bottom of the metal outer shell 3 and abutting against the bottom surface of the ceramic inner liner 2.
[0044] Specifically, such as Figure 1 and Figure 4 As shown, a through hole is provided at the center of the bottom of the metal outer shell 3. The bottom fixing post 4 passes through the through hole from bottom to top, and its top end face forms a point contact or surface contact with the bottom surface of the ceramic inner liner 2. Since both the ceramic inner liner 2 and the metal outer shell 3 have dimensional tolerances during manufacturing, and the mating part has a process gap reserved for melt filling, if only gravity or lateral restraint is relied upon, the final position of the ceramic inner liner 2 in the axial direction may be deviated, which will affect the installation alignment of the top metal decorative frame 1 or the overall appearance proportion. In this embodiment, by rotating the bottom fixing post 4, the rotational motion is converted into precise axial displacement by utilizing the helix angle of the threaded pair, thereby realizing continuous and precise adjustment of the height of the ceramic inner liner 2. This active fine-tuning mechanism not only compensates for the cumulative processing errors of the parts, but also provides a stable initial positioning reference for the subsequent melt filling process, ensuring the positional consistency of the ceramic inner liner 2 during the welding and sealing process. It should be understood that although this embodiment uses threaded transmission as the means of fine adjustment, in other embodiments, mechanical structures such as eccentric wheel lifting, wedge block adjustment, or multi-stage slot positioning can also be used to achieve the height adjustment function, as long as they can provide controllable axial displacement and maintain support stability.
[0045] Furthermore, in a preferred embodiment, the bottom fixing post 4 is threadedly connected to the metal housing 3, and threadlocker is applied to the threads; a silicone gasket 5 is installed between the head of the bottom fixing post 4 and the bottom surface of the metal housing 3, and one side of the silicone gasket 5 is provided with an adhesive layer.
[0046] Specifically, considering that handicrafts may be subjected to vibration, impact, or temperature cycling loads during daily use or transportation, simple threaded connections are prone to preload reduction or even loosening due to fretting wear or thermal expansion and contraction. Therefore, this embodiment applies thread-locking adhesive to the thread engagement surface. After the adhesive cures, it fills the gaps between the thread teeth, forming an elastic locking layer that combines adhesion and damping, effectively suppressing the relative slippage tendency of the threaded pair and improving the vibration resistance and anti-loosening performance of the connection. Meanwhile, the silicone gasket 5, positioned between the head of the bottom fixing post 4 and the bottom surface of the metal casing 3, serves multiple engineering functions: First, the silicone material itself possesses excellent elasticity and energy dissipation characteristics, capable of absorbing mechanical vibrations transmitted to the connection node from the outside, preventing scratches or fatigue damage to the metal surface caused by rigid contact; Second, the single-sided adhesive design of the silicone gasket 5 allows it to adhere firmly to the bottom surface of the metal casing 3, ensuring the gasket's own positioning reliability while maintaining a low-friction interface between it and the head of the bottom fixing post 4, allowing the fixing post to rotate smoothly during fine-tuning without being affected by the torsional resistance of the gasket; Third, the gasket also plays an auxiliary sealing role, filling the microscopic unevenness between the head of the fixing post and the bottom surface of the casing, enhancing the dustproof and moisture-proof capabilities of the container bottom. It should be understood that although this embodiment preferably uses a single-sided adhesive silicone gasket, in other embodiments, fluororubber, polyurethane, or cork composite materials can be selected according to vibration reduction requirements, and the bonding method can also be replaced with double-sided adhesive, pressure-sensitive adhesive, or mechanical clamping structure, as long as it can achieve the synergistic effect of buffering and shock absorption and auxiliary positioning.
[0047] Example 5
[0048] Based on any one of Examples 1 to 4, this embodiment further defines the surface treatment process after the metal-ceramic composite craft is prepared. As one implementation, after obtaining the metal-ceramic composite craft, the process further includes: sequentially performing degreasing and dust removal, low-temperature baking and dehumidification, surface activation and wiping, high-temperature heat coloring, and pigment painting; and then spraying a colorless, transparent, high-hardness, wear-resistant nano-coating onto the entire surface for sealing.
[0049] Specifically, the aforementioned post-processing steps constitute the key links in the transformation of the product from a semi-finished product to a final work of art, with strict temporal dependencies and functional synergies among the steps. Step S501, degreasing and dust removal, involves thoroughly removing residual cutting fluid, fingerprint grease, and dust particles from the surface of the metal shell 3 and the metal decorative frame 1 using organic solvents or alkaline cleaning agents. This step is a prerequisite for the adhesion of all subsequent coatings; incomplete cleaning will directly lead to uneven coloring or paint film peeling. Step S502, low-temperature baking and dehumidification, is usually carried out at an environment of 60-80℃, aiming to remove moisture adsorbed in the micropores and crevices of the substrate. Since both metal and ceramics are porous or easily hygroscopic materials, residual moisture will vaporize and expand during high-temperature coloring, causing pinholes in the glaze or blistering of the paint film. Therefore, dehumidification is a necessary pretreatment to ensure the stability of surface quality. Step S503, Surface Activation Wiping: A special activator is used to chemically treat the metal surface. The microscopic mechanism involves removing the passivated oxide layer and introducing active groups, improving the wettability and chemical bonding of the metal surface to subsequent hot-dyeing and organic coatings, thus solving the problem of poor adhesion caused by the low surface energy of metal materials. Step S504, High-Temperature Burning and Hot-Dyeing: At a specific temperature, the coloring agent undergoes a controlled oxidation reaction with the metal surface, generating a dense and color-stable metal oxide film in situ. This process differs from simple physical coating; instead, it uses a thermochemical reaction to integrate color into the metal surface, giving the product a rustic and substantial texture and excellent weather resistance, while avoiding the environmental pollution risks of traditional electroplating processes. Step S505, Pigment Painting: Artistic creation is performed on the base color formed by hot-dyeing, including overall color application and detailed local painting. Because the preceding activation and hot-dyeing treatments have established a good interface foundation, the painting pigments adhere firmly and produce pure colors, achieving an organic combination of industrial preparation and handcrafted art. Step S506: A colorless, transparent, high-hardness, wear-resistant nano-coating is sprayed onto the entire surface for sealing treatment. As the outermost protective barrier, this nano-coating, after curing, forms a dense three-dimensional network structure. This not only isolates moisture, oxygen, and pollutants from corroding the internal metal and glaze, preventing the formation of verdigris or glaze weathering, but also effectively resists scratches and wear during daily use due to its high hardness, maintaining the product's gloss and artistic expression for a long time. It should be understood that although this embodiment uses a six-step method as the preferred process flow, in actual production, the combination of processes can be adjusted according to product positioning and environmental adaptability requirements. For example, for decorative items used in dry indoor environments, the dehumidification step can be omitted, or a frosted textured sealing coating can be used for products that pursue a matte effect, as long as it follows the basic technical logic of cleaning-activation-coloring-sealing and can achieve the expected surface performance.
[0050] Example 6
[0051] like Figure 1 , Figure 5 and Figure 6As shown, this embodiment provides a metal-ceramic composite craft, which achieves reliable composite of heterogeneous materials and integrated surface decoration in its structure.
[0052] Specifically, the metal-ceramic composite craft includes a metal outer shell 3, a ceramic inner liner 2, a metal decorative frame 1, and a low-temperature glaze sintering layer. The metal outer shell 3, as the external load-bearing shell, forms the overall outline and mechanical support of the product. Its material is preferably copper or a copper alloy, possessing excellent ductility and impact resistance. The ceramic inner liner 2 is housed within the cavity of the metal outer shell 3, serving as the core of the functional container. Its material is preferably white porcelain, with a dense, smooth glaze and extremely low water absorption (below 0.2%), effectively isolating water from the external metal environment and preventing metal ion leaching that pollutes the water or burns the roots of plants.
[0053] At the mating point between the ceramic inner liner 2 and the metal outer shell 3, the two are not in rigid direct contact, but rather a pre-existing process gap is provided. This gap is filled with a weld formed by molten metal. From a structural perspective, this weld is not only a connecting medium but also a solidified form of a stress-buffering gap. Figure 6 As shown in the enlarged view of detail A, the weld metal, after solidification, completely fills the pre-defined space between the outer wall of the ceramic inner liner 2 and the inner wall of the metal outer shell 3, forming a continuous metallurgical bonding interface. This structural design physically retains a buffer margin to accommodate differences in thermal expansion coefficients. When the ambient temperature changes or thermal stress is generated during use, the weld metal absorbs and releases the interface stress through its own plastic deformation capacity, preventing the brittle ceramic material from cracking due to stress concentration, while ensuring the overall airtightness and watertightness of the container. It should be understood that although the figure shows a uniformly distributed annular weld morphology, in other embodiments, the process gaps and welds can also be designed as locally discrete or variable cross-section forms according to the stress requirements, as long as they can maintain the structural connection and stress release function.
[0054] The metal decorative frame 1 is integrally molded onto the surface of the metal shell 3. For example... Figure 6As shown, there are no seams, welds, or mechanical fastener marks between the metal decorative frame 1 and the metal shell 3. The two are seamlessly connected in terms of material or integrally cast geometrically. This integrated structure eliminates the weak points and aesthetic defects caused by segmented splicing in traditional cloisonné enamel techniques, resulting in smooth and continuous surface texture lines. It can withstand the mechanical loads of subsequent grinding and polishing processes without detachment or displacement. A low-temperature glaze sintered layer fills the gaps in the metal decorative frame 1. Microscopically, this sintered layer forms a tight physical fit with the sidewalls of the metal decorative frame 1. Its upper surface, after grinding, is flush with the top surface of the metal decorative frame 1, together forming a smooth and flat decorative surface. Due to the use of a low-temperature sintering system, the glaze layer contains no unmelted hard particles, has a uniform and dense texture, and does not cause oxidation damage or grain coarsening to the metal substrate during its thermal history, thus maintaining the original mechanical properties and color texture of the metal shell 3.
[0055] In practical applications, such as when used as a vase, the above structural design demonstrates comprehensive performance advantages. The ceramic inner liner 2 provides a chemically inert water-holding environment, solving the problems of pure copper containers easily developing verdigris, polluting water, and damaging flower stems; the metal outer shell 3 gives the product extremely high structural strength and drop resistance, overcoming the safety hazards of traditional ceramic vases being brittle and easily broken; while the one-piece molded metal decorative frame 1 and the low-temperature glaze sintering layer ensure the durability and weather resistance of the surface decorative layer while guaranteeing artistic expression. This composite structure, with its inner ceramic and outer metal, and integrated glaze and frame, successfully combines the physical and chemical advantages of the two materials, avoids their inherent defects, and achieves a high degree of unity between practical function, structural reliability, and aesthetic value.
[0056] The technical scope of this invention is not limited to the content described above. Those skilled in the art can make various modifications and variations to the above embodiments without departing from the technical concept of this invention, and all such modifications and variations should fall within the protection scope of this invention.
Claims
1. A method for preparing a metal-ceramic composite craft, characterized in that, include: The ceramic inner liner is placed into the inner cavity of the metal outer shell. A process gap is reserved at the mating part between the ceramic inner liner and the metal outer shell. The process gap is filled with molten metal and then welded and sealed. A metal decorative frame is integrally formed on the surface of the metal casing; The gaps in the metal decorative frame are filled with low-temperature glaze, and the low-temperature glaze is subjected to multiple filling and sintering processes.
2. The method for preparing metal-ceramic composite handicrafts according to claim 1, characterized in that, The ceramic inner liner and the metal outer shell are fitted with a mechanical interlocking structure; the molten metal is a copper-based molten metal.
3. The method for preparing metal-ceramic composite handicrafts according to claim 2, characterized in that, The mechanical interlocking structure is a dovetail-shaped fit structure, and the outer wall of the ceramic inner liner is provided with an outwardly protruding tooth structure to form the dovetail-shaped fit structure; the top inner wall of the ceramic inner liner is provided with an anti-overflow protrusion, and the height of the anti-overflow protrusion is 1-1.5mm.
4. The method for preparing metal-ceramic composite handicrafts according to claim 1, characterized in that, The process of integrally forming a metal decorative skeleton on the surface of the metal shell includes: integrally forming the metal decorative skeleton on the surface of the metal shell by using an additive manufacturing sacrificial mold combined with a lost-wax casting process; and performing multiple filling and sintering treatments on the low-temperature glaze, including: performing multiple fillings and secondary sintering of the low-temperature glaze at corresponding temperatures in a low-temperature range below the oxidation deformation temperature of the metal shell.
5. The method for preparing metal-ceramic composite handicrafts according to claim 4, characterized in that, The additive manufacturing sacrificial mold is a 3D printed wax film; the temperature of the low-temperature range is 720-780℃, and the holding time for each sintering is 3-5 minutes; the number of filling operations is 2-4 times.
6. The method for preparing metal-ceramic composite handicrafts according to claim 4, characterized in that, The low-temperature glaze is mainly composed of quartz, borax and feldspar, with zinc oxide or borate added as flux, and is combined with metal oxide colorants. The low-temperature glaze has no high melting point hard components.
7. The method for preparing metal-ceramic composite handicrafts according to claim 1, characterized in that, Inserting the ceramic inner liner into the inner cavity of the metal outer shell includes: passing a bottom fixing post through the central hole at the bottom of the metal outer shell and abutting against the bottom surface of the ceramic inner liner, and finely adjusting the height of the ceramic inner liner.
8. The method for preparing metal-ceramic composite handicrafts according to claim 7, characterized in that, The bottom fixing post is threadedly connected to the metal shell, and threadlocker is applied to the threads; a silicone gasket is installed between the head of the bottom fixing post and the bottom surface of the metal shell, and one side of the silicone gasket has an adhesive layer.
9. The method for preparing metal-ceramic composite handicrafts according to claim 1, characterized in that, After obtaining the metal and ceramic composite crafts, the process further includes: sequentially performing degreasing and dust removal, low-temperature baking and dehumidification, surface activation and wiping, high-temperature firing and hot coloring, and pigment painting; and spraying the entire surface with colorless, transparent, high-hardness, wear-resistant nano paint for surface sealing treatment.
10. A composite metal and ceramic craft, characterized in that, include: Metal casing; A ceramic inner liner is housed within the inner cavity of the metal outer shell. A process gap is provided at the mating part between the ceramic inner liner and the metal outer shell, and the process gap is filled with a weld formed by molten metal. A metal decorative frame is integrally formed on the surface of the metal shell; A low-temperature glaze sintering layer is filled into the gaps of the metal decorative frame.