A columnar alumina powder and its preparation method
By using nucleation inducing agents and morphology modifiers to regulate the grain growth of aluminum hydroxide during hydrothermal treatment, the problem of difficulty in controlling the morphology and aspect ratio of columnar alumina powder in the prior art has been solved, and columnar alumina powder with high specific surface area and excellent morphology has been prepared.
Patent Information
- Application Number
- CN202611556732.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-09
- Publication Date
- 2026-11-17
AI Technical Summary
Existing preparation methods are insufficient to obtain columnar alumina powder with high aspect ratio and controllable morphology, and the grains tend to agglomerate in the hydrothermal method, resulting in a decrease in specific surface area.
A precursor slurry was formed by mixing aluminum hydroxide with a nucleation inducing agent and a morphology modifier, and then subjected to hydrothermal treatment to control the grain growth rate, thereby obtaining alumina powder with columnar morphology and high aspect ratio.
Columnar alumina powder with controllable specific surface area, high aspect ratio and excellent morphology was prepared, avoiding excessive grain growth and agglomeration.
Smart Images

Figure CN123105697A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of powder materials technology, specifically to a columnar alumina powder and its preparation method. Background Technology
[0002] Columnar alumina powder exhibits unique application potential in the field of catalyst supports due to its high aspect ratio, good thermal stability, and tunable surface acidity / alkalinity. Its anisotropic grains not only construct a continuous "skeletal" pore structure, promoting rapid mass transfer of reactant molecules, but also form numerous mesoporous-macroporous hierarchical pores through grain overlap, providing ample sites for highly dispersed loading of active components. Simultaneously, the excellent anti-sintering ability of the alumina matrix ensures the structural stability of the support under high-temperature regeneration conditions. Currently, the main methods for preparing columnar alumina include the molten salt method, the precipitation-hydrothermal conversion method, and the template method.
[0003] While the molten salt method can yield well-crystallized columnar grains, the resulting products often have coarse grains, low specific surface area, and poor columnar morphology. Furthermore, high-temperature washing is required to remove the molten salt, making the process cumbersome. Although the precipitation method combined with calcination can produce mesoporous structures, the morphology controllability is poor, making it difficult to consistently obtain columnar particles with high aspect ratios. The hydrothermal method is considered an ideal approach for preparing columnar alumina because it can control the preferred growth direction of grains under mild conditions. However, current hydrothermal research struggles to control the morphology of columnar crystals, and the resulting columnar grains tend to grow excessively along the axial direction, resulting in increased transverse dimensions and a rapid decrease in specific surface area. At the same time, grain aggregation easily occurs in the hydrothermal system, hindering the effective specific surface area. Summary of the Invention
[0004] In view of this, the purpose of this invention is to provide a columnar alumina powder and its preparation method. This invention involves mixing aluminum hydroxide with a nucleation inducing agent and a morphology modifier to form a precursor slurry, followed by hydrothermal treatment. The nucleation inducing agent promotes nucleation, and the morphology modifier regulates the growth rate of each crystal facet, causing aluminum hydroxide to transform in a liquid phase environment and achieve preferential grain growth. The resulting columnar alumina powder has a good columnar morphology and a high aspect ratio, and the specific surface area of the powder is controllable.
[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a method for preparing columnar alumina powder, comprising the following steps: Aluminum hydroxide, water, and composite additives are mixed to obtain a precursor slurry; The precursor slurry was subjected to hydrothermal treatment to obtain the columnar alumina powder. The composite additive includes nucleation inducing agents and morphology modifiers.
[0006] Preferably, the nucleation inducing agent includes one or more of α-Al₂O₃, α-Fe₂O₃, Cr₂O₃ and α-AlOOH.
[0007] Preferably, the morphology modifier includes one or more of sulfuric acid, hydrochloric acid, oxalic acid, acetic acid, boric acid, and citric acid.
[0008] Preferably, the hydrothermal treatment temperature is 400~430℃, the pressure is 20~35MPa, and the heat and pressure holding time is 12~72h.
[0009] Preferably, the amount of nucleation inducing agent added is 0.5-1% of the mass of aluminum hydroxide; and the amount of morphology modifier added is 0.05-0.4% of the mass of aluminum hydroxide.
[0010] Preferably, the solid content of the precursor slurry is 50-85 wt%.
[0011] Preferably, the aluminum hydroxide has an average particle size of 2~10μm and a purity of ≥99.9wt%.
[0012] Preferably, the nucleation inducer has an average particle size of 2~10μm and a purity of ≥99wt%.
[0013] Preferably, the hydrothermal treatment further includes cleaning, wherein the cleaning is performed sequentially using an ammonium citrate solution and water, and the mass fraction of the ammonium citrate solution is 10%.
[0014] The present invention also provides columnar alumina powder prepared by the preparation method described above, wherein the columnar alumina powder has a crystal length of 1~22 μm, an aspect ratio of 1.5~7, and a specific surface area of 0.31~5.60 m². 2 / g.
[0015] This invention provides a method for preparing columnar alumina powder, comprising the following steps: Aluminum hydroxide, water, and composite additives are mixed to obtain a precursor slurry; The precursor slurry was subjected to hydrothermal treatment to obtain the columnar alumina powder. The composite additive includes nucleation inducing agents and morphology modifiers.
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention involves mixing aluminum hydroxide with a nucleation inducing agent and a morphology modifier to form a precursor slurry, followed by hydrothermal treatment. This allows the nucleation inducing agent to promote nucleation, while the morphology modifier regulates the growth rate of each crystal facet. As a result, aluminum hydroxide undergoes transformation in a liquid environment, achieving preferential grain growth. The resulting columnar alumina powder exhibits a good columnar morphology and a high aspect ratio, and its specific surface area is controllable.
[0017] Furthermore, the parameters of hydrothermal treatment controlled by this invention can ensure sufficient phase transformation of aluminum hydroxide while avoiding excessive grain growth. Attached Figure Description
[0018] Figure 1 The image shows the XRD pattern of the columnar alumina powder in Example 1. Figure 2 These are scanning electron microscope (SEM) images of the columnar alumina powder in Example 1 at different magnifications. Figure 3 These are SEM images of the columnar alumina powder in Example 2 at different magnifications; Figure 4 These are SEM images of the columnar alumina powder in Example 3 at different magnifications; Figure 5 The XRD pattern of the powder prepared in Comparative Example 1; Figure 6 SEM image of the powder prepared in Comparative Example 1; Figure 7 The XRD pattern of the powder prepared in Comparative Example 2; Figure 8 The image shows the SEM image of the powder prepared in Comparative Example 2. Detailed Implementation
[0019] This invention provides a method for preparing columnar alumina powder, comprising the following steps: Aluminum hydroxide, water, and composite additives are mixed to obtain a precursor slurry; The precursor slurry was subjected to hydrothermal treatment to obtain the columnar alumina powder. The composite additive includes nucleation inducing agents and morphology modifiers.
[0020] Unless otherwise specified, the materials and equipment used in this invention are all commercially available products in the field.
[0021] This invention involves mixing aluminum hydroxide, water, and composite additives to obtain a precursor slurry.
[0022] In this invention, the aluminum hydroxide is preferably micron-sized powder, the average particle size of the aluminum hydroxide is preferably 2~10μm, and the purity of the aluminum hydroxide is preferably ≥99.9wt%.
[0023] In this invention, the nucleation inducing agent preferably includes one or more of α-Al2O3, α-Fe2O3, Cr2O3 and α-AlOOH, the nucleation inducing agent is preferably a micron-sized powder, the average particle size of the nucleation inducing agent is preferably 2~10μm, the purity of the nucleation inducing agent is preferably ≥99wt%, and the nucleation inducing agent provides a coherent epitaxial template that significantly reduces the phase transition energy barrier and accelerates nucleation.
[0024] In this invention, the morphology control agent preferably includes one or more of sulfuric acid, hydrochloric acid, oxalic acid, acetic acid, boric acid, and citric acid. The purity of boric acid, oxalic acid, sulfuric acid, acetic acid, and citric acid in the morphology control agent is preferably ≥99.5 wt%, and the purity of hydrochloric acid is preferably ≥36 wt%. In specific embodiments, the morphology control agent can preferably be a mixture of oxalic acid and citric acid in a mass ratio of 9:1 or 5:3, a mixture of boric acid and acetic acid in a mass ratio of 4:1, a mixture of sulfuric acid and hydrochloric acid in a mass ratio of 3:5, a mixture of boric acid and oxalic acid in a mass ratio of 5:3, or a mixture of sulfuric acid and oxalic acid in a mass ratio of 2:3. The morphology control agent regulates the growth rate of each crystal face of the grain, so that aluminum hydroxide undergoes transformation in the liquid phase environment and achieves preferential grain growth, thereby obtaining a columnar morphology.
[0025] In this invention, the amount of nucleation inducing agent added is preferably 0.5 to 1% of the mass of aluminum hydroxide, and the amount of morphology modifier added is preferably 0.05 to 0.4% of the mass of aluminum hydroxide.
[0026] In this invention, the mass ratio of aluminum hydroxide to water is preferably 1:1 to 17:3, and the solid content of the precursor slurry is preferably 50 to 85 wt%.
[0027] In this invention, the mixing is preferably carried out in a mechanical mixer, and the mixing time is preferably 20 minutes.
[0028] After obtaining the precursor slurry, the present invention performs hydrothermal treatment on the precursor slurry to obtain the columnar alumina powder.
[0029] In this invention, the preferred temperature for hydrothermal treatment is 400-430℃, specifically 410, 420, or 425℃; the preferred pressure is 20-35 MPa, specifically 24, 30, or 33 MPa; and the preferred holding time is 12-72 hours, specifically 24, 48, or 70 hours. By controlling the parameters of hydrothermal treatment, this invention can ensure sufficient phase transformation of aluminum hydroxide while avoiding excessive grain growth.
[0030] The present invention preferably heats the temperature from room temperature to the temperature of the hydrothermal treatment at a heating rate of 1.5°C / min.
[0031] In this invention, a phase transformation occurs during the hydrothermal treatment process, and the phase transformation path is Al(OH)3→AlO(OH)→α-Al2O3.
[0032] In this invention, it is preferable to allow the product obtained after the hydrothermal treatment to cool naturally to room temperature.
[0033] In this invention, the hydrothermal treatment is preferably followed by cleaning. The cleaning is preferably performed by sequentially using ammonium citrate solution and water. The mass fraction of the ammonium citrate solution is preferably 10%. The electrostatic repulsion and surface complexation of the ammonium citrate solution are used to depolymerize the agglomerates obtained by the hydrothermal treatment. This invention does not have any special limitations on the specific operation method of cleaning. Conventional solid-liquid separation and washing methods in the art can be used.
[0034] The present invention also provides columnar alumina powder prepared by the preparation method described above. The morphology of the columnar alumina powder is controllable. The crystal length of the columnar alumina powder is preferably 1~22 μm, the aspect ratio is preferably 1.5~7, specifically 3, 4, 5 or 7, and the specific surface area is preferably 0.31~5.60 m². 2 / g, specifically 2.89, 3.37, 3.98 or 4.09m 2 / g.
[0035] To further illustrate the present invention, the solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0036] Example 1 10 kg of aluminum hydroxide with an average particle size of 10 μm and a purity of ≥99%, 10 kg of deionized water, 50 g of nucleation inducing agent (α-Al2O3), and 5 g of morphology modifier (4.5 g oxalic acid + 0.5 g citric acid) were mixed and stirred with a mechanical mixer for 20 min to obtain the precursor slurry. The precursor slurry was loaded into a crucible and placed in a reactor. The temperature was increased from room temperature to 400℃ at a rate of 1.5℃ / min, with a furnace pressure of 20MPa, and held at this temperature and pressure for 12 hours. After conversion, the mixture was cooled to room temperature, and the powder was removed. It was then subjected to a first wash in a 10wt% ammonium citrate solution, followed by washing with deionized water. The final product had crystal lengths of 1–10 μm, an aspect ratio of 5, and a specific surface area of 4.09 m². 2 / g columnar alumina powder; Figure 1 The image shown is the XRD pattern of the columnar alumina powder in Example 1. Figure 1 It can be seen that pure-phase α-Al2O3 was prepared in Example 1; Figure 2 These are scanning electron microscope (SEM) images of the columnar alumina powder in Example 1 at different magnifications. Figure 2 It can be seen that the columnar alumina powder prepared in Example 1 has good dispersibility and excellent columnar morphology of crystals.
[0037] Example 2 10 kg of aluminum hydroxide with an average particle size of 10 μm and a purity of ≥99%, 3 kg of deionized water, 100 g of nucleation inducing agent (α-Al2O3), and 25 g of morphology modifier (20 g boric acid + 5 g acetic acid) were mixed and stirred with a mechanical mixer for 20 min to obtain the precursor slurry. The precursor slurry was loaded into a crucible and placed in a reactor. The temperature was increased from room temperature to 430°C at a rate of 1.5°C / min, with a furnace pressure of 35 MPa, and held at this temperature and pressure for 72 hours. After conversion, the mixture was cooled to room temperature, and the powder was removed. It was then subjected to a first wash in a 10 wt% ammonium citrate solution, followed by washing with deionized water. The final product had crystal lengths of 13–22 μm, an aspect ratio of 1.5, and a specific surface area of 0.31 m². 2 / g columnar alumina powder; Figure 3 These are SEM images of the columnar alumina powder in Example 2 at different magnifications. Figure 3 It can be seen that the columnar powder prepared in Example 2 has a low aspect ratio and exhibits a short columnar morphology.
[0038] Example 3 10 kg of aluminum hydroxide with an average particle size of 10 μm and a purity of ≥99%, 5 kg of deionized water, 80 g of nucleation inducing agent (α-AlOOH), and 40 g of morphology modifier (25 g boric acid + 15 g oxalic acid) were mixed and stirred with a mechanical mixer for 20 min to obtain the precursor slurry. The precursor slurry was loaded into a crucible and placed in a reactor. The temperature was increased from room temperature to 400℃ at a rate of 1.5℃ / min, with a furnace pressure of 24MPa, and held at this temperature and pressure for 72 hours. After conversion, the mixture was cooled to room temperature, and the powder was removed. It was then subjected to a first wash in a 10wt% ammonium citrate solution, followed by washing with deionized water. The final product had crystal lengths of 4–13 μm, an aspect ratio of 4, and a specific surface area of 3.98 m². 2 / g columnar alumina powder.
[0039] Figure 4 These are SEM images of the columnar alumina powder in Example 3 at different magnifications. Figure 4 It can be seen that the columnar powder prepared in Example 3 has a medium aspect ratio and exhibits a columnar morphology.
[0040] Example 4 10 kg of aluminum hydroxide with an average particle size of 10 μm and a purity ≥99%, 1.8 kg of deionized water, 100 g of nucleation inducing agent (α-Al₂O₃), and 40 g of morphology modifier (15 g sulfuric acid + 25 g hydrochloric acid) were mixed and stirred with a mechanical stirrer for 20 min to obtain a slurry. The slurry was placed in a crucible and then placed in a reactor. The temperature was increased from room temperature to 400 °C at a rate of 1.5 °C / min, and the furnace pressure was 20 MPa. The temperature and pressure were maintained for 12 h. After conversion, the mixture was cooled to room temperature, and the powder was removed. It was then placed in a 10 wt% ammonium citrate solution for the first washing, followed by washing with deionized water. The final product had a crystal length of 1-5 μm, an aspect ratio of 7, and a specific surface area of 5.60 m². 2 / g columnar alumina powder.
[0041] Example 5 10 kg of aluminum hydroxide with an average particle size of 10 μm and a purity of ≥99%, 8 kg of deionized water, 50 g of nucleation inducing agent (10 g α-Fe2O3 + 40 g α-Al2O3), and 20 g of morphology modifier (8 g sulfuric acid + 12 g oxalic acid) were mixed and stirred with a mechanical mixer for 20 min to obtain the precursor slurry. The precursor slurry was loaded into a crucible and placed in a reactor. The temperature was increased from room temperature to 420°C at a rate of 1.5°C / min, with a furnace pressure of 30 MPa, and held at this temperature and pressure for 72 hours. After conversion, the mixture was cooled to room temperature, and the powder was removed. It was then subjected to a first wash in a 10 wt% ammonium citrate solution, followed by washing with deionized water. The final product had crystal lengths of 8–15 μm, an aspect ratio of 3, and a specific surface area of 2.89 m². 2 / g columnar alumina powder.
[0042] Example 6 10 kg of aluminum hydroxide with an average particle size of 10 μm and a purity of ≥99%, 10 kg of deionized water, 80 g of nucleation inducing agent (α-Al2O3), and 40 g of morphology modifier (25 g oxalic acid + 15 g citric acid) were mixed and stirred with a mechanical mixer for 20 min to obtain the precursor slurry. The precursor slurry was loaded into a crucible and placed in a reactor. The temperature was increased from room temperature to 410°C at a rate of 1.5°C / min, with a furnace pressure of 30 MPa, and held at this temperature and pressure for 24 hours. After conversion, the mixture was cooled to room temperature, and the powder was removed. It was then subjected to a first wash in a 10 wt% ammonium citrate solution, followed by washing with deionized water. The final product yielded crystals with a length of 10–15 μm, an aspect ratio of 4, and a specific surface area of 3.37 m². 2 / g columnar alumina powder.
[0043] Comparative Example 1 10 kg of aluminum hydroxide with an average particle size of 10 μm and a purity of ≥99%, 10 kg of deionized water, and 5 g of morphology modifier (4.5 g oxalic acid + 0.5 g citric acid) were mixed and stirred with a mechanical mixer for 20 min to obtain the precursor slurry. The precursor slurry was loaded into a crucible and placed in a reactor. The temperature was increased from room temperature to 400°C at a rate of 1.5°C / min, and the pressure inside the furnace was 20 MPa. The temperature and pressure were maintained for 12 hours. After the conversion was completed, the powder was cooled to room temperature and removed. It was then placed in a 10 wt% ammonium citrate solution for the first cleaning, and then cleaned with deionized water. The final powder was a mixture of boehmite and columnar alumina.
[0044] Figure 5 The XRD pattern of the powder prepared in Comparative Example 1; Figure 6 The SEM image of the powder prepared in Comparative Example 1 shows that the phase transformation of Comparative Example 1 without the addition of a nucleation inducing agent is incomplete, and platy boehmite is present.
[0045] Comparative Example 2 10 kg of aluminum hydroxide with an average particle size of 10 μm and a purity of ≥99%, 10 kg of deionized water, and 50 g of nucleation inducing agent (α-Al2O3) were mixed and stirred with a mechanical mixer for 20 min to obtain a precursor slurry. The precursor slurry was loaded into a crucible and placed in a reactor. The temperature was increased from room temperature to 400°C at a rate of 1.5°C / min, and the pressure inside the furnace was 20 MPa. The temperature and pressure were maintained for 12 hours. After the conversion was completed, the powder was cooled to room temperature, removed, and placed in a 10 wt% ammonium citrate solution for the first cleaning. Then it was cleaned with deionized water. The final powder obtained was polyhedral alumina.
[0046] Figure 7 The XRD pattern of the powder prepared in Comparative Example 2; Figure 8 The SEM image of the powder prepared in Comparative Example 2 shows that, without the addition of a morphology modifier, the crystals in Comparative Example 2 no longer have a columnar morphology.
[0047] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing columnar alumina powder, characterized in that, Includes the following steps: Aluminum hydroxide, water, and composite additives are mixed to obtain a precursor slurry; The precursor slurry was subjected to hydrothermal treatment to obtain the columnar alumina powder. The composite additive includes nucleation inducing agents and morphology modifiers.
2. The preparation method according to claim 1, characterized in that, The nucleation inducing agent includes one or more of α-Al₂O₃, α-Fe₂O₃, Cr₂O₃, and α-AlOOH.
3. The preparation method according to claim 1, characterized in that, The morphology modifier includes one or more of sulfuric acid, hydrochloric acid, oxalic acid, acetic acid, boric acid, and citric acid.
4. The preparation method according to claim 1, characterized in that, The hydrothermal treatment temperature is 400~430℃, the pressure is 20~35MPa, and the heat and pressure holding time is 12~72h.
5. The preparation method according to claim 1, characterized in that, The nucleation inducing agent is added at a rate of 0.5-1% of the mass of aluminum hydroxide; the morphology modifier is added at a rate of 0.05-0.4% of the mass of aluminum hydroxide.
6. The preparation method according to claim 1, characterized in that, The precursor slurry has a solid content of 50-85 wt%.
7. The preparation method according to claim 1, characterized in that, The aluminum hydroxide has an average particle size of 2~10μm and a purity of ≥99.9wt%.
8. The preparation method according to claim 1, characterized in that, The nucleation inducer has an average particle size of 2~10μm and a purity of ≥99wt%.
9. The preparation method according to claim 1, characterized in that, The hydrothermal treatment is followed by cleaning, which involves sequentially using an ammonium citrate solution and water, wherein the mass fraction of the ammonium citrate solution is 10%.
10. The columnar alumina powder prepared by the preparation method according to any one of claims 1 to 9, characterized in that, The columnar alumina powder has a crystal length of 1~22μm, an aspect ratio of 1.5~7, and a specific surface area of 0.31~5.60m². 2 / g.