A method for preparing highly crystalline indium tin oxide nanoparticles under microfluidic conditions

By using a microfluidic reactor and a segmented calcination process, the problems of uneven mixing, wide particle size distribution, and agglomeration in the preparation of ITO nanoparticles were solved, resulting in nanoparticles with high crystallinity and good dispersibility, which are suitable for industrial production.

CN123105704APending Publication Date: 2026-11-17KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611066019.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing ITO nanoparticle preparation technologies suffer from problems such as uneven mixing, wide particle size distribution, insufficient precursor crystallization and transformation, severe agglomeration, and poor batch repeatability, making it difficult to meet the quality requirements of high-end applications.

Method used

A two-stage process of co-precipitation-calcination under microfluidic conditions is adopted. The microfluidic reactor enables efficient mixing and precise control of the reactants. Combined with an online pH monitoring and feedback control system, the feed flow rate of the precipitant is adjusted. Subsequently, aging, washing, drying and staged calcination are carried out to transform it into highly crystalline ITO nanoparticles.

Benefits of technology

It achieves high crystallinity and good dispersibility of ITO nanoparticles, with precise particle size control, high product consistency, and suitability for industrial production, meeting the performance requirements of high-end applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105704A_ABST
    Figure CN123105704A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing highly crystalline indium tin oxide (ITO) nanoparticles under microfluidic conditions, comprising: preparing a mixed solution of precursors containing indium and tin sources and a precipitant solution; injecting them into a microfluidic reactor for rapid mixing and co-precipitation within a microchannel to obtain an ITO precursor suspension; obtaining an amorphous hydroxide precursor powder after aging, washing, and drying; and then forming highly crystalline ITO solid solution nanoparticles with a cubic indium manganese oxide crystal structure through a segmented calcination process. The ITO nanoparticles obtained by this invention have a primary particle size of 15–30 nm, a narrow particle size distribution, good dispersibility, and a high specific surface area; after sintering at 1580 °C, the ITO ceramic achieves a relative density of 98.46% and a resistivity as low as 3.532 × 10⁻⁶. ‑4 The sintering activity and conductivity are excellent, with a Ω·cm sintering capacity. This process is continuously controllable, easily scaled up linearly, and exhibits high batch repeatability, making it a promising candidate for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of nanomaterial preparation technology, and in particular to a method for preparing highly crystalline indium tin oxide nanoparticles under microfluidic conditions. Background Technology

[0002] Indium tin oxide (ITO) is a heavily doped, degenerate n-type semiconductor material. Due to its high transmittance (>80%) in the visible light region and high reflectivity in the infrared light region, it is widely used in flat panel displays, photovoltaic cells, touch screens, energy-saving glass, smart windows, organic light-emitting diodes (OLEDs), and aerospace.

[0003] In industry, magnetron sputtering is commonly used to prepare transparent conductive films using ITO targets. The performance of the target (such as density, resistivity, uniformity, etc.) directly depends on the quality of the ITO powder.

[0004] Currently, the main methods for preparing ITO nanoparticles include chemical coprecipitation, sol-gel method, hydrothermal method, and spray pyrolysis method.

[0005] Among these methods, chemical coprecipitation is considered the simplest and most economical. However, traditional coprecipitation methods still face many technical bottlenecks in large-scale applications:

[0006] 1. Uneven mixing: In traditional stirred tank reactors, the mixing efficiency of reactants is low, which can easily lead to problems such as excessively high or low local concentrations, resulting in asynchronous precipitation reactions and deviations of the product stoichiometry from the target composition.

[0007] 2. Large pH fluctuations: During the addition of the precipitant, the local pH value of the reaction system changes drastically, making it difficult to accurately control the crystal nucleation and growth process, resulting in a wide particle size distribution of the product.

[0008] 3. Incomplete precursor crystallization transformation: The co-precipitation method directly yields an amorphous mixed precipitate of indium hydroxide (In(OH)3) and tin hydroxide (Sn(OH)4), which must be calcined at high temperature to transform into an ITO solid solution with a functional cubic bixbyite crystal structure. In traditional processes, due to poor precursor particle uniformity and severe agglomeration, abnormal grain growth and incomplete crystallization are common during calcination, resulting in poor conductivity and low sintering activity in the final product.

[0009] 4. Severe agglomeration: ITO powder prepared by traditional methods is prone to hard agglomeration of primary particles, resulting in poor dispersibility and severely affecting the sintering density and conductivity of subsequent target materials.

[0010] 5. Poor batch repeatability: Due to the uneven mass and heat transfer in the macroscopic reactor, the product quality fluctuates greatly between different batches, making it difficult to meet the stringent requirements of high-end applications for powder consistency.

[0011] To overcome these shortcomings, researchers have tried improved techniques such as hydrothermal methods, sol-gel methods, and microwave-assisted methods. However, these methods often suffer from problems such as complex processes, high equipment costs, and low production efficiency, making it difficult to achieve large-scale industrial applications.

[0012] Microreactors have shown great potential for application in the field of nanomaterial synthesis in recent years. Microreactors achieve efficient mixing and precise control of reactants through microscale channels (typically tens to hundreds of micrometers), and have outstanding advantages such as fast reaction speed, high mass transfer efficiency, narrow residence time distribution, and good product uniformity.

[0013] However, research on the application of microfluidic technology to the continuous preparation of ITO nanoparticles is still very limited, and a mature and industrializable technical solution has not yet been formed.

[0014] Therefore, in order to solve the problems of uneven mixing, wide particle size distribution, insufficient precursor crystallization transformation, severe agglomeration, and poor batch repeatability in the existing ITO nanoparticle preparation technology, it is an urgent technical problem to be solved by those skilled in the art to provide a method for the continuous preparation of highly crystalline ITO nanoparticles under microfluidic conditions through a two-stage process of co-precipitation-calcination. Summary of the Invention

[0015] In view of this, the present invention provides a method for preparing highly crystalline indium tin oxide nanoparticles under microfluidic conditions.

[0016] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:

[0017] A method for preparing highly crystalline indium tin oxide nanoparticles under microfluidic conditions includes the following steps:

[0018] Step 1: Prepare the precursor solution by dissolving the indium source compound and the tin source compound in a solvent to prepare a mixed precursor solution;

[0019] Step 2: Prepare the precipitant solution;

[0020] Step 3: Microfluidic coprecipitation reaction. The precursor solution obtained in Step 1 and the precipitant solution obtained in Step 2 are injected into different inlets of the microfluidic reactor through independent delivery pumps. They are mixed and coprecipitated in the microchannel to obtain an ITO precursor suspension.

[0021] During the reaction, the feed flow rate of the precipitant solution is adjusted by an online pH monitoring and feedback control system to stabilize the pH value at the reaction outlet between 7.0 and 9.5.

[0022] Step 4: Aging. The ITO precursor suspension obtained in Step 3 is aged at 20℃~80℃ for 0.5 h~6 h.

[0023] Step 5: Washing and drying. The aged precipitate is washed, separated into solid and liquid phases, and dried to obtain amorphous ITO precursor powder.

[0024] Step Six: Segmented Calcination and Crystallization Transformation. The precursor powder obtained in Step Five is calcined in segments in an air or oxygen atmosphere to transform the amorphous hydroxide into an ITO solid solution with a cubic indium manganese oxide crystal structure, thereby obtaining a highly crystalline ITO nanoparticle product.

[0025] Preferably, in step one, the indium source compound is selected from one or more of InCl3·4H2O, In(NO3)3, and In2(SO4)3;

[0026] The tin source compound is selected from one or more of SnCl4·5H2O, SnCl2·2H2O, and sodium stannate.

[0027] The solvent is deionized water or ultrapure water.

[0028] Preferably, in step one, the molar ratio of indium source to tin source is set according to a mass ratio of In2O3 to SnO2 in the final product of 85:15 to 95:5.

[0029] The total concentration of In³⁺ in the precursor mixture solution is 0.05 mol / L to 1.0 mol / L.

[0030] Preferably, in step two, the precipitant is selected from one or more of ammonia, ammonium carbonate, sodium carbonate, and sodium hydroxide;

[0031] Its concentration ranges from 1 mol / L to 5 mol / L.

[0032] Preferably, in step three, the microfluidic reactor is a capillary microreactor, a microchannel chip reactor, or a tubular microreactor.

[0033] The microchannel diameter of the microfluidic reactor is 50 μm to 1000 μm;

[0034] The microchannel contains a micro-mixing structure;

[0035] The micro-hybrid structure is selected from one or more of the following: a split-convergence structure, an interlaced herringbone structure, and a micro-pillar array structure.

[0036] The microfluidic reactor is a continuous flow microreactor;

[0037] The precursor solution and precipitant solution are continuously injected in a continuous flow manner, and the ITO precursor suspension is continuously effluent in a continuous flow manner, thereby realizing the continuous preparation of ITO nanoparticle precursor.

[0038] Preferably, in step three, the feed flow rate of the precursor solution is 0.5 mL / min to 20 mL / min;

[0039] The feed flow rate of the precipitant solution is 0.5 mL / min to 20 mL / min; and the volume flow ratio of the precursor solution to the precipitant solution is 1:0.5 to 1:2.

[0040] Preferably, in step three, the temperature of the coprecipitation reaction is 10℃~90℃;

[0041] The outlet back pressure of the microfluidic reactor is 0.1 MPa to 2.0 MPa.

[0042] Preferably, in step six, the segmented calcination includes the following stages:

[0043] The first stage, the dehydroxylation stage: the temperature is increased to 200℃ to 400℃ at a rate of 1℃ / min to 5℃ / min, and held for 0.5 h to 2 h.

[0044] The second stage, the solution conversion stage: continue heating at a rate of 2℃ / min to 8℃ / min to 600℃ to 900℃, and hold for 1 h to 6 h.

[0045] Preferably, the second stage calcination temperature is 650℃~800℃, and the holding time is 2 h~4 h;

[0046] The heating rate during the entire calcination process is controlled at 1℃ / min to 10℃ / min.

[0047] The present invention achieves the following technical effects compared to the prior art:

[0048] (1) Excellent crystal quality: This invention can achieve a full and uniform transformation of amorphous precursors into cubic indium manganese oxide structure ITO solid solution. The resulting ITO nanoparticles are free of impurities, have sharp characteristic peaks, and have a crystallinity far higher than that of products prepared by traditional processes.

[0049] (2) Precise particle size control: This invention relies on instantaneous uniform mixing and explosive nucleation in microchannels to solve the problem of uneven local concentration in traditional methods. The resulting ITO nanoparticles can be controlled in the primary particle size range of 15 nm to 30 nm and the D50 can reach 22.75 nm, which has the characteristics of small particle size and narrow distribution.

[0050] (3) Good dispersion performance: The precipitation process of this invention is carried out in a uniform supersaturation environment, the formation and growth of crystal nuclei are controllable, and the precursor has no hard agglomeration; the segmented calcination process inhibits abnormal grain growth and sintering neck formation, and the final product has excellent dispersibility and a specific surface area of ​​more than 36.86 m² / g.

[0051] (4) Outstanding target material performance: This invention relies on the characteristics of small particle size, narrow distribution, high dispersion and high crystallinity of the powder, which significantly improves the sintering activity of the powder. After sintering at 1580℃ for 4 hours, the relative density of ITO ceramic can reach 98.46% and the resistivity is as low as 3.532×10 -4 Ω·cm, the sintered body is free of pores, and both densification and electrical conductivity reach excellent levels;

[0052] (5) Strong industrial adaptability: The present invention adopts microfluidic continuous flow process, the reaction only takes seconds to minutes, the equipment occupies little space, and linear scale-up can be achieved by increasing the number of microchannels or expanding the size of microchannels. It can smoothly complete the scale transition from laboratory to industrial production, and has good prospects for industrial application.

[0053] (6) High product stability: The mass transfer and heat transfer conditions of the microfluidic reactor of the present invention are precisely controllable and consistent from batch to batch. The quality fluctuation of products produced in different batches is small, which can meet the strict requirements of high-end applications for the consistency of ITO powder. Attached Figure Description

[0054] Figure 1 This is a flowchart of the present invention. Detailed Implementation

[0055] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0056] This invention discloses a method for preparing highly crystalline indium tin oxide nanoparticles under microfluidic conditions, comprising the following steps:

[0057] Step 1: Prepare the precursor solution by dissolving the indium source compound and the tin source compound in a solvent to prepare a mixed precursor solution;

[0058] Step 2: Prepare the precipitant solution;

[0059] Step 3: Microfluidic coprecipitation reaction. The precursor solution obtained in Step 1 and the precipitant solution obtained in Step 2 are injected into different inlets of the microfluidic reactor through independent delivery pumps. They are mixed and coprecipitated in the microchannel to obtain an ITO precursor suspension.

[0060] During the reaction, the feed flow rate of the precipitant solution is adjusted by an online pH monitoring and feedback control system to stabilize the pH value at the reaction outlet between 7.0 and 9.5.

[0061] Step 4: Aging. The ITO precursor suspension obtained in Step 3 is aged at 20℃~80℃ for 0.5 h~6 h.

[0062] Step 5: Washing and drying. The aged precipitate is washed, separated into solid and liquid phases, and dried to obtain amorphous ITO precursor powder.

[0063] Step Six: Segmented Calcination and Crystallization Transformation. The precursor powder obtained in Step Five is calcined in segments in an air or oxygen atmosphere to transform the amorphous hydroxide into an ITO solid solution with a cubic indium manganese oxide crystal structure, thereby obtaining a highly crystalline ITO nanoparticle product.

[0064] In step one, the indium source compound is selected from one or more of InCl3·4H2O, In(NO3)3, and In2(SO4)3;

[0065] The tin source compound is selected from one or more of SnCl4·5H2O, SnCl2·2H2O, and sodium stannate;

[0066] The solvent is deionized water or ultrapure water.

[0067] In step one, the molar ratio of indium source to tin source is set according to the mass ratio of In2O3 to SnO2 in the final product being 85:15 to 95:5.

[0068] The total concentration of In³⁺ in the precursor mixture solution was 0.05 mol / L to 1.0 mol / L.

[0069] In step two, the precipitant is selected from one or more of ammonia, ammonium carbonate, sodium carbonate, and sodium hydroxide;

[0070] Its concentration ranges from 1 mol / L to 5 mol / L.

[0071] In step three, the microfluidic reactor is a capillary microreactor, a microchannel chip reactor, or a tubular microreactor.

[0072] The microchannel diameter of the microfluidic reactor ranges from 50 μm to 1000 μm;

[0073] The microchannel contains a micro-mixing structure;

[0074] The micro-mixing structure is selected from one or more of the following: split-flow-merge structure, staggered herringbone structure, and micro-pillar array structure;

[0075] The microfluidic reactor is a continuous flow microreactor;

[0076] The precursor solution and precipitant solution are continuously injected in a continuous flow manner, while the ITO precursor suspension is continuously effluent in a continuous flow manner, thereby realizing the continuous preparation of ITO nanoparticle precursor.

[0077] In step three, the feed flow rate of the precursor solution is 0.5 mL / min to 20 mL / min;

[0078] The feed flow rate of the precipitant solution is 0.5 mL / min to 20 mL / min; and the volume flow ratio of the precursor solution to the precipitant solution is 1:0.5 to 1:2.

[0079] In step three, the temperature of the coprecipitation reaction is 10℃~90℃;

[0080] The outlet back pressure of the microfluidic reactor is 0.1 MPa to 2.0 MPa.

[0081] Step six, segmented calcination, includes the following stages:

[0082] The first stage, the dehydroxylation stage: the temperature is increased to 200℃ to 400℃ at a rate of 1℃ / min to 5℃ / min, and held for 0.5 h to 2 h.

[0083] The second stage, the solution conversion stage: continue heating at a rate of 2℃ / min to 8℃ / min to 600℃ to 900℃, and hold for 1 h to 6 h.

[0084] The second stage of calcination is at a temperature of 650℃~800℃, and the holding time is 2 h~4 h;

[0085] The heating rate during the entire calcination process is controlled at 1℃ / min to 10℃ / min.

[0086] Example 1

[0087] Step 1: Prepare the precursor solution

[0088] Weigh out 5.86 g of InCl3·4H2O (purity ≥99.99%) and 0.70 g of SnCl4·5H2O (purity ≥99.99%), so that the molar ratio of In to Sn satisfies In2O3:SnO2=90:10.

[0089] Dissolve the above raw materials in 200 mL of deionized water and stir until completely dissolved to prepare a precursor mixed solution (In). 3+ The total concentration is approximately 0.1 mol / L.

[0090] Step 2: Prepare the precipitant solution

[0091] Take 28% concentrated ammonia solution and dilute it with deionized water to 2 mol / L to prepare a precipitant solution.

[0092] Step 3: Microfluidic coprecipitation reaction

[0093] A capillary microreactor with a hydraulic diameter of 250 μm was used as a microfluidic reactor, and its microchannel was equipped with a split-flow-convergence micro-mixing structure.

[0094] The precursor solution and precipitant solution were injected into the two inlets of the microreactor at flow rates of 2 mL / min and 1.5 mL / min, respectively, using two precision injection pumps (the volumetric flow rate ratio was approximately 1:0.75).

[0095] The reaction temperature is controlled at 30℃ using a constant-temperature water bath. A back pressure valve is installed at the reactor outlet to control the back pressure at 0.5MPa.

[0096] An online pH meter is installed at the reaction outlet to monitor the pH value in real time and adjust the flow rate of the precipitant through feedback control to keep the outlet pH value stable at 8.5±0.2.

[0097] The reactants remain in the microchannel for about 5 to 10 seconds, and the ITO precursor suspension flows out continuously from the outlet.

[0098] Step 4: Aging

[0099] The collected ITO precursor suspension was aged at 50°C for 2 h.

[0100] Step 5: Washing and Drying

[0101] The aged suspension was centrifuged (8000 rpm, 10 min), the supernatant was discarded, and the precipitate was washed repeatedly with deionized water 6 times until no Cl was detected in the washing solution using AgNO3 solution. - .

[0102] The washed precipitate was dried in an oven at 80°C for 12 h to obtain amorphous ITO precursor powder.

[0103] Step Six: Segmented Calcination and Crystallization Transformation

[0104] The dried amorphous ITO precursor powder was placed in a tube furnace and calcined in stages under an air atmosphere.

[0105] First stage: The temperature is increased from room temperature to 300℃ at a rate of 3℃ / min and held for 1 h to allow In(OH)3 and Sn(OH)4 to fully dehydrate and decompose into In2O3 and SnO2.

[0106] Second stage: Continue heating at a rate of 5℃ / min to 750℃, hold for 3 hours, and allow Sn to... 4+ It diffuses fully into the In2O3 lattice to form a highly crystalline ITO solid solution with a cubic indium manganese oxide structure.

[0107] After calcination, the furnace was cooled to room temperature to obtain ITO nanoparticles.

[0108] Product performance characterization:

[0109] XRD analysis: The XRD pattern of the prepared product showed that all diffraction peaks were in high agreement with the cubic In2O3 standard card (JCPDS No. 06-0416), and there were no SnO2 or other impurity phase peaks, indicating that Sn... 4+ It has been completely dissolved into the In2O3 lattice and has good crystallinity.

[0110] TEM observation: The particles are spherical, well dispersed, without hard agglomeration, and the average particle size is about 22.75 nm.

[0111] BET specific surface area: 36.86 m² / g.

[0112] Sintering performance: After sintering the obtained powder at 1580℃ for 4 hours, the ITO ceramic achieved a relative density of 98.46% and a resistivity of 3.532×10⁻⁶. -4 Ω·cm.

[0113] Example 2:

[0114] Step 1: Prepare the precursor solution

[0115] Weigh out 11.72 g InCl3·4H2O (purity ≥99.99%) and 1.40 g SnCl4·5H2O (purity ≥99.99%), so that the molar ratio of In to Sn satisfies In2O3:SnO2=90:10.

[0116] Dissolve the above raw materials in 200 mL of deionized water and stir until completely dissolved to prepare a precursor mixed solution (total In³⁺ concentration is approximately 0.2 mol / L).

[0117] Steps two through five: Same as in Example 1.

[0118] Step Six: Segmented Calcination and Crystallization Transformation

[0119] First stage: Increase the temperature to 350℃ at a rate of 2℃ / min and keep it warm for 1 hour.

[0120] Second stage: Increase the temperature to 800℃ at a rate of 4℃ / min and keep warm for 2 hours.

[0121] Product performance characterization:

[0122] The prepared ITO nanoparticles are ellipsoidal in shape, have good crystallinity, and XRD shows a pure-phase cubic structure with an average particle size of about 25 nm and a narrow particle size distribution.

[0123] The resistivity of the powder is approximately (1.56±0.19) Ω·cm.

[0124] Example 3:

[0125] Step 1: Prepare the precursor solution

[0126] Weigh 29.30 g InCl3·4H2O (purity ≥99.99%) and 3.50 g SnCl4·5H2O (purity ≥99.99%), so that the molar ratio of In to Sn satisfies In2O3:SnO2=90:10.

[0127] Dissolve the above raw materials in 200 mL of deionized water and stir until completely dissolved to prepare a precursor mixed solution (total In³⁺ concentration is approximately 0.5 mol / L).

[0128] Steps two through five: Same as in Example 1.

[0129] Step Six: Segmented Calcination and Crystallization Transformation

[0130] First stage: Increase the temperature to 250℃ at a rate of 5℃ / min and hold for 0.5 h.

[0131] Second stage: Increase to 700℃ at 6℃ / min and keep warm for 4 hours.

[0132] Product performance characterization:

[0133] The prepared ITO nanoparticles have a particle size of approximately 28 nm, are spherical, and have good dispersibility. XRD shows a pure-phase cubic structure.

[0134] Example 4: Continuous Production

[0135] A multi-channel parallel microfluidic reactor was adopted, with each channel having a hydraulic diameter of 500 μm, and a total of 10 channels operating in parallel.

[0136] The precursor solution (total concentration of In³⁺ 0.15 mol / L) was continuously injected into the reactor at a total flow rate of 10 mL / min, and the precipitant solution (2 mol / L ammonia water) was continuously injected at a total flow rate of 7.5 mL / min. The reaction temperature was controlled at 35℃.

[0137] The subsequent aging, washing, drying, and segmented calcination processes are the same as in Example 1.

[0138] This embodiment enables continuous production of ITO precursor suspension with a throughput of up to 17.5 mL / min. The capacity can be further increased by increasing the number of channels.

[0139] Comparative Example 1: Traditional Coprecipitation Method

[0140] The coprecipitation reaction was carried out using a traditional stirred tank reactor: the precursor solution (0.1 mol / L, In:Sn=90:10) was placed in a 2L beaker, and 2 mol / L ammonia solution was slowly added dropwise under vigorous stirring, with the final pH controlled at 8.5.

[0141] The resulting precipitate was aged, washed, and dried, and then directly calcined at 750℃ for 3 hours (without a segmented process).

[0142] The resulting product has a wide particle size distribution (20–200 nm), severe hard agglomeration between particles, and significant broadening of XRD diffraction peaks.

[0143] Under the same sintering conditions, the relative density of the ceramic was only 92.3%, and the resistivity was 8.7 × 10⁻⁶. -4 The Ω·cm value indicates that the performance is significantly inferior to that of Example 1.

[0144] As can be seen, this invention achieves co-precipitation reaction under uniform supersaturation through a microfluidic reactor, and combined with a segmented calcination process, it solves the problems of wide particle size distribution, severe agglomeration, and insufficient crystallinity of ITO nanoparticles obtained by traditional methods. The final product shows significant advantages in both powder characteristics and target sintering performance, and can meet the performance requirements of high-end ITO targets for raw materials, making it suitable for industrial continuous production.

[0145] The above description is merely a preferred embodiment of the present invention and does not constitute any limitation on the technical scope of the present invention. Therefore, any minor modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention shall still fall within the scope of the technical solution of the present invention.

Claims

1. A method for preparing highly crystalline indium tin oxide nanoparticles under microfluidic conditions, characterized in that, Includes the following steps: Step 1: Prepare the precursor solution by dissolving the indium source compound and the tin source compound in a solvent to prepare a mixed precursor solution; Step 2: Prepare the precipitant solution; Step 3: Microfluidic coprecipitation reaction. The precursor solution obtained in Step 1 and the precipitant solution obtained in Step 2 are injected into different inlets of the microfluidic reactor through independent delivery pumps. They are mixed and coprecipitated in the microchannel to obtain an ITO precursor suspension. During the reaction, the feed flow rate of the precipitant solution is adjusted by an online pH monitoring and feedback control system to stabilize the pH value at the reaction outlet between 7.0 and 9.

5. Step 4: Aging. The ITO precursor suspension obtained in Step 3 is aged at 20℃~80℃ for 0.5 h~6 h. Step 5: Washing and drying. The aged precipitate is washed, separated into solid and liquid phases, and dried to obtain amorphous ITO precursor powder. Step Six: Segmented Calcination and Crystallization Transformation. The precursor powder obtained in Step Five is calcined in segments in an air or oxygen atmosphere to transform the amorphous hydroxide into an ITO solid solution with a cubic indium manganese oxide crystal structure, thereby obtaining a highly crystalline ITO nanoparticle product.

2. The method for preparing highly crystalline indium tin oxide nanoparticles under microfluidic conditions according to claim 1, characterized in that, In step one, the indium source compound is selected from one or more of InCl3·4H2O, In(NO3)3, and In2(SO4)3; The tin source compound is selected from one or more of SnCl4·5H2O, SnCl2·2H2O, and sodium stannate. The solvent is deionized water or ultrapure water.

3. The method for preparing highly crystalline indium tin oxide nanoparticles under microfluidic conditions according to claim 1, characterized in that, In step one, the molar ratio of indium source to tin source is set according to the mass ratio of In2O3 to SnO2 in the final product being 85:15 to 95:

5. In the precursor mixture solution 3+ The total concentration is 0.05 mol / L to 1.0 mol / L.

4. The method for preparing highly crystalline indium tin oxide nanoparticles under microfluidic conditions according to claim 1, characterized in that, In step two, the precipitant is selected from one or more of ammonia, ammonium carbonate, sodium carbonate, and sodium hydroxide. Its concentration ranges from 1 mol / L to 5 mol / L.

5. The method for preparing highly crystalline indium tin oxide nanoparticles under microfluidic conditions according to claim 1, characterized in that, In step three, the microfluidic reactor is a capillary microreactor, a microchannel chip reactor, or a tubular microreactor. The microchannel diameter of the microfluidic reactor is 50 μm to 1000 μm; The microchannel contains a micro-mixing structure; The micro-hybrid structure is selected from one or more of the following: a split-convergence structure, an interlaced herringbone structure, and a micro-pillar array structure. The microfluidic reactor is a continuous flow microreactor; The precursor solution and precipitant solution are continuously injected in a continuous flow manner, and the ITO precursor suspension is continuously effluent in a continuous flow manner, thereby realizing the continuous preparation of ITO nanoparticle precursor.

6. The method for preparing highly crystalline indium tin oxide nanoparticles under microfluidic conditions according to claim 1, characterized in that, In step three, the feed flow rate of the precursor solution is 0.5 mL / min to 20 mL / min; The feed flow rate of the precipitant solution is 0.5 mL / min to 20 mL / min; and the volume flow ratio of the precursor solution to the precipitant solution is 1:0.5 to 1:

2.

7. The method for preparing highly crystalline indium tin oxide nanoparticles under microfluidic conditions according to claim 1, characterized in that, In step three, the temperature of the coprecipitation reaction is 10℃~90℃; The outlet back pressure of the microfluidic reactor is 0.1 MPa to 2.0 MPa.

8. The method for preparing highly crystalline indium tin oxide nanoparticles under microfluidic conditions according to claim 1, characterized in that, Step six, segmented calcination, includes the following stages: The first stage, the dehydroxylation stage: the temperature is increased to 200℃ to 400℃ at a rate of 1℃ / min to 5℃ / min, and held for 0.5 h to 2 h; The second stage, the solution conversion stage: continue heating at a rate of 2℃ / min to 8℃ / min to 600℃ to 900℃, and hold for 1 h to 6 h.

9. The method for preparing highly crystalline indium tin oxide nanoparticles under microfluidic conditions according to claim 8, characterized in that, The second stage calcination temperature is 650℃~800℃, and the holding time is 2 h~4 h; The heating rate during the entire calcination process is controlled at 1℃ / min to 10℃ / min.