A method for controlling the particle size of narrow-distribution electronic-grade silica sol and its application

By employing constant low supersaturation quantitative speed control and online DLS feedback adjustment on conventional equipment, the acceleration rate of silica droplets is controlled, secondary nucleation is suppressed, and silica sol with narrow particle size distribution and low metal impurities is prepared. This solves the problems of high equipment investment and non-uniform particle size in the prior art, and realizes the efficient preparation of semiconductor wafer polishing.

CN123105663APending Publication Date: 2026-11-17SHANGHAI EACO GASES CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611259197.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies cannot achieve the preparation of narrow-distribution electronic-grade silica sol on conventional equipment. The particle size distribution is uneven, making it difficult to meet the high standards required for semiconductor wafer polishing. Furthermore, the process is costly, requires significant equipment investment, or causes severe pollution.

Method used

A dual mechanism of constant low supersaturation quantitative rate control and online DLS real-time particle size feedback adjustment was adopted, combined with conventional reactors, metering pumps and ceramic membrane equipment, to control the silica droplet acceleration rate, suppress secondary nucleation, and prepare silica sol with PDI stability ≤0.08 through ion purification, low temperature concentration and clean encapsulation processes.

Benefits of technology

It enables the preparation of silica sol with narrow particle size distribution and low metal impurities on conventional equipment, meeting the needs of semiconductor polishing. It has low equipment investment, good batch consistency, and a wide adjustable particle size range, which meets the industrialization requirements of electronic-grade silica sol.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105663A_ABST
    Figure CN123105663A_ABST
Patent Text Reader

Abstract

This invention relates to a narrow-distribution electronic-grade silica sol, a particle size control method, and its application. It is used for preparing silica sol specifically for semiconductor CMP polishing slurries and includes the following steps: S1, seed crystal preparation; S2, preparation of active silicic acid supply solution; S3, constant-rate low-supersaturation seed crystal growth; S4, online DLS particle size monitoring and dynamic adjustment of droplet acceleration rate: The reactor is equipped with an online dynamic light scattering DLS analyzer, which automatically samples and detects the average particle size D every 10-15 minutes. 50 With polydispersity index (PDI); adjustment rules: if PDI is stable <0.08, maintain the current dropping rate; if the increase in PDI exceeds 0.01 in two consecutive tests, reduce the dropping rate by 20%~30%; when the average particle size reaches 90% of the target particle size, gradually reduce the dropping rate until the target particle size is reached and dropping stops; S5, heat preservation and aging; S6, concentration and purification; S7, clean packaging: HDPE drums are sealed with nitrogen in a Class 100 clean environment to avoid secondary pollution from CO2 and particulate matter in the air.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of inorganic nanoelectronic material preparation technology, and relates to a narrow-distribution electronic-grade silica sol, a particle size control method, and its application. Background Technology

[0002] Electronic-grade silica sol is the core abrasive in semiconductor wafer polishing slurries. Wafer polishing has stringent requirements for the uniformity of silica sol particle size. Industry standards require a polydispersity index (PDI) of less than 0.1 and prohibit the presence of ultra-large particles larger than twice the average particle size, otherwise it will cause scratches on the wafer surface and a significant decrease in polishing yield.

[0003] The current mainstream industrial method for preparing silica sol is the seed crystal growth method: first, small-diameter seed crystals of 10-20 nm are prepared, and then active silicic acid is continuously added dropwise under an alkaline environment. The silicic acid grows on the seed crystal surface, achieving particle size expansion. The core drawback of this process is that secondary nucleation easily occurs during the growth process. Local supersaturation of free silicic acid in the system spontaneously generates new small crystal nuclei, resulting in a wider particle size distribution and excessive PDI in the finished product. At the same time, fluctuations in the silicic acid dropping rate, reaction temperature, and pH can all exacerbate the problem of particle size inhomogeneity.

[0004] Existing related patent technologies have significant shortcomings: CN114249330B stabilizes pH by adding silica in stages and adding buffer salts, relies solely on manually fixing the dropping rate, lacks the ability to quantitatively calculate and match seed consumption, and cannot fundamentally inhibit secondary nucleation, making it difficult for the finished product's PDI to remain consistently below 0.1. CN117654408A uses a neural network + ADRC complex algorithm to achieve fully automatic closed-loop control. The supporting automated control system equipment has a high investment cost, and conventional reaction vessel production lines cannot be modified and implemented, resulting in a high industrialization threshold. CN119841322A uses organosilane as the silicon source, which has high raw material costs and hydrolysis byproducts that pollute the silica sol, and cannot meet the requirements of low metal and low impurity for electronic grade. Conventional simple seed growth processes only fix the acceleration rate of a single droplet, without dynamically reducing the rate as the specific surface area of ​​the seed crystal decreases, and there is no online real-time particle size correction. This results in poor particle size consistency between batches and makes the seed crystals prone to stratification and aggregation during long-term storage.

[0005] The aforementioned existing technologies fail to simultaneously meet the four major semiconductor polishing requirements: simple and easily industrialized processes, low cost, compatibility with conventional equipment, stable PDI < 0.08, and low metal impurities. They lack a complete technical solution that "quantitatively calibrates the maximum silica consumption rate based on the seed crystal surface area, limits the drop rate to 70%~90% Vmax, and uses online DLS segmented feedback speed regulation," and also lack a complete process for the purification, low-temperature concentration, and clean packaging of electronic-grade silica sol. Therefore, this paper designs a narrow-distribution electronic-grade silica sol, a particle size control method, and its application to overcome the aforementioned problems. Summary of the Invention

[0006] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a narrow-distribution electronic-grade silica sol, a particle size control method, and its application. It suppresses secondary nucleation at its source through a dual mechanism of constant low supersaturation quantitative rate control and real-time particle size feedback adjustment via online DLS. The entire process can be implemented using conventional reactors, metering pumps, online DLS, and ceramic membrane equipment, without the need for complex automated control systems. Combined with ion purification, low-temperature concentration, and Class 100 nitrogen-filled encapsulation processes, it produces a semiconductor CMP-specific silica sol with a stable PDI of ≤0.08, low metal impurities, and no ultra-large particles.

[0007] This invention is achieved through the following technical solution: a method for controlling the particle size of narrow-distribution electronic-grade silica sol, used for preparing silica sol specifically for semiconductor CMP polishing slurries, comprising the following steps: S1. Seed Crystal Preparation: Water glass is processed through a strongly acidic cation exchange resin to obtain active silicic acid with a SiO2 concentration of 3-5% and a pH of 2-3; the pH is adjusted to 9.5-10.5 with electronic-grade ammonia, and the mixture is reacted at 85-95℃ for 2-4 hours to obtain a silica sol seed solution with an average particle size of 10-20 nm; the seed solution is then purified again by cation exchange to control the Na... + Content <1ppm; S2. Preparation of active silicic acid supply solution: Fresh active silicic acid solution is obtained by passing water glass through a strong acidic cation exchange resin. The SiO2 concentration is 3-5%. It should be prepared and used immediately and the storage time should not exceed 2 hours. S3. Constant-rate low-supersaturation seed crystal growth: Transfer the seed crystal solution into the reaction vessel, adjust the pH to 9.5~10.0 with ammonia water, heat to 85~95℃ and stir at a constant temperature; add fresh active silicic acid S2 dropwise to the seed crystal solution at a constant rate; The method for determining the dropping acceleration rate is as follows: First, calculate the total specific surface area S of the seed crystals in the system based on the initial average particle size D0 of the seed crystals and the mass fraction C of SiO2 in the seed crystal solution. Then, calibrate the maximum safe consumption rate Vmax of silicic acid at the reaction temperature. The actual dropping acceleration rate is set to 70% to 90% of Vmax, so that the concentration of free silicic acid in the system remains below the critical nucleation concentration. S4. Online DLS Particle Size Monitoring and Dynamic Adjustment of Dropping Acceleration Rate: The reactor is equipped with an online dynamic light scattering DLS analyzer, which automatically samples and detects the average particle size D every 10-15 minutes. 50 With the Proportional Dispersion Index (PDI); Adjustment rules: If PDI is consistently <0.08, maintain the current dropping rate; if the increase in PDI exceeds 0.01 in two consecutive tests, reduce the dropping rate by 20%~30%; when the average particle size reaches 90% of the target particle size, gradually reduce the dropping rate until the target particle size is reached and dropping stops. S5. Heat preservation and aging: After stopping the addition of silica, heat preservation and aging at 90~95℃ for 2~4 hours; the surface structure of the particles tends to be complete and the particle size tends to be stable. S6. Concentration and purification: The aged silica sol is concentrated to a SiO2 mass fraction of 30-50% at low temperature of 15-35℃ through a ceramic membrane with a molecular weight cutoff of 10kDa; then it is filtered through a 0.1μm precision filter to remove large particulate impurities. S7. Clean Packaging: HDPE drums are sealed with nitrogen in a Class 100 clean environment to avoid secondary pollution from CO2 and particulate matter in the air.

[0008] Preferably, the formula for calculating the total specific surface area S in step S3 is:

[0009] In the formula: S is the total specific surface area of ​​the seed crystals per unit volume (m² / L); C0 is the mass fraction of SiO2 in the seed crystal solution; ≈2.2 g / cm³ is the density of silicon dioxide; D0 is the initial average particle size of the seed crystals (nm); This is the conversion factor for the mass concentration of SiO2 in silica sol.

[0010] Preferably, the initial drop rate in step S3 is gradually reduced as the seed crystal size increases; for a 1L reaction system with an initial seed crystal size of 15nm and a solid content of 5%, the initial drop rate of active silica with a SiO2 concentration of 4% is 0.52mL / min.

[0011] Preferably, the seed solution prepared in step S1 has a PDI < 0.15 according to DLS detection; the final product silica sol has a stable PDI ≤ 0.08, and no particles with a particle size greater than twice the average particle size are detected.

[0012] Preferably, the electronic-grade ammonia used in steps S3 and S1 is free of metal impurities, and the sodium ion content of the purified seed solution is <1ppm, which is suitable for the low metal contamination requirements of semiconductor polishing.

[0013] As a preferred option, the average particle size of the target silica sol is controllable in the range of 20~150nm, including three commonly used polishing abrasive specifications: 50nm, 80nm, and 120nm.

[0014] A narrow-distribution electronic-grade silica sol is prepared using the particle size control method described in claim 1. The silica sol consists of spherical particles with a PDI ≤ 0.08, a SiO2 solid content of 30-50%, a sodium ion content < 1 ppm, and no large particles exceeding twice the average particle size. It is used as an abrasive in CMP chemical mechanical polishing slurries for semiconductor wafers.

[0015] This invention also discloses the application of a narrow-distribution electronic-grade silica sol in chemical mechanical polishing slurries for silicon substrates, silicon carbide, and gallium nitride semiconductor wafers.

[0016] The beneficial effects of this invention are as follows: 1) Simple operation and easy to industrialize: This invention only requires conventional reaction vessels, metering pumps, online DLS and ceramic membrane concentration systems, without the need for complex partitioned reaction vessels or graded membrane circulation systems. The equipment investment is low and it is easy to implement on existing production lines.

[0017] 2) Effectively suppress secondary nucleation: By controlling the silica droplet acceleration rate below the seed growth consumption rate, the concentration of free silica in the system is always lower than the critical nucleation concentration, thus fundamentally suppressing secondary nucleation.

[0018] 3) Narrow particle size distribution: Using the method of this invention, the PDI of the obtained silica sol can be stably controlled below 0.08, which is better than the industry standard of 0.1.

[0019] 4) Wide adjustable particle size range: By controlling the amount of seed crystals and the growth time, the particle size can be precisely controlled within the range of 20~150 nm.

[0020] 5) Good batch consistency: Real-time online DLS monitoring and feedback adjustment ensure the reproducibility of particle size between different batches.

[0021] In this invention, when the concentration of silicic acid in the system is below the critical nucleation concentration, no new nucleation reaction will occur, and silicic acid can only grow on the surface of existing seed crystals. Therefore, as long as the dropping rate of silicic acid is controlled to be slow enough so that the silicic acid is consumed by the seed crystal surface as soon as it is added, the concentration of free silicic acid in the system is always maintained below the critical nucleation concentration, thus fundamentally suppressing secondary nucleation. Attached Figure Description

[0022] Figure 1 This is a process flow diagram of the electronic-grade silica sol particle size control method of the present invention; Figure 2 This is a TEM image of the silica sol obtained in Example 1 of the present invention. Detailed Implementation

[0023] To enable those skilled in the art to more clearly understand the purpose, technical solution, and advantages of the present invention, the present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0024] The invention will now be described in detail with reference to the accompanying drawings: Figure 1 As shown, a method for controlling the particle size of narrow-distribution electronic-grade silica sol, used for preparing silica sol specifically for semiconductor CMP polishing slurries, includes the following steps: S1. Seed Crystal Preparation: Water glass is processed through a strongly acidic cation exchange resin to obtain active silicic acid with a SiO2 concentration of 3-5% and a pH of 2-3; the pH is adjusted to 9.5-10.5 with electronic-grade ammonia, and the mixture is reacted at 85-95℃ for 2-4 hours to obtain a silica sol seed solution with an average particle size of 10-20 nm; the seed solution is then purified again by cation exchange to control the Na... + Content <1ppm; S2. Preparation of active silicic acid supply solution: Fresh active silicic acid solution is obtained by passing water glass through a strong acidic cation exchange resin. The SiO2 concentration is 3-5%. It should be prepared and used immediately and the storage time should not exceed 2 hours. S3. Constant-rate low-supersaturation seed crystal growth: Transfer the seed crystal solution into the reaction vessel, adjust the pH to 9.5~10.0 with ammonia water, heat to 85~95℃ and stir at a constant temperature; add fresh active silicic acid S2 dropwise to the seed crystal solution at a constant rate; The method for determining the dropping acceleration rate is as follows: First, calculate the total specific surface area S of the seed crystals in the system based on the initial average particle size D0 of the seed crystals and the mass fraction C of SiO2 in the seed crystal solution. Then, calibrate the maximum safe consumption rate Vmax of silicic acid at the reaction temperature. The actual dropping acceleration rate is set to 70% to 90% of Vmax, so that the concentration of free silicic acid in the system remains below the critical nucleation concentration. S4. Online DLS Particle Size Monitoring and Dynamic Adjustment of Dropping Acceleration Rate: The reactor is equipped with an online dynamic light scattering DLS analyzer, which automatically samples and detects the average particle size D every 10-15 minutes. 50 With the Proportional Dispersion Index (PDI); Adjustment rules: If PDI is consistently <0.08, maintain the current dropping rate; if the increase in PDI exceeds 0.01 in two consecutive tests, reduce the dropping rate by 20%~30%; when the average particle size reaches 90% of the target particle size, gradually reduce the dropping rate until the target particle size is reached and dropping stops. S5. Heat preservation and aging: After stopping the addition of silica, heat preservation and aging at 90~95℃ for 2~4 hours; the surface structure of the particles tends to be complete and the particle size tends to be stable.

[0025] S6. Concentration and purification: The aged silica sol is concentrated to a SiO2 mass fraction of 30-50% at low temperature of 15-35℃ through a ceramic membrane with a molecular weight cutoff of 10kDa; then it is filtered through a 0.1μm precision filter to remove large particulate impurities. S7. Clean Packaging: HDPE drums are sealed with nitrogen in a Class 100 clean environment to avoid secondary pollution from CO2 and particulate matter in the air.

[0026] The formula for calculating the total specific surface area S in step S3 is as follows:

[0027] In the formula: S is the total specific surface area of ​​the seed crystals per unit volume (m² / L); C0 is the mass fraction of SiO2 in the seed crystal solution; ≈2.2 g / cm³ is the density of silicon dioxide; D0 is the initial average particle size of the seed crystals (nm); This is the conversion factor for the mass concentration of SiO2 in silica sol.

[0028] The initial drop rate in step S3 is gradually reduced as the seed crystal size increases; for a 1L reaction system with an initial seed crystal size of 15nm and a solid content of 5%, the initial drop rate of active silica with a SiO2 concentration of 4% is 0.52mL / min.

[0029] Preferably, the seed solution prepared in step S1 has a PDI < 0.15 according to DLS detection; the final product silica sol has a stable PDI ≤ 0.08, and no particles with a particle size greater than twice the average particle size are detected.

[0030] The electronic-grade ammonia used in steps S3 and S1 is free of metal impurities, and the sodium ion content of the purified seed solution is <1ppm, which is suitable for the low metal contamination requirements of semiconductor polishing.

[0031] The target silica sol has a controllable average particle size range of 20~150nm, including three commonly used polishing abrasive specifications: 50nm, 80nm, and 120nm.

[0032] A narrow-distribution electronic-grade silica sol is prepared using the particle size control method described in claim 1. The silica sol consists of spherical particles with a PDI ≤ 0.08, a SiO2 solid content of 30-50%, a sodium ion content < 1 ppm, and no large particles exceeding twice the average particle size. It is used as an abrasive in CMP chemical mechanical polishing slurries for semiconductor wafers.

[0033] This invention also discloses the application of a narrow-distribution electronic-grade silica sol in chemical mechanical polishing slurries for silicon substrates, silicon carbide, and gallium nitride semiconductor wafers.

[0034] Example 1 (Target particle size 50 nm) (1) Seed crystal preparation: Take 500 mL of high-purity water glass (SiO2 content 28%, modulus 3.2) and pass it through a strong acidic cation exchange resin (H + A cation exchange resin (1 L column volume) was used to obtain approximately 600 mL of active silicic acid solution (SiO2 concentration 4.2%, pH 2.5). 300 mL of this silicic acid solution was taken, and the pH was adjusted to 10.0 with electronic-grade ammonia. The mixture was stirred at 90°C for 3 hours to obtain a seed solution with an average particle size of approximately 15 nm. The seed solution was then purified again using a cation exchange resin for later use. DLS analysis showed an average seed particle size of 15.5 nm and a PDI of 0.13.

[0035] (2) Preparation of active silicic acid supply solution: using water glass as raw material, the solution is exchanged with cation exchange resin to obtain fresh active silicic acid solution (SiO2 concentration 4.2%, pH 2.5), which is prepared and used immediately and the storage time does not exceed 1 hour.

[0036] (3) Constant-rate dropwise growth: Add 200 mL of seed solution to a 1 L reactor, adjust the pH to 10.0 with ammonia, and heat to 90 °C. Add active silicic acid solution dropwise at an initial rate of 1.5 mL / min. Take online DLS samples every 10 minutes.

[0037] After 3 hours of growth, DLS showed an average particle size of 42 nm and a PDI of 0.06. The dropping rate was reduced to 1.0 mL / min. After another 1.5 hours of growth, the average particle size reached 49.5 nm and the PDI reached 0.07, at which point the dropping was stopped.

[0038] (4) Heat preservation and aging: heat preservation and aging at 90℃ for 2 hours.

[0039] (5) Concentration: The SiO2 concentration is concentrated to 40% by ceramic membrane.

[0040] Product test results: average particle size 50.2 nm, PDI=0.07, particles larger than 100 nm were not detected (DLS verification).

[0041] like Figure 2 The image shown is a TEM image of the silica sol obtained in Example 1. As can be seen from the image, the particles are spherical, uniform in size, and well dispersed. No large particles larger than twice the average particle size were observed.

[0042] Example 2 (Target particle size 80 nm) The difference from Example 1 is that the seed solution volume was reduced to 100 mL, the initial dropping rate was 2.0 mL / min, and the growth time was approximately 6 hours. During the growth process, the dropping rate was gradually reduced based on DLS feedback. The remaining steps were the same as in Example 1.

[0043] Product test results: average particle size 80.5 nm, PDI=0.08, particles larger than 160 nm were not detected.

[0044] Example 3 (Target particle size 120 nm) The difference from Example 1 is that the amount of seed solution used is reduced to 50 mL, the initial dropping rate is 1.5 mL / min, and the growth time is approximately 9 hours. The remaining steps are the same as in Example 1.

[0045] Product test results: average particle size 119.8 nm, PDI=0.08, particles larger than 240 nm were not detected.

[0046] Comparative Example 1 (Drip acceleration rate too fast) The difference from Example 1 is that the initial dropping rate of the active silica was set to 4.0 mL / min (approximately 2.7 times that of Example 1), and the growth rate was not reduced during the growth process. All other conditions were the same as in Example 1.

[0047] Product testing results: average particle size 53.1 nm, PDI=0.23, DLS analysis showed obvious secondary nucleation particles (approximately 10~15 nm). This does not meet the requirement of electronic grade PDI<0.1.

[0048] The specific embodiments described herein are merely illustrative of the principles and effects of the invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in this invention should still be covered by the claims of this invention.

Claims

1. A method for controlling the particle size of a narrow distribution electronic grade silica sol, characterized by, The preparation of a special silica sol for semiconductor CMP polishing slurry includes the following steps: S1. Seed Crystal Preparation: Water glass is processed through a strongly acidic cation exchange resin to obtain active silicic acid with a SiO2 concentration of 3-5% and a pH of 2-3; the pH is adjusted to 9.5-10.5 with electronic-grade ammonia, and the mixture is reacted at 85-95℃ for 2-4 hours to obtain a silica sol seed solution with an average particle size of 10-20 nm; the seed solution is then purified again by cation exchange to control the Na... + Content <1ppm; S2. Preparation of active silicic acid supply solution: Fresh active silicic acid solution is obtained by passing water glass through a strong acidic cation exchange resin. The SiO2 concentration is 3-5%. It should be prepared and used immediately and the storage time should not exceed 2 hours. S3. Constant-rate low-supersaturation seed crystal growth: Transfer the seed crystal solution into the reaction vessel, adjust the pH to 9.5~10.0 with ammonia water, heat to 85~95℃ and stir at a constant temperature; Fresh active silicic acid S2 is added dropwise to the seed crystal solution at a constant rate; The method for determining the dropping acceleration rate is as follows: First, calculate the total specific surface area S of the seed crystals in the system based on the initial average particle size D0 of the seed crystals and the mass fraction C of SiO2 in the seed crystal solution. Then, calibrate the maximum safe consumption rate Vmax of silicic acid at the reaction temperature. The actual dropping acceleration rate is set to 70% to 90% of Vmax, so that the concentration of free silicic acid in the system remains below the critical nucleation concentration. S4. Online DLS Particle Size Monitoring and Dynamic Adjustment of Dropping Acceleration Rate: The reactor is equipped with an online dynamic light scattering DLS analyzer, which automatically samples and detects the average particle size D every 10-15 minutes. 50 With the Proportional Dispersion Index (PDI); Adjustment rules: If PDI is consistently <0.08, maintain the current dropping rate; if the increase in PDI exceeds 0.01 in two consecutive tests, reduce the dropping rate by 20%~30%; when the average particle size reaches 90% of the target particle size, gradually reduce the dropping rate until the target particle size is reached and dropping stops. S5. Heat preservation and aging: After stopping the addition of silica, heat preservation and aging at 90~95℃ for 2~4 hours; the surface structure of the particles tends to be complete and the particle size tends to be stable. S6. Concentration and purification: The aged silica sol is concentrated to a SiO2 mass fraction of 30-50% at low temperature of 15-35℃ through a ceramic membrane with a molecular weight cutoff of 10kDa; then it is filtered through a 0.1μm precision filter to remove large particulate impurities. S7. Clean Packaging: HDPE drums are sealed with nitrogen in a Class 100 clean environment to avoid secondary pollution from CO2 and particulate matter in the air.

2. The method of claim 1, wherein the narrow distribution electronic grade silicon sol has a particle size of 5 to 50 nm. The formula for calculating the total specific surface area S in step S3 is as follows:

3. In the formula: S is the total specific surface area of ​​the seed crystals per unit volume (m² / L); C0 is the mass fraction of SiO2 in the seed crystal solution; D0 is the density of silicon dioxide; D0 is the initial average particle size of the seed crystal (nm). This is the conversion factor for the mass concentration of SiO2 in silica sol.

4. The particle size control method for narrow-distribution electronic-grade silica sol according to claim 1, characterized in that, The initial drop rate in step S3 is gradually reduced as the seed crystal size increases; for a 1L reaction system with an initial seed crystal size of 15nm and a solid content of 5%, the initial drop rate of active silica with a SiO2 concentration of 4% is 0.52mL / min.

5. The method of claim 1, wherein the narrow distribution electronic grade silica sol has a particle size of 5 to 50 nm. The seed solution prepared in step S1 has a PDI < 0.15 according to DLS testing; the final product, silica sol, has a stable PDI ≤ 0.08, and no particles with a diameter greater than twice the average particle size are detected.

6. The particle size control method for narrow-distribution electronic-grade silica sol according to claim 1, characterized in that, The electronic-grade ammonia used in steps S3 and S1 is free of metal impurities, and the sodium ion content of the purified seed solution is <1ppm, which is suitable for the low metal contamination requirements of semiconductor polishing.

7. The particle size control method for narrow-distribution electronic-grade silica sol according to claim 1, characterized in that, The target silica sol has a controllable average particle size range of 20~150nm, including three commonly used polishing abrasive specifications: 50nm, 80nm, and 120nm.

8. A narrow-distribution electronic-grade silica sol, characterized in that, Prepared using the particle size control method described in any one of claims 1-6; the silica sol consists of spherical particles with PDI ≤ 0.08, SiO2 solid content of 30-50%, sodium ion content < 1 ppm, and no large particles exceeding twice the average particle size, and is used as an abrasive for CMP chemical mechanical polishing slurry of semiconductor wafers.

9. The application of the narrow-distribution electronic-grade silica sol according to claim 7 in the chemical mechanical polishing slurry of silicon substrates, silicon carbide, and gallium nitride semiconductor wafers.

Citation Information

Patent Citations

  • A method for preparing large-particle-size, narrow-distribution silica sol

    CN114249330B

  • Silicon sol seed crystal growth control method and system for wafer grinding and medium

    CN117654408A

  • Preparation method of wide-distribution large-particle-size silica sol, silica sol and application thereof