Optical glass and optical components

By controlling the composition and proportion of optical glass, optical glass with excellent melting properties and thermal stability is prepared, solving the problem of insufficient uniformity of optical glass in the prior art and meeting the high-performance requirements of optical components.

CN123105975APending Publication Date: 2026-11-17HOYA CORPORATION +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610655446.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2026-04-06
Filing Date
2026-05-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to manufacture optical glass with excellent melting properties and thermal stability, especially when it is not possible to obtain materials for optical components with sufficient uniformity without using containerless solidification methods.

Method used

By controlling the composition of optical glass and ensuring that the content and ratio of components such as SiO2, B2O3, La2O3, and Nb2O5 meet specific mass ratios, optical glass with excellent melting properties and thermal stability can be prepared.

Benefits of technology

Optical glass with high melting and thermal stability has been achieved, making it suitable for the manufacture of optical components and improving the uniformity and performance of the glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105975A_ABST
    Figure CN123105975A_ABST
Patent Text Reader

Abstract

In the optical glass of the present invention, the contents of SiO2, B2O3, La2O3, Nb2O5, the total contents of SiO2 and B2O3, Ln2O3, the mass ratio of Ln2O3 to the total contents of SiO2 and B2O3, the total contents of Nb2O5, TiO2, WO3 and Ta2O5, the mass ratio of TiO2 to the total contents of SiO2 and B2O3, and the values ​​obtained by subtracting the contents of Nb2O5, TiO2, WO3 and Ta2O5 from the contents of Ln2O3 are all given ranges, and the mass ratio y of Ln2O3 to the total contents of Ln2O3, SiO2 and B2O3 and the mass ratio x of Ln2O3 to the total contents of Ln2O3, Nb2O5, TiO2, WO3 and Ta2O5 satisfy y ≥ -0.7058x + 1.38.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to optical glass and optical components. Background Technology

[0002] Optical glass is useful as a material for optical components such as lenses (see, for example, Patent Document 1).

[0003] Existing technical documents

[0004] Patent documents

[0005] Patent Document 1: Japanese Patent Application Publication No. 2016-011228 Summary of the Invention

[0006] The problem that the invention aims to solve

[0007] Patent Document 1 discloses a containerless solidification method for manufacturing optical glass. The containerless solidification method is a method for manufacturing optical glass by melting and cooling a glass raw material block while it is suspended in a container. In cases where the glass composition has low melt flowability and thermal stability, it is generally difficult to obtain glass with uniformity suitable for use as a material in optical components without using the containerless solidification method. In contrast, a method for manufacturing optical glass with excellent melt flowability and thermal stability is not limited to the containerless solidification method, and is therefore more ideal.

[0008] In view of the above, one aspect of the present invention aims to provide optical glass with excellent melting properties and thermal stability.

[0009] Problem Solving Methods

[0010] One aspect of the present invention is described below.

[0011] [1] An optical glass, wherein,

[0012] Based on quality standards,

[0013] The SiO2 content is above 2.50% and below 15.00%.

[0014] The B2O3 content is above 2.00% and below 17.50%.

[0015] The La2O3 content is above 40.00%.

[0016] The Nb₂O₅ content is greater than 0.00% and less than 14.00%.

[0017] The total content of SiO2 and B2O3 (SiO2+B2O3) is above 14.00% and below 20.00%.

[0018] Rare earth oxides (La₂O₃, Gd₂O₃, Y₂O₃, and Yb₂O₃) are represented as Ln₂O₃.

[0019] The Ln2O3 content is the total content of La2O3, Gd2O3, Y2O3, and Yb2O3 (La2O3+Gd2O3+Y2O3+Yb2O3).

[0020] The Ln2O3 content is above 50.00%.

[0021] The mass ratio of Ln2O3 content to the total content of SiO2 and B2O3 (Ln2O3 / (SiO2+B2O3)) is greater than 3.41.

[0022] The total content of Nb2O5, TiO2, WO3, and Ta2O5 (Nb2O5+TiO2+WO3+Ta2O5) is less than 14.00%.

[0023] The mass ratio of TiO2 content to the total content of SiO2 and B2O3 (TiO2 / (SiO2+B2O3)) is less than 0.17.

[0024] The value obtained by subtracting the contents of Nb2O5, TiO2, WO3, and Ta2O5 from the Ln2O3 content (Ln2O3-Nb2O5-TiO2-WO3-Ta2O5) is over 49.00%, and...

[0025] Let y be the mass ratio of Ln2O3 content to the total content of Ln2O3, SiO2, and B2O3 (Ln2O3 / (Ln2O3+SiO2+B2O3)).

[0026] And with the mass ratio of Ln2O3 content to the total content of Ln2O3, Nb2O5, TiO2, WO3, and Ta2O5 (Ln2O3 / (Ln2O3+Nb2O5+TiO2+WO3+Ta2O5)) set as x,

[0027] The condition y ≥ -0.7058x + 1.38 is satisfied.

[0028] [2] According to the optical glass described in [1], wherein,

[0029] The Ta2O5 content is above 0.00% and below 15.00%.

[0030] [3] The optical glass according to [1] or [2], wherein,

[0031] The total content of SiO2, B2O3 and P2O5 (SiO2+B2O3+P2O5) is above 14.00% and below 19.50%.

[0032] [4] The optical glass according to any one of [1] to [3], wherein,

[0033] The mass ratio of Ln2O3 content to the total content of Ln2O3, Nb2O5, TiO2, WO3 and Ta2O5 (Ln2O3 / (Ln2O3+Nb2O5+TiO2+WO3+Ta2O5)) is greater than 0.845.

[0034] [5] The optical glass according to any one of [1] to [4], wherein,

[0035] The total content of ZnO, ZrO2, Nb2O5, TiO2, WO3 and Ta2O5 (ZnO+ZrO2+Nb2O5+TiO2+WO3+Ta2O5) is above 6.00%.

[0036] [6] The optical glass according to any one of [1] to [5] satisfies y≥-0.2797x+1.0181.

[0037] [7] The optical glass according to any one of [1] to [6], wherein,

[0038] The refractive index nd and the Abbe number νd satisfy the following equation:

[0039] nd≥-0.01000×νd+2.28500.

[0040] [8] The optical glass according to any one of [1] to [7], wherein,

[0041] The Ta2O5 content is above 0.00% and below 15.00%.

[0042] The total content of SiO2, B2O3, and P2O5 (SiO2+B2O3+P2O5) is above 14.00% and below 19.50%.

[0043] The mass ratio of Ln2O3 content to the total content of Ln2O3, Nb2O5, TiO2, WO3, and Ta2O5 (Ln2O3 / (Ln2O3+Nb2O5+TiO2+WO3+Ta2O5)) is greater than 0.845.

[0044] The total content of ZnO, ZrO2, Nb2O5, TiO2, WO3, and Ta2O5 (ZnO+ZrO2+Nb2O5+TiO2+WO3+Ta2O5) is above 6.00%.

[0045] It satisfies y ≥ -0.2797x + 1.0181, and

[0046] The refractive index nd and the Abbe number νd satisfy the following equation:

[0047] nd≥-0.01000×νd+2.28500.

[0048] [9] An optical element made of any one of the optical glass described in [1] to [8].

[0049] The effects of the invention

[0050] According to one aspect of the present invention, optical glass with excellent melting properties and thermal stability can be provided. Furthermore, according to another aspect of the present invention, optical elements made from such optical glass can also be provided. Attached Figure Description

[0051] Figure 1 An example of a glass molding manufacturing apparatus is shown.

[0052] Figure 2 This is an illustrative diagram showing an example of a method for controlling the speed at which glass is removed from a through-hole.

[0053] Figure 3 This is an explanatory diagram showing a specific example of a method for cutting a glass molded body.

[0054] Figure 4 This is an explanatory diagram showing a specific example of a method for cutting a glass molded body.

[0055] Figure 5 This is an explanatory diagram showing a specific example of a method for cutting a glass molded body.

[0056] Figure 6 The comparison results of the melting properties of the comparative example (Photo A) and Example 1 No. 60 (Photo B) are shown. Detailed Implementation

[0057] Optical Glass

[0058] <Glass Composition>

[0059] In this invention and specification, glass composition is expressed as an oxide-based glass composition. Here, "oxide-based glass composition" refers to a glass composition obtained by converting it to a composition that exists in the glass as oxides when the glass raw material is completely decomposed during melting. Furthermore, unless otherwise stated, glass composition is expressed as a mass basis (mass%, mass ratio).

[0060] The glass composition described in this invention and specification can be determined, for example, by methods such as ICP-AES (Inductively Coupled Plasma-Atomic Emision Spectrometry). Quantitative analysis can be performed on each element separately using ICP-AES. The analytical values ​​are then converted to oxide representations. ICP-AES-based analytical values ​​sometimes contain, for example, a measurement error of about ±5% of the analytical value. Therefore, the oxide representations converted from the analytical values ​​sometimes also contain an error of about ±5%.

[0061] Furthermore, in this invention and this specification, the content of a constituent element being 0.00% or not containing or not introduced means that the constituent element is substantially not contained, implying that the content of the constituent element is below the level of impurities. "Below the level of impurities" means, for example, less than 0.01%.

[0062] The glass composition of the aforementioned optical glass (also referred to as "glass") will be explained in further detail below.

[0063] SiO2 is a component that helps improve the melting and thermal stability of glass.

[0064] From the viewpoint of maintaining the meltability and thermal stability of the glass, the SiO2 content is 2.50% or more, preferably 2.70% or more, and more preferably 2.90% or more, 3.10% or more, 3.30% or more, 3.50% or more, 3.70% or more, 3.90% or more, 4.00% or more, 4.10% or more, 4.30% or more, 4.40% or more, 4.50% or more, 4.60% or more, 4.70% or more, 4.80% or more, 4.90% or more, 5.00% or more, 5.10% or more, 5.20% or more, 5.30% or more, 5.40% or more, 5.50% or more, and 5.60% or more.

[0065] On the other hand, from the viewpoint of maintaining a high refractive index of the glass, the SiO2 content is 15.00% or less, preferably 14.50% or less, and more preferably 14.00% or less, 13.50% or less, 13.00% or less, 12.50% or less, 12.00% or less, 11.50% or less, 11.30% or less, 11.10% or less, 11.00% or less, 10.90% or less, 10.80% or less, 10.70% or less, 10.60% or less, 10.50% or less, 10.40% or less, 10.30% or less, 10.20% or less, 10.10% or less, 10.00% or less, 9.90% or less, 9.80% or less, and 9.70% or less.

[0066] B2O3 is also a component that helps improve the meltability and thermal stability of glass.

[0067] From the viewpoint of maintaining the meltability and thermal stability of the glass, the B2O3 content is 2.00% or more, preferably 2.50% or more, and more preferably 3.00% or more, 3.50% or more, 4.00% or more, 4.50% or more, 5.00% or more, 5.50% or more, 6.00% or more, 6.50% or more, 7.00% or more, 7.10% or more, 7.20% or more, 7.30% or more, 7.40% or more, 7.50% or more, 7.60% or more, 7.70% or more, 7.80% or more, 7.90% or more, and 8.00% or more.

[0068] On the other hand, from the viewpoint of maintaining a high refractive index of the glass, the B2O3 content is 17.50% or less, preferably 17.00% or less, and more preferably 16.50% or less, 16.00% or less, 15.50% or less, 15.00% or less, 14.50% or less, 14.00% or less, 13.50% or less, 13.40% or less, 13.30% or less, 13.20% or less, 13.10% or less, 13.00% or less, 12.90% or less, 12.80% or less, 12.70% or less, 12.60% or less, 12.50% or less, 12.40% or less, 12.30% or less, 12.20% or less, 12.10% or less, and 12.00% or less.

[0069] From the viewpoint of maintaining the meltability and thermal stability of the glass, the total content of SiO2 and B2O3 (SiO2+B2O3) is 14.00% or more, preferably 14.10% or more, and more preferably 14.20% or more, 14.30% or more, 14.40% or more, 14.50% or more, 14.60% or more, 14.70% or more, 14.80% or more, 14.90% or more, 15.00% or more, 15.10% or more, 15.20% or more, 15.30% or more, 15.40% or more, 15.50% or more, 15.60% or more, 15.70% or more, 15.80% or more, 15.90% or more, and 16.00% or more.

[0070] On the other hand, from the viewpoint of maintaining a high refractive index of the glass, the total content (SiO2+B2O3) is 20.00% or less, preferably 19.90% or less, and more preferably 19.80% or less, 19.70% or less, 19.60% or less, 19.50% or less, 19.40% or less, 19.30% or less, 19.20% or less, 19.10% or less, 19.00% or less, 18.90% or less, and 18.80% or less.

[0071] From the viewpoint of maintaining the thermal stability of the glass and maintaining a high refractive index, the mass ratio of SiO2 to the total content of SiO2 and B2O3 (SiO2 / (SiO2+B2O3)) is preferably 0.65 or less, more preferably 0.64 or less, and even more preferably 0.63 or less, 0.62 or less, 0.61 or less, 0.60 or less, 0.59 or less, 0.58 or less, 0.57 or less, 0.56 or less, 0.55 or less, 0.54 or less, 0.53 or less, 0.52 or less, 0.51 or less, and 0.50 or less.

[0072] On the other hand, from the viewpoint of maintaining the meltability and thermal stability of the glass, the mass ratio (SiO2 / (SiO2+B2O3)) is preferably 0.05 or more, more preferably 0.10 or more, and even more preferably 0.15 or more, 0.20 or more, 0.25 or more, 0.26 or more, 0.27 or more, 0.28 or more, 0.29 or more, 0.30 or more, 0.31 or more, 0.32 or more, 0.33 or more, and 0.34 or more.

[0073] P2O5 is a component that helps improve the thermal stability of glass.

[0074] The P2O5 content can be 0.00%, above 0.00%, or greater than 0.00%.

[0075] From the viewpoint of maintaining the meltability and thermal stability of the glass, the P2O5 content is preferably 0.00% or more, more preferably 0.10% or more, and even more preferably 0.20% or more, 0.30% or more, 0.40% or more, and 0.50% or more.

[0076] On the other hand, from the viewpoint of maintaining a high refractive index of the glass, the P2O5 content is preferably 10.00% or less, more preferably 9.50% or less, and even more preferably 9.00% or less, 8.50% or less, 8.00% or less, 7.50% or less, 7.00% or less, 6.50% or less, 6.00% or less, 5.50% or less, 5.00% or less, 4.50% or less, 4.00% or less, 3.50% or less, 3.00% or less, 2.50% or less, and 2.00% or less.

[0077] From the viewpoint of maintaining the meltability and thermal stability of the glass, the total content of SiO2, B2O3 and P2O5 (SiO2+B2O3+P2O5) is preferably 14.00% or more, more preferably 14.10% or more, and even more preferably 14.20% or more, 14.30% or more, 14.40% or more, 14.50% or more, 14.60% or more, 14.70% or more, 14.80% or more, 14.90% or more, 15.00% or more, 15.10% or more, 15.20% or more, 15.30% or more, 15.40% or more, 15.50% or more, 15.60% or more, 15.70% or more, 15.80% or more, 15.90% or more, and 16.00% or more.

[0078] On the other hand, from the viewpoint of maintaining a high refractive index of the glass, the total content (SiO2+B2O3+P2O5) is preferably 20.00% or less, more preferably 19.90% or less, and even more preferably 19.80% or less, 19.70% or less, 19.60% or less, 19.50% or less, 19.40% or less, 19.30% or less, 19.20% or less, 19.10% or less, 19.00% or less, 18.90% or less, and 18.80% or less.

[0079] Al2O3 is also a component that helps improve the thermal stability of glass.

[0080] The Al2O3 content can be 0.00%, more than 0.00%, or greater than 0.00%.

[0081] From the viewpoint of maintaining the meltability and thermal stability of the glass, the Al2O3 content is preferably 0.00% or more, more preferably 0.10% or more, and even more preferably 0.20% or more, 0.30% or more, 0.40% or more, and 0.50% or more.

[0082] On the other hand, from the viewpoint of maintaining a high refractive index of the glass, the Al2O3 content is preferably 10.00% or less, more preferably 9.50% or less, and even more preferably 9.00% or less, 8.50% or less, 8.00% or less, 7.50% or less, 7.00% or less, 6.50% or less, 6.00% or less, 5.50% or less, 5.00% or less, 4.50% or less, 4.00% or less, 3.50% or less, 3.00% or less, 2.50% or less, and 2.00% or less.

[0083] In this invention and specification, rare earth oxides (La₂O₃, Gd₂O₃, Y₂O₃, and Yb₂O₃) are referred to as Ln₂O₃, and the Ln₂O₃ content is the total content of La₂O₃, Gd₂O₃, Y₂O₃, and Yb₂O₃ (La₂O₃ + Gd₂O₃ + Y₂O₃ + Yb₂O₃). Rare earth oxides are components that help maintain the high refractive index and low dispersion of glass.

[0084] From the viewpoint of maintaining a high refractive index and low dispersion of the glass, the Ln2O3 content is 50.00% or more, preferably 50.50% or more, and more preferably 51.00% or more, 51.50% or more, 52.00% or more, 52.50% or more, 53.00% or more, 53.50% or more, 54.00% or more, 54.50% or more, 55.00% or more, 55.50% or more, 56.00% or more, 56.50% or more, 57.00% or more, 57.50% or more, 58.00% or more, 58.50% or more, 59.00% or more, 59.50% or more, 60.00% or more, 60.50% or more, 61.00% or more, 61.50% or more, and 62.00% or more.

[0085] On the other hand, from the viewpoint of suppressing the rise of the glass transition temperature Tg and maintaining the meltability and thermal stability of the glass, the Ln2O3 content is preferably 75.00% or less, more preferably 74.50% or less, and even more preferably 74.00% or less, 73.50% or less, 73.00% or less, 72.50% or less, 72.00% or less, 71.50% or less, 71.00% or less, 70.50% or less, 70.00% or less, 69.50% or less, 69.00% or less, 68.50% or less, 68.00% or less, 67.50% or less, and 67.00% or less.

[0086] From the viewpoint of maintaining a high refractive index and low dispersion of the glass, the La2O3 content is 40.00% or more, preferably 40.20% or more, and more preferably 40.40% or more, 40.60% or more, 40.80% or more, 41.00% or more, 41.20% or more, 41.40% or more, 41.60% or more, 41.80% or more, 42.00% or more, 42.20% or more, 42.40% or more, 42.60% or more, 42.80% or more, 43.00% or more, 43.20% or more, 43.40% or more, 43.60% or more, 43.80% or more, 44.00% or more, 44.20% or more, 44.40% or more, 44.60% or more, 44.80% or more, and 45.00% or more.

[0087] On the other hand, from the viewpoint of suppressing the rise of the glass transition temperature Tg and maintaining the meltability and thermal stability of the glass, the La2O3 content is preferably 70.00% or less, more preferably 69.00% or less, and even more preferably 68.00% or less, 67.00% or less, 66.00% or less, 65.00% or less, 64.80% or less, 64.60% or less, 64.40% or less, 64.20% or less, 64.00% or less, 63.80% or less, 63.60% or less, 63.40% or less, 63.20% or less, 63.00% or less, 62.80% or less, 62.60% or less, 62.40% or less, 62.20% or less, and 62.00% or less.

[0088] The Gd2O3 content can be 0.00%, above 0.00%, or greater than 0.00%.

[0089] From the viewpoint of maintaining a high refractive index and low dispersion of the glass, the Gd2O3 content is preferably 0.00% or more, more preferably 0.50% or more, and even more preferably 1.00% or more, 1.50% or more, 2.00% or more, 2.50% or more, 3.00% or more, 3.50% or more, and 4.00% or more.

[0090] On the other hand, from the viewpoint of suppressing the rise in glass transition temperature (Tg) and maintaining the meltability and thermal stability of the glass, the Gd₂O₃ content is preferably 30.00% or less, more preferably 29.00% or less, and even more preferably 28.00% or less, 27.00% or less, 26.00% or less, 25.00% or less, 24.00% or less, 23.00% or less, 22.00% or less, 21.00% or less, 20.00% or less, and 19.00% or less. Below, below 18.00%, below 17.00%, below 16.00%, below 15.00%, below 14.00%, below 13.00%, below 12.00%, below 11.00%, below 10.50%, below 10.00%, below 9.50%, below 9.00%, below 8.50%, below 8.00%, below 7.50%, below 7.00%, below 6.50%, below 6.00%, below 5.50%, below 5.00%.

[0091] The Y2O3 content can be 0.00%, above 0.00%, or greater than 0.00%.

[0092] From the viewpoint of maintaining a high refractive index and low dispersion of the glass, the Y2O3 content is preferably 0.00% or more, more preferably 0.10% or more, and even more preferably 0.20% or more, 0.30% or more, 0.40% or more, and 0.50% or more.

[0093] On the other hand, from the viewpoint of suppressing the rise in glass transition temperature (Tg) and maintaining the meltability and thermal stability of the glass, the Y₂O₃ content is preferably 30.00% or less, more preferably 29.00% or less, and even more preferably 28.00% or less, 27.00% or less, 26.00% or less, 25.00% or less, 24.00% or less, 23.00% or less, 22.00% or less, 21.00% or less, 20.00% or less, and 19.00% or less. Below, below 18.00%, below 17.00%, below 16.00%, below 15.00%, below 14.00%, below 13.00%, below 12.00%, below 11.00%, below 10.50%, below 10.00%, below 9.50%, below 9.00%, below 8.50%, below 8.00%, below 7.50%, below 7.00%, below 6.50%, below 6.00%, below 5.50%, below 5.00%.

[0094] The Yb2O3 content can be 0.00%, above 0.00%, or greater than 0.00%.

[0095] From the viewpoint of maintaining a high refractive index and low dispersion of the glass, the Yb2O3 content is preferably 0.00% or more, more preferably 0.50% or more, and even more preferably 1.00% or more, 1.50% or more, 2.00% or more, 2.50% or more, 3.00% or more, 3.10% or more, 3.20% or more, 3.30% or more, 3.40% or more, and 3.50% or more.

[0096] On the other hand, from the viewpoint of suppressing the rise in glass transition temperature (Tg) and maintaining the meltability and thermal stability of the glass, the Yb₂O₃ content is preferably 30.00% or less, more preferably 29.00% or less, and even more preferably 28.00% or less, 27.00% or less, 26.00% or less, 25.00% or less, 24.00% or less, 23.00% or less, 22.00% or less, 21.00% or less, 20.00% or less, and 19.00% or less. Below, below 18.00%, below 17.00%, below 16.00%, below 15.00%, below 14.00%, below 13.00%, below 12.00%, below 11.00%, below 10.50%, below 10.00%, below 9.50%, below 9.00%, below 8.50%, below 8.00%, below 7.50%, below 7.00%, below 6.50%, below 6.00%, below 5.50%, below 5.00%.

[0097] From the viewpoint of maintaining a high refractive index and low dispersion of the glass, the mass ratio of Ln2O3 content to the total content of SiO2 and B2O3 (Ln2O3 / (SiO2+B2O3)) is 3.41 or more, preferably 3.42 or more, and even more preferably 3.43 or more, 3.44 or more, 3.45 or more, 3.46 or more, 3.47 or more, 3.48 or more, 3.49 or more, 3.50 or more, 3.51 or more, 3.52 or more, 3.53 or more, 3.54 or more, and 3.55 or more.

[0098] On the other hand, from the viewpoint of suppressing the rise of the glass transition temperature Tg and maintaining the melting and thermal stability of the glass, the mass ratio (Ln2O3 / (SiO2+B2O3)) is preferably 6.00 or less, more preferably 5.80 or less, and even more preferably 5.60 or less, 5.40 or less, 5.20 or less, 5.00 or less, 4.80 or less, 4.70 or less, 4.60 or less, 4.50 or less, 4.40 or less, and 4.30 or less.

[0099] From the viewpoint of maintaining a high refractive index and low dispersion of glass, the mass ratio of La2O3 to Ln2O3 (La2O3 / Ln2O3) is preferably 0.50 or more, more preferably 0.55 or more, and even more preferably 0.60 or more, 0.65 or more, 0.70 or more, 0.71 or more, 0.72 or more, 0.73 or more, 0.74 or more, 0.75 or more, 0.76 or more, 0.77 or more, 0.78 or more, 0.79 or more, and 0.80 or more.

[0100] On the other hand, from the viewpoint of maintaining the meltability and thermal stability of the glass, the mass ratio (La2O3 / Ln2O3) is preferably 1.00 or less, more preferably 0.99 or less, and even more preferably 0.98 or less, 0.97 or less, 0.96 or less, 0.95 or less, 0.94 or less, 0.93 or less, 0.92 or less, 0.91 or less, and 0.90 or less.

[0101] From the viewpoint of maintaining a high refractive index and low dispersion of the glass, the mass ratio of Ln2O3 content to B2O3 content (Ln2O3 / B2O3) is preferably 3.41 or more, more preferably 3.42 or more, and even more preferably 3.43 or more, 3.44 or more, 3.45 or more, 3.46 or more, 3.47 or more, 3.48 or more, 3.49 or more, 3.50 or more, 3.51 or more, 3.52 or more, 3.53 or more, 3.54 or more, and 3.55 or more.

[0102] On the other hand, from the viewpoint of suppressing the rise of the glass transition temperature Tg and maintaining the melting and thermal stability of the glass, the mass ratio (Ln2O3 / B2O3) is preferably 6.00 or less, more preferably 5.80 or less, and even more preferably 5.60 or less, 5.40 or less, 5.20 or less, 5.00 or less, 4.80 or less, 4.70 or less, 4.60 or less, 4.50 or less, 4.40 or less, and 4.30 or less.

[0103] From the viewpoint of maintaining a high refractive index and low dispersion of glass, the mass ratio of Ln2O3 content to the total content of Ln2O3, SiO2 and B2O3 (Ln2O3 / (Ln2O3+SiO2+B2O3)) is preferably 0.70 or more, more preferably 0.71 or more, and even more preferably 0.72 or more, 0.73 or more, 0.74 or more, 0.75 or more, 0.76 or more, and 0.77 or more.

[0104] On the other hand, from the viewpoint of suppressing the rise of the glass transition temperature Tg and maintaining the melting and thermal stability of the glass, the mass ratio (Ln2O3 / (Ln2O3+SiO2+B2O3)) is preferably 1.00 or less, more preferably 0.99 or less, and even more preferably 0.98 or less, 0.97 or less, 0.96 or less, 0.95 or less, 0.94 or less, 0.93 or less, 0.92 or less, 0.91 or less, 0.90 or less, 0.89 or less, 0.88 or less, 0.87 or less, 0.86 or less, 0.85 or less, 0.84 or less, and 0.83 or less.

[0105] Nb2O5 is a component that helps to increase the refractive index of glass.

[0106] From the viewpoint of maintaining a high refractive index of the glass, the Nb2O5 content is greater than 0.00%, preferably 0.20% or more, more preferably 0.40% or more, and even more preferably 0.60% or more, 0.80% or more, 1.00% or more, 1.20% or more, 1.40% or more, 1.60% or more, 1.80% or more, 2.00% or more, 2.20% or more, 2.40% or more, 2.60% or more, 2.80% or more, 3.00% or more, 3.20% or more, 3.40% or more, and 3.60% or more.

[0107] On the other hand, from the viewpoint of maintaining the meltability, thermal stability and low dispersion of the glass, the Nb2O5 content is 14.00% or less, preferably 13.80% or less, more preferably 13.60% or less, and even more preferably 13.40% or less, 13.20% or less, 13.00% or less, 12.80% or less, 12.60% or less, 12.40% or less, 12.20% or less, 12.00% or less, 11.80% or less, 11.60% or less, 11.40% or less, 11.20% or less, 11.00% or less, 10.80% or less, 10.60% or less, 10.40% or less, 10.20% or less, 10.00% or less, 9.80% or less, 9.60% or less, and 9.40% or less.

[0108] From the viewpoint of maintaining low dispersion of the glass, the total content of Nb2O5, TiO2, WO3 and Ta2O5 (Nb2O5+TiO2+WO3+Ta2O5) is 14.00% or less, preferably 13.80% or less, and more preferably 13.60% or less, 13.40% or less, 13.20% or less, 13.00% or less, 12.80% or less, 12.60% or less, 12.40% or less, 12.20% or less, 12.00% or less, 11.80% or less, 11.60% or less, 11.40% or less, 11.20% or less, 11.00% or less, 10.80% or less, 10.60% or less, 10.40% or less, 10.20% or less, 10.00% or less, 9.80% or less, 9.60% or less, and 9.40% or less.

[0109] On the other hand, since the Nb2O5 content is greater than 0.00%, the total content (Nb2O5+TiO2+WO3+Ta2O5) is greater than 0.00%. From the viewpoint of maintaining a high refractive index of the glass, the total content (Nb2O5+TiO2+WO3+Ta2O5) is preferably 0.20% or more, more preferably 0.40% or more, and even more preferably 0.60% or more, 0.80% or more, 1.00% or more, 1.20% or more, 1.40% or more, 1.60% or more, 1.80% or more, 2.00% or more, 2.20% or more, 2.40% or more, 2.60% or more, 2.80% or more, 3.00% or more, 3.20% or more, 3.40% or more, and 3.60% or more.

[0110] TiO2 is a component that contributes to low dispersion in glass.

[0111] The TiO2 content can be 0.00%, more than 0.00%, or greater than 0.00%.

[0112] From the viewpoint of maintaining the meltability and thermal stability of the glass, the TiO2 content is preferably 0.00% or more, more preferably 0.50% or more, and even more preferably 1.00% or more, 1.50% or more, 2.00% or more, 2.20% or more, 2.40% or more, 2.60% or more, 2.80% or more, 3.00% or more, 3.20% or more, and 3.40% or more.

[0113] On the other hand, from the viewpoint of maintaining the thermal stability of the glass and low dispersion, the TiO2 content is preferably 10.00% or less, more preferably 9.50% or less, and even more preferably 9.00% or less, 8.50% or less, 8.00% or less, 7.50% or less, 7.00% or less, 6.50% or less, 6.00% or less, 5.50% or less, 5.00% or less, 4.50% or less, 4.00% or less, 3.90% or less, 3.80% or less, 3.70% or less, 3.60% or less, 3.50% or less, 3.40% or less, 3.30% or less, 3.20% or less, 3.10% or less, 3.00% or less, 2.90% or less, 2.80% or less, 2.70% or less, 2.60% or less, and 2.50% or less.

[0114] WO3 is a component that helps to increase the refractive index of glass.

[0115] The WO3 content can be 0.00%, above 0.00%, or greater than 0.00%.

[0116] From the viewpoint of maintaining the high refractive index, meltability and thermal stability of the glass, the WO3 content is preferably 0.00% or more, more preferably 0.10% or more, and even more preferably 0.20% or more, 0.30% or more, 0.40% or more, and 0.50% or more.

[0117] On the other hand, from the viewpoint of maintaining low dispersion of the glass, the WO3 content is preferably 10.00% or less, more preferably 9.50% or less, and even more preferably 9.00% or less, 8.50% or less, 8.00% or less, 7.50% or less, 7.00% or less, 6.50% or less, 6.00% or less, 5.50% or less, 5.00% or less, 4.50% or less, 4.00% or less, 3.50% or less, 3.00% or less, and 2.50% or less.

[0118] Ta2O5 is a component that contributes to the high refractive index and low dispersion of glass.

[0119] The Ta2O5 content can be 0.00%, more than 0.00%, or greater than 0.00%.

[0120] From the viewpoint of maintaining a high refractive index and low dispersion of the glass, the Ta2O5 content is preferably 0.00% or more, more preferably 0.10% or more, and even more preferably 0.20% or more, 0.30% or more, 0.40% or more, and 0.50% or more.

[0121] On the other hand, from the viewpoint of keeping the raw material cost of glass at a low level, the Ta2O5 content is preferably 15.00% or less, more preferably 14.00% or less, and even more preferably 13.00% or less, 12.00% or less, 11.00% or less, 10.00% or less, 9.00% or less, 8.00% or less, 7.00% or less, 6.00% or less, 5.00% or less, 4.00% or less, 3.00% or less, 2.50% or less, 2.00% or less, 1.50% or less, and 1.00% or less.

[0122] From the viewpoint of maintaining the meltability, thermal stability and low dispersion of glass, the mass ratio of TiO2 content to the total content of SiO2 and B2O3 (TiO2 / (SiO2+B2O3)) is 0.17 or less, preferably 0.16 or less, and more preferably 0.15 or less, 0.14 or less, 0.13 or less, 0.12 or less, 0.11 or less, 0.10 or less, 0.09 or less, 0.08 or less, 0.07 or less, 0.06 or less, and 0.05 or less.

[0123] The mass ratio (TiO2 / (SiO2+B2O3)) can be 0.00, 0.00 or more, or greater than 0.00. From the viewpoint of maintaining the meltability and thermal stability of the glass, the mass ratio (TiO2 / (SiO2+B2O3)) is preferably 0.00 or more, and more preferably 0.00.

[0124] From the viewpoint of maintaining low dispersion of the glass, the value obtained by subtracting the contents of Nb2O5, TiO2, WO3 and Ta2O5 from the Ln2O3 content (Ln2O3-Nb2O5-TiO2-WO3-Ta2O5) is 49.00% or more, preferably 49.50% or more, and more preferably 50.00% or more, 50.50% or more, 51.00% or more, 51.10% or more, 51.20% or more, 51.30% or more, 51.40% or more, 51.50% or more, 51.60% or more, 51.70% or more, 51.80% or more, 51.90% or more, 52.00% or more, 52.10% or more, and 52.20% or more.

[0125] On the other hand, from the viewpoint of suppressing the rise of the glass transition temperature Tg, and from the viewpoint of maintaining the meltability, thermal stability and high refractive index of the glass, the above-mentioned value (Ln2O3-Nb2O5-TiO2-WO3-Ta2O5) is preferably 70.00% or less, more preferably 69.50% or less, and even more preferably 69.00% or less, 68.50% or less, 68.00% or less, 67.50% or less, 67.00% or less, 66.50% or less, 66.00% or less, 65.50% or less, 65.00% or less, 64.50% or less, and 64.00% or less.

[0126] With the mass ratio of Ln2O3 content to the total content of Ln2O3, SiO2 and B2O3 (Ln2O3 / (Ln2O3+SiO2+B2O3)) set as y, and the mass ratio of Ln2O3 content to the total content of Ln2O3, Nb2O5, TiO2, WO3 and Ta2O5 (Ln2O3 / (Ln2O3+Nb2O5+TiO2+WO3+Ta2O5)) set as x, from the viewpoint of maintaining high refractive index and low dispersion, the above glass satisfies the following equation (1).

[0127] (1) y≥-0.7058x+1.38

[0128] The glass described above preferably satisfies the following formula (1-1), more preferably satisfies the following formula (1-2), even more preferably satisfies formula (1-3), even more preferably satisfies formula (1-4), and even more preferably satisfies formula (1-5).

[0129] (1-1) y≥-0.7058x+1.381

[0130] (1-2) y≥-0.7058x+1.382

[0131] (1-3) y≥-0.7058x+1.383

[0132] (1-4) y≥-0.7058x+1.384

[0133] (1-5) y≥-0.7058x+1.385

[0134] For x and y above, from the viewpoint of maintaining a high refractive index and low dispersion of the glass, the glass preferably satisfies the following equation (2).

[0135] (2) y≥-0.2797x+1.0181

[0136] The glass described above more preferably satisfies the following formula (2-1), further preferably satisfies the following formula (2-2), even more preferably satisfies formula (2-3), and even more preferably satisfies formula (2-4).

[0137] (2-1) y≥-0.2797x+1.0182

[0138] (2-2) y≥-0.2797x+1.0183

[0139] (2-3) y≥-0.2797x+1.0184

[0140] (2-4) y≥-0.2797x+1.0185

[0141] From the viewpoint of maintaining low dispersion of the glass, the mass ratio of Ln2O3 content to the total content of Ln2O3, Nb2O5, TiO2, WO3 and Ta2O5 (Ln2O3 / (Ln2O3+Nb2O5+TiO2+WO3+Ta2O5)) is preferably 0.845 or more, more preferably 0.846 or more, and even more preferably 0.847 or more, 0.848 or more, 0.849 or more, 0.850 or more, 0.851 or more, 0.852 or more, 0.853 or more, 0.854 or more, 0.855 or more, 0.856 or more, 0.857 or more, 0.858 or more, 0.859 or more, and 0.860 or more.

[0142] On the other hand, from the viewpoint of maintaining the meltability and thermal stability of the glass, the mass ratio (Ln2O3 / (Ln2O3+Nb2O5+TiO2+WO3+Ta2O5)) is preferably 1.000 or less, more preferably 0.990 or less, and even more preferably 0.980 or less, 0.970 or less, 0.960 or less, 0.950 or less, 0.940 or less, 0.930 or less, 0.920 or less, 0.910 or less, and 0.900 or less.

[0143] From the viewpoint of maintaining a high refractive index of the glass, the total content of ZnO, ZrO2, Nb2O5, TiO2, WO3, and Ta2O5 (ZnO+ZrO2+Nb2O5+TiO2+WO3+Ta2O5) is preferably 6.00% or more, more preferably 6.20% or more, and even more preferably 6.40% or more, 6.60% or more, 6.80% or more, 7.00% or more, 7.20% or more, and 7. More than 40%, more than 7.60%, more than 7.80%, more than 8.00%, more than 8.20%, more than 8.40%, more than 8.60%, more than 8.80%, more than 9.00%, more than 9.20%, More than 9.40%, more than 9.60%, more than 9.80%, more than 10.00%, more than 10.20%, more than 10.40%, more than 10.60%, more than 10.80%, more than 11.00%.

[0144] On the other hand, from the viewpoint of maintaining low dispersion of the glass, the total content (ZnO+ZrO2+Nb2O5+TiO2+WO3+Ta2O5) is preferably 30.00% or less, more preferably 29.00% or less, and even more preferably 28.00% or less, 27.00% or less, 26.00% or less, 25.00% or less, 24.00% or less, 23.00% or less, 22.50% or less, 22.00% or less, 21.50% or less, 21.00% or less, 20.50% or less, and 20.00% or less.

[0145] ZnO is a component that helps lower the glass transition temperature (Tg) and improves the meltability of glass.

[0146] The ZnO content can be 0.00%, above 0.00%, or greater than 0.00%.

[0147] From the viewpoint of maintaining the meltability and thermal stability of the glass, the ZnO content is preferably 0.00% or more, more preferably 0.10% or more, and even more preferably 0.20% or more, 0.30% or more, 0.40% or more, and 0.50% or more.

[0148] On the other hand, from the viewpoint of maintaining a high refractive index and low dispersion of the glass, the ZnO content is preferably 20.00% or less, more preferably 19.00% or less, and even more preferably 18.00% or less, 17.00% or less, 16.00% or less, 15.50% or less, 15.00% or less, 14.50% or less, 14.00% or less, 13.50% or less, 13.00% or less, 12.50% or less, and 12.00% or less.

[0149] ZrO2 is a component that helps improve the thermal stability of glass.

[0150] The ZrO2 content can be 0.00%, above 0.00%, or greater than 0.00%.

[0151] From the viewpoint of maintaining the glass's meltability, thermal stability, high refractive index, and low dispersion, the ZrO2 content is preferably 0.00% or more, more preferably 0.10% or more, and even more preferably 0.20% or more, 0.30% or more, 0.40% or more, and 0.50% or more.

[0152] On the other hand, from the viewpoint of maintaining the meltability and thermal stability of the glass, the ZrO2 content is preferably 15.00% or less, more preferably 14.00% or less, and even more preferably 13.00% or less, 12.00% or less, 11.00% or less, 10.50% or less, 10.00% or less, 9.50% or less, 9.00% or less, 8.50% or less, 8.00% or less, 7.80% or less, 7.60% or less, 7.50% or less, 7.40% or less, 7.30% or less, 7.20% or less, 7.10% or less, 7.00% or less, 6.90% or less, 6.80% or less, 6.70% or less, 6.60% or less, 6.50% or less, 6.40% or less, 6.30% or less, 6.20% or less, 6.10% or less, and 6.00% or less.

[0153] From the viewpoint of maintaining low dispersion of the glass, the value obtained by subtracting the contents of ZnO, ZrO2, Nb2O5, TiO2, WO3, and Ta2O5 from the Ln2O3 content (Ln2O3-ZnO-ZrO2-Nb2O5-TiO2-WO3-Ta2O5) is preferably 39.80% or more, more preferably 40.00% or more, and even more preferably 40.20% or more, 40.40% or more, 40.60% or more, 40.80% or more, 41.00% or more, 41.20% or more, 41.40% or more, 41.60% or more, 41.80% or more, 42.00% or more, 42.20% or more, 42.40% or more, 42.60% or more, 42.80% or more, and 43.00% or more.

[0154] On the other hand, from the viewpoint of maintaining the meltability, thermal stability and high refractive index of the glass, the above-mentioned value (Ln2O3-ZnO-ZrO2-Nb2O5-TiO2-WO3-Ta2O5) is preferably 70.00% or less, more preferably 69.00% or less, and even more preferably 68.00% or less, 67.00% or less, 66.00% or less, 65.00% or less, 64.00% or less, 63.00% or less, 62.00% or less, 61.00% or less, 60.00% or less, 59.00% or less, 58.00% or less, and 57.00% or less.

[0155] Li2O is a component that helps lower the glass transition temperature (Tg), and also helps improve the melting properties of glass and reduce its specific gravity.

[0156] The Li2O content can be 0.00%, more than 0.00%, or greater than 0.00%.

[0157] From the viewpoint of lowering the glass transition temperature Tg and maintaining the melting and thermal stability of the glass, the Li2O content is preferably 0.00% or more, more preferably 0.10% or more, and even more preferably 0.20% or more, 0.30% or more, 0.40% or more, and 0.50% or more.

[0158] On the other hand, from the viewpoint of maintaining a high refractive index and low dispersion of the glass and keeping the raw material cost at a low level, the Li2O content is preferably 5.00% or less, more preferably 4.50% or less, and even more preferably 4.00% or less, 3.50% or less, 3.00% or less, 2.50% or less, and 2.00% or less.

[0159] The Na2O content can be 0.00%, more than 0.00%, or greater than 0.00%.

[0160] From the viewpoint of lowering the glass transition temperature Tg and maintaining the melting and thermal stability of the glass, the Na2O content is preferably 0.00% or more, more preferably 0.10% or more, and even more preferably 0.20% or more, 0.30% or more, 0.40% or more, and 0.50% or more.

[0161] On the other hand, from the viewpoint of maintaining a high refractive index and low dispersion of the glass and keeping the raw material cost at a low level, the Na2O content is preferably 5.00% or less, more preferably 4.50% or less, and even more preferably 4.00% or less, 3.50% or less, 3.00% or less, 2.50% or less, and 2.00% or less.

[0162] The K2O content can be 0.00%, above 0.00%, or greater than 0.00%.

[0163] From the viewpoint of lowering the glass transition temperature Tg and maintaining the meltability and thermal stability of the glass, the K2O content is preferably 0.00% or more, more preferably 0.10% or more, and even more preferably 0.20% or more, 0.30% or more, 0.40% or more, and 0.50% or more.

[0164] On the other hand, from the viewpoint of maintaining a high refractive index and low dispersion of the glass and keeping the raw material cost at a low level, the K2O content is preferably 5.00% or less, more preferably 4.50% or less, and even more preferably 4.00% or less, 3.50% or less, 3.00% or less, 2.50% or less, and 2.00% or less.

[0165] BaO is a component that helps improve the meltability of glass.

[0166] The BaO content can be 0.00%, more than 0.00%, or greater than 0.00%.

[0167] From the viewpoint of maintaining the meltability and thermal stability of the glass, the BaO content is preferably 0.00% or more, more preferably 0.10% or more, and even more preferably 0.20% or more, 0.30% or more, 0.40% or more, and 0.50% or more.

[0168] On the other hand, from the viewpoint of maintaining a high refractive index and low dispersion of the glass, the BaO content is preferably 10.00% or less, more preferably 9.00% or less, and even more preferably 8.00% or less, 7.00% or less, 6.00% or less, 5.00% or less, and 4.00% or less.

[0169] The MgO content can be 0.00%, more than 0.00%, or greater than 0.00%.

[0170] From the viewpoint of maintaining the meltability and thermal stability of the glass, the MgO content is preferably 0.00% or more, more preferably 0.10% or more, and even more preferably 0.20% or more, 0.30% or more, 0.40% or more, and 0.50% or more.

[0171] On the other hand, from the viewpoint of maintaining a high refractive index and low dispersion of the glass, the MgO content is preferably 10.00% or less, more preferably 9.00% or less, and even more preferably 8.00% or less, 7.00% or less, 6.00% or less, 5.00% or less, and 4.00% or less.

[0172] The CaO content can be 0.00%, above 0.00%, or greater than 0.00%.

[0173] From the viewpoint of maintaining the meltability and thermal stability of the glass, the CaO content is preferably 0.00% or more, more preferably 0.10% or more, and even more preferably 0.20% or more, 0.30% or more, 0.40% or more, and 0.50% or more.

[0174] On the other hand, from the viewpoint of maintaining a high refractive index and low dispersion of the glass, the CaO content is preferably 10.00% or less, more preferably 9.00% or less, and even more preferably 8.00% or less, 7.00% or less, 6.00% or less, 5.00% or less, and 4.00% or less.

[0175] The SrO content can be 0.00%, above 0.00%, or greater than 0.00%.

[0176] From the viewpoint of maintaining the meltability and thermal stability of the glass, the SrO content is preferably 0.00% or more, more preferably 0.10% or more, and even more preferably 0.20% or more, 0.30% or more, 0.40% or more, and 0.50% or more.

[0177] On the other hand, from the viewpoint of maintaining a high refractive index and low dispersion of the glass, the SrO content is preferably 10.00% or less, more preferably 9.00% or less, and even more preferably 8.00% or less, 7.00% or less, 6.00% or less, 5.00% or less, and 4.00% or less.

[0178] BiO3 is a component that helps to increase the refractive index of glass.

[0179] The BiO3 content can be 0.00%, more than 0.00%, or greater than 0.00%.

[0180] From the viewpoint of maintaining the high refractive index, meltability and thermal stability of the glass, the BiO3 content is preferably 0.00% or more, and more preferably 0.10% or more, 0.20% or more, 0.30% or more, 0.40% or more and 0.50% or more.

[0181] From the viewpoint of maintaining low dispersion of the glass, the BiO3 content is preferably 10.00% or less, more preferably 9.50% or less, and even more preferably 9.00% or less, 8.50% or less, 8.00% or less, 7.50% or less, 7.00% or less, 6.50% or less, 6.00% or less, 5.50% or less, 5.00% or less, 4.50% or less, 4.00% or less, 3.50% or less, 3.00% or less, and 2.50% or less.

[0182] Sb₂O₃ is a component that can be added as a clarifying agent. It can suppress the decrease in light transmittance caused by the incorporation of impurities such as Fe with a small amount added. However, if the amount of Sb₂O₃ added increases, the glass tends to show increased coloration. Therefore, the amount of Sb₂O₃ added is preferably 0.00% or more and 0.10% or less, more preferably 0.00% or more and 0.05% or less, and even more preferably 0.00% or more and 0.03% or less, based on the added proportion. The Sb₂O₃ content based on the added proportion refers to the Sb₂O₃ content expressed as a percentage by mass when the total content of glass components other than Sb₂O₃ and SnO₂ is set to 100% by mass.

[0183] SnO2 can also be added as a clarifying agent, but if it is added in a proportion greater than 1.00%, glass coloring may occur, or Sn may become the starting point for crystal nucleation during re-forming processes such as heating and softening the glass for pressing, leading to devitrification. Therefore, it is preferable to set the amount of SnO2 added to 0.00% or more and 1.00% or less, more preferably 0.00% or more and 0.50% or less, and particularly preferably not to add it at all, based on the proportion. The SnO2 content based on the proportion refers to the SnO2 content expressed as a percentage by mass when the total content of glass components other than Sb2O3 and SnO2 is set to 100% by mass.

[0184] The aforementioned optical glass can be manufactured without Lu and Hf. Since Lu and Hf are expensive components, it is preferable to suppress the content of Lu2O3 and HfO2 to 0.00% or more and 2.00% or less, more preferably to 0.00% or more and 1.00% or less, even more preferably to 0.00% or more and 0.80% or less, even more preferably to 0.00% or more and 0.10% or less, and particularly preferably without introducing Lu2O3 or HfO2.

[0185] In addition, considering the environmental impact, it is preferable not to introduce Pb, and it is also preferable not to introduce As, U, Th, Te, and Cd.

[0186] Furthermore, from the viewpoint of fully utilizing the excellent light transmittance of glass, it is preferable to avoid introducing substances such as Cu, Cr, V, Fe, Ni, and Co that cause coloration.

[0187] F (fluorine) is a component that lowers the refractive index, significantly increases the volatility of the glass during melting, and also improves thermal stability, maintains low dispersion, and lowers the glass transition temperature (Tg). The F content can be defined as the content (in mass%) of the total F element relative to the glass composition, calculated as described above, based on oxides, plus a proportion (unit: mass%). From the viewpoint of maintaining a high refractive index and low dispersion in the glass, in the aforementioned optical glass, the specified F content is preferably less than 20.00%, more preferably less than 18.00%, and subsequently even more preferably less than 16.00%, less than 14.00%, less than 12.00%, less than 10.00%, less than 8.00%, less than 6.00%, less than 4.00%, less than 2.00%, and less than 1.00%. The F content can be 0.00% or more, or it can be 0.00%.

[0188] <Properties of Glass>

[0189] (Refractive index nd, Abbe number νd)

[0190] In this invention and this specification, "refractive index" refers to "refractive index nd".

[0191] The Abbe number νd is a value representing a property related to dispersion, expressed as νd=(nd-1) / (nF-nC) using the refractive indices nd, nF, and nC under d-rays, F-rays, and C-rays.

[0192] From the viewpoint of its usefulness as a material for optical components, the glass described above is preferably a high-refractive-index, low-dispersion glass. From this perspective, regarding the refractive index nd and the Abbe number νd, the glass preferably satisfies the following equation (3).

[0193] (3) nd≥-0.01000×νd+2.28500

[0194] The refractive index nd is preferably 1.80000 or higher, and more preferably 1.81000 or higher, 1.82000 or higher, 1.83000 or higher, 1.83000 or higher, 1.84000 or higher, 1.85000 or higher, 1.86000 or higher, 1.87000 or higher, 1.87500 or higher, 1.88000 or higher, and 1.88300 or higher.

[0195] The refractive index nd can be, for example, below 1.95000, below 1.94000, below 1.93000, below 1.92000, below 1.91000, or below 1.90500.

[0196] The Abbe number νd is preferably 35.00 or higher, and more preferably 36.00 or higher, 37.00 or higher, 38.00 or higher, and 38.50 or higher.

[0197] The Abbe number νd is, for example, 50.00 or less, 49.00 or less, 48.00 or less, 47.00 or less, 46.00 or less, 45.00 or less, 44.00 or less, 43.00 or less, 42.00 or less, 41.50 or less, 41.00 or less, 36.80 or less, or 36.60 or less.

[0198] (proportion)

[0199] In optical elements that constitute an optical system, the refractive power is determined by the refractive index of the glass constituting the element and the curvature of the optical functional surfaces (the surfaces through which the light rays are incident and emitted, which are to be controlled). If the curvature of the optical functional surfaces is increased, the thickness of the optical element also increases. As a result, the optical element becomes heavier. Conversely, if glass with a high refractive index is used, a large refractive power can be obtained even without increasing the curvature of the optical functional surfaces.

[0200] Therefore, as long as the increase in the specific gravity of glass can be suppressed and the refractive index can be increased, it is possible to make optical components with a certain refractive power lighter.

[0201] From the above perspectives, the specific gravity of the aforementioned glass is preferably 5.80 or less, and more preferably 5.75 or less, 5.70 or less, 5.65 or less, 5.60 or less, 5.55 or less, 5.50 or less, 5.45 or less, 5.40 or less, and 5.35 or less. From the viewpoint of lightweight optical components, a lower specific gravity is preferred; therefore, there is no particular limitation on the lower limit of the specific gravity of the aforementioned optical glass. In one embodiment, the specific gravity can be 4.40 or more, 4.50 or more, or 4.60 or more. In this specification, "specific gravity" is also referred to as "sg" (specific gravity).

[0202] (Glass transition temperature Tg)

[0203] From the viewpoint of reducing the burden on the annealing furnace and forming mold, the glass transition temperature Tg of the aforementioned glass is preferably 800°C or lower, more preferably 790°C or lower, 780°C or lower, 770°C or lower, and 760°C or lower. On the other hand, from the viewpoint of machinability (specifically, from the viewpoint of minimizing damage during mechanical processing of glass such as cutting, shaving, grinding, and polishing), the glass transition temperature Tg of optical glass is preferably 640°C or higher, more preferably 650°C or higher, and even more preferably 660°C or higher. The glass transition temperature Tg can be determined by the method described later.

[0204] <Methods for Manufacturing Optical Glass>

[0205] The aforementioned optical glass can be obtained by the following method: weighing and mixing oxides, carbonates, sulfates, nitrates, hydroxides, etc., as raw materials in a manner that yields the target glass composition, thoroughly mixing them to form a mixed batch, heating, melting, degassing, and stirring in a molten container to produce a uniform, bubble-free molten glass, and then shaping it. Molten glass can be produced using known melting methods.

[0206] [Glass Molded Body]

[0207] One aspect of the present invention relates to a rod-shaped glass molding body (hereinafter also referred to as "rod-shaped glass") made of the aforementioned optical glass. "Rod-shaped glass molding body" and "rod-shaped glass" refer to glass molding bodies having a rectangular, polygonal, or other cross-sectional shape having a circle, ellipse, square, or a ratio of the long side length to the short side length (long side length / short side length) of 2 or less. In contrast, "plate-shaped glass" refers to a glass molding body having a width-to-thickness ratio (width / thickness) greater than 2.

[0208] Furthermore, the outer diameter of a rod-shaped glass refers to the length of the thinnest part of the glass in a cross-section perpendicular to the central axis of the rod. For example, in cylindrical glass, since the cross-section perpendicular to the central axis of the cylinder is a circle, the outer diameter is the diameter of that circle; in elliptical cylindrical glass, since the cross-section perpendicular to the central axis is an ellipse, the outer diameter is the minor axis of that ellipse; in regular square prism glass, since the cross-section perpendicular to the central axis is a square, the outer diameter is the length of one side of that square. For a square prism glass with a rectangular cross-section perpendicular to the central axis, the outer diameter is equivalent to the length of the minor side of that rectangle.

[0209] The aforementioned glass molded body can be manufactured, for example, by the glass molded body manufacturing method described below.

[0210] The method for manufacturing glass molded bodies involves heating and melting glass raw materials to obtain molten glass, which is then poured into a mold and formed into a glass molded body made of optical glass. In this method,

[0211] Using a mold with through holes, molten glass is continuously poured into the through holes and shaped. The shaped glass is then continuously discharged from the through holes.

[0212] The inner wall of the through-hole is brought into contact with the molten glass in a manner that surrounds the molten glass moving within the through-hole, and the molten glass is cooled to produce a glass molded body made of the aforementioned optical glass.

[0213] The manufacturing method of the above-mentioned glass molded body will be described in further detail below.

[0214] In the above-described method for manufacturing a glass molded body, a mold with a through-hole is used to continuously draw molten glass from a pipe into the inlet of the through-hole and continuously remove it from the outlet of the through-hole, forming a solid glass. By contacting the side surface of the glass within the through-hole with the inner wall of the through-hole in at least a portion of the through-hole (cooling zone), heat is carried away from the side surface of the glass, and the temperature of the center of the glass is brought closer to that of the side surface.

[0215] In this method, a mold with a through hole is used to continuously draw molten glass from the pipe into the inlet of the through hole and continuously remove it from the outlet of the through hole to form solid glass.

[0216] When molding optically uniform glass bodies, it is preferable to avoid disturbing the flow of molten glass within the mold. To mold hollow glass, a mechanism is needed within the mold to locally impede the glass flow, preventing molten glass from flowing into the hollow portion, i.e., the unfilled portion. For example, when aiming to mold the central axis portion of a rod-shaped glass body as hollow, a heat-resistant rod, identical to the mold, is positioned along the central axis, and molten glass flows in surrounding the rod. In this case, a mechanism preventing glass from filling the hollow portion corresponding to the rod would disrupt the flow of molten glass. Therefore, to obtain an optically uniform glass body, it is preferable to manufacture the glass body as a solid shape without a hollow portion.

[0217] The mold used has a through-hole, which has an inlet for molten glass to flow in and an outlet for removing solid glass. Molten glass flowing out of the molten glass outlet pipe continuously flows into the inlet of the through-hole. Then, by contacting the side of the glass, from its molten state to at least surface solidification, with the inner wall of the through-hole in at least a portion of the through-hole (cooling zone), heat is removed from the glass from the side, where the side faces a direction perpendicular to the overall direction of glass movement. This reduces or prevents the formation of ripples. In particular, by ensuring that the side is in contact with the inner wall of the through-hole around its entire circumference without gaps, the glass can be cooled efficiently.

[0218] As described below, to prevent devitrification of the glass, it is preferable to set the temperature of the molten glass flowing from the tube into the through-hole inlet to a temperature near or above the liquidus temperature. Specifically, it is preferable to set the surface temperature of the molten glass flowing into the through-hole inlet to the range of (liquidus temperature + 10°C) to (liquidus temperature + 100°C). The surface temperature of the molten glass flowing into the through-hole inlet can be considered to be the same as the temperature at the lower end of the outlet tube, which can be measured using a thermocouple. Furthermore, the temperature of the center of the molten glass flowing into the through-hole inlet can be measured by inserting a thermocouple inside the molten glass. The temperature difference between the surface temperature and the center temperature of the molten glass flow measured in this way is preferably set to 120°C or less, more preferably 60°C or less, and even more preferably 50°C or less.

[0219] The optimal temperature of the mold (inner wall of the through-hole) is determined by considering (1) preventing the glass from melting and sticking together, and (2) ensuring that the molten glass spreads without gaps within the through-hole. To control the temperature, the mold can be equipped with a heater or a cooler as needed. Adjustments can be made by: air cooling or water cooling plates, etc., when the temperature of the glass forming surface at the through-hole outlet is too high; or by heating with a heater when the temperature is too low.

[0220] The temperature of the upper inner wall of the through-hole in the aforementioned cooling zone can, for example, be set to be 50-150°C lower than the glass transition temperature of the glass to be formed. As described later, when the entire glass flow path within the through-hole is designated as a cooling zone, the temperature of the inner wall of the through-hole can be set 20-50°C lower than the glass transition temperature of the glass to be formed near the inlet, and 100-400°C lower than the glass transition temperature near the outlet when using a forming furnace. The temperature in the middle section between the inlet and outlet can be set below the temperature near the inlet and above the temperature near the outlet. It should be noted that the temperature of the inner wall of the through-hole can be measured by opening a hole in the mold and inserting a thermocouple close to the inner wall of the through-hole.

[0221] In this way, by bringing the glass sidewalls into contact with the inner wall of the through-hole in the cooling zone to remove heat, the cooling of the glass can be promoted, thereby preventing or reducing the formation of ripples. However, as explained above, especially for glass with low viscosity at the time of flow, if the temperature difference between the interior and surface of the glass taken out of the mold is too large, the glass may sometimes break or fracture due to internal stress. Therefore, it is preferable to pass the glass that has passed through the aforementioned cooling zone in an environment at a temperature 150°C lower than the glass transition temperature Tg (Tg-150°C), so that the center of the glass is close to the temperature of the sidewalls. This prevents the glass, which has been rapidly cooled in the cooling zone to reduce or prevent ripples, from breaking or fractured due to internal stress after passing through the cooling zone.

[0222] The aforementioned cooling zone can be the entire glass flow path within the through-hole. In this case, the environment described above (Tg-150°C) can be the gas atmosphere exposed to the glass taken from the through-hole outlet. When the glass taken from the through-hole outlet passes through a gas atmosphere above (Tg-150°C) to bring the temperature of the center and sides of the glass closer together, it is preferable to immediately immerse the glass taken from the through-hole outlet into the aforementioned gas atmosphere.

[0223] Alternatively, the through-hole can be roughly divided into two regions: an inlet side and an outlet side. In the inlet side region, the glass sidewall is brought into contact with the inner wall of the through-hole to remove heat from the glass from the side. Meanwhile, the temperature of the inner wall of the through-hole in the outlet side region is controlled to be at least 150°C lower than the glass transition temperature Tg (Tg-150°C). In this case, the environment described above (Tg-150°C) is the temperature-controlled outlet side region. Here, both the inlet and outlet sides can be insulated to facilitate temperature control in both regions.

[0224] In any of the above situations, the operation of bringing the temperature of the center and the side of the glass closer together is preferably carried out by passing the glass through a temperature at least 100°C lower than the glass transition temperature (Tg-100°C), more preferably by passing the glass through a temperature at least 50°C lower than the glass transition temperature (Tg-50°C), and even more preferably by passing the glass through a temperature at the glass transition temperature Tg.

[0225] If the temperature in the aforementioned environment is too low, the furnace size must be increased if operations are performed in the forming furnace to bring the center and sides of the glass to a similar temperature. Similarly, the mold size must be increased if operations are performed in the mold to bring the center and sides of the glass to a similar temperature. This results in the need for large spaces and makes it difficult to control the speed at which the glass is removed from the through-hole.

[0226] Furthermore, when cutting a glass mold, if the glass temperature is too low, it becomes difficult to cut due to the increased Young's modulus. Typically, glass is a continuous body from molten glass to the glass mold; if a large force is applied to cut the glass mold, the impact can affect the molten glass in the mold, causing disturbances in the glass flow. Cutting can also be done using a wire saw or a grinding stone, but the glass must be cooled to near room temperature, requiring a space tens of meters long for slow cooling. For efficient cutting of the glass mold, the glass temperature is preferably near or below its glass transition temperature, more preferably at least 150°C below and below the glass transition temperature, further preferably at least 100°C below and below the glass transition temperature, even more preferably at least 50°C below and below the glass transition temperature, and particularly preferably near the glass transition temperature. Considering the above aspects, the operation to bring the temperature of the center and sides of the glass closer together is preferably performed in an environment with a temperature of (Tg-150°C) or higher. After the operation of bringing the temperature of the center and sides of the glass close together, i.e. reducing the strain, the glass mold can be separated at the desired location without breaking by cutting or severing the glass mold.

[0227] The upper limit of the temperature used for operating to heat the interior and sides of the glass can be set to the temperature at which the outer diameter shape of the glass (the cross-sectional shape perpendicular to the removal direction) formed by the rapid cooling of the glass sides does not deform. It is preferably set below the softening temperature of the glass, and more preferably below the softening temperature.

[0228] When performing the above operations in a gas atmosphere, a furnace, referred to as a forming furnace, can be connected to a through-hole outlet, allowing glass continuously drawn from the outlet to directly enter the furnace and exit when the temperature of the center and sides is close. Furthermore, the transit time within the furnace should be set at a level that prevents explosive failure of the internal stress of the glass forming body, or at a level that prevents breakage due to minor thermal or mechanical shocks. Therefore, the length of the forming furnace along the glass removal direction can be appropriately determined through experiments, taking into account the glass removal speed and the furnace transit time. The gas atmosphere temperature within the furnace can be controlled, for example, by controlling the current value or the duration of current flow through a heater located within the furnace.

[0229] By performing the operation described above to bring the temperature of the center portion and the side portion of the glass closer together, the temperature difference between the center portion and the side portion of the glass can be set to, for example, 0~150°C, preferably 0~100°C, and more preferably 0~50°C. It should be noted that the operation of bringing the temperature of the center portion and the side portion of the glass closer together is different from annealing, which is an operation of slowly cooling the glass to near room temperature, and it ends at a high temperature where the glass temperature is much higher than room temperature.

[0230] Next, the mold used will be explained.

[0231] From the viewpoint of preventing glass from melting, spreading, or bending, in the molding process, it is preferable to set the ratio of the inner diameter of the through-hole to its length (inner diameter / length) to a range of 1 / 50 to 3, more preferably 1 / 20 to 2. Furthermore, the inner diameter of the through-hole is preferably determined with consideration of the desired outer diameter of the glass molded body, and for example, it can be set to 10 to 100 mm. However, it is not intended to be limited to this size.

[0232] To prevent hindering the movement of the glass within the mold, it is preferable to set the cross-sectional shape of any portion of the mold through which the glass passes, perpendicular to the direction of glass movement, to be consistent with the cross-sectional shape perpendicular to the direction of glass movement. Without controlling the temperature distribution of the mold, the temperature at the inlet side of the mold during molding is higher than the temperature at the outlet side. Therefore, if the inner diameter of the through-hole is formed constantly at room temperature, the inner diameter of the through-hole along the direction of glass movement will no longer be constant during molding due to the thermal expansion of the mold. In this method, it is preferable to make the through-hole tapered, taking thermal expansion into account, and to determine the inclination of the tapered shape, so that the inner diameter of the through-hole gradually increases from the inlet to the outlet, and that the inner diameter remains constant along the direction of glass movement during molding, or that it is slightly enlarged towards the outlet. In particular, when molding glass with low viscosity at the time of flow, or when using a mold made of a material with high glass wettability, it is preferable to increase the inclination of the tapered shape to prevent the glass from sintering and sticking to the mold.

[0233] The preferred materials for the mold are carbon, castings, and heat-resistant metals such as nickel. Furthermore, from the viewpoint of preventing mold deterioration, the process of producing the glass molded body from molten glass is preferably carried out in a non-reactive gas atmosphere.

[0234] When the gas atmosphere affects the quality of the glass molded body, it is preferable to surround the path of molten glass flow between the tube outlet and the through-hole inlet and control the atmosphere therein. In this method, the area of ​​the high-temperature glass exposed to the gas atmosphere is not as large as in conventional molding methods. Therefore, even without completely sealing the tube tip and molding apparatus and replacing the internal gas atmosphere, as long as the necessary minimum narrow area is surrounded as described above and the internal gas atmosphere is replaced with the desired gas, the purpose of controlling the gas atmosphere can be achieved. From the viewpoint of suppressing the volatilization of the high-temperature glass surface, reducing and preventing the wetting and creeping of the glass to the outer peripheral surface of the tube tip, and improving the quality of the glass molded body, it is preferable to set the gas atmosphere as a dry gas atmosphere, an inactive gas atmosphere, or a dry inactive gas atmosphere.

[0235] For this method, regardless of whether the operation of passing the glass through the cooling zone at a temperature 150°C or higher below the glass transition temperature is performed to bring the temperature of the center and side of the glass closer together, it is suitable as a method to reduce or prevent ripples when the molded body is made of glass containing volatile components, such as boric acid.

[0236] More preferably, a mold with a through-hole having a straight connection between the inlet and outlet can be used. In this case, it is preferable to configure the mold such that the inlet is located at a higher position than the outlet, and to allow the molten glass to flow in in a manner that keeps the height of the molten glass level in the through-hole constant.

[0237] Figure 1 An example of a glass molding manufacturing apparatus is shown. For example... Figure 1 As shown, molten glass 9 flowing from pipe 1 enters mold 2, and is formed into a glass molded body 11 by the process of the glass moving from a high position to a low position. Figure 1 As shown, if the part through which the flowing glass passes is a through hole with a straight connection between the inlet and outlet, the flow of molten glass in the mold is smoother and less prone to turbulence, resulting in a more stable production of optically uniform glass molded bodies.

[0238] In this method, such as Figure 1 As shown, the mold 2 is preferably arranged vertically with the central axis of the through hole aligned with the vertical line. However, the central axis can also be arranged at an angle relative to the vertical line. When the mold 2 is arranged vertically with the central axis, the fluid of the molten glass 9 flowing vertically downward in the pipe 1 travels in the mold 2 toward the outlet direction without changing the overall flow direction. Therefore, the turbulence in the flow within the mold can be further reduced, and the corrugations can be further reduced.

[0239] Furthermore, by flowing the molten glass 9 into a through-hole that connects the inlet and outlet in a straight line, a straight glass molded body can be obtained. A straight glass molded body is convenient for processing into glass raw materials for compression molding or for manufacturing optical components. To obtain a glass molded body with a straight central axis and a cross-section perpendicular to the central axis whose shape and size are identical at any position, it is preferable to use a mold 2 with a through-hole that connects the inlet and outlet in a straight line, and to uniformly cool the glass removed from the mold 2. Uniform cooling ensures uniform shrinkage of the glass, maintaining the straight-line travel of the glass molded body. Additionally, this invention has the advantage of improving the straight-line travel of the glass molded body by performing the operation described above, which brings the temperature of the center and sides of the glass closer together.

[0240] To stabilize the molding conditions, it is preferable to keep the height of the molten glass 9 in the through-hole constant. This can be achieved by keeping the outflow rate of the molten glass 9 from the pipe 1 constant and the speed at which the glass is removed from the outlet constant. However, since the outflow rate of the molten glass may sometimes fluctuate slightly over time, it is preferable to control the speed at which the glass is removed from the mold 2 in a manner that keeps the aforementioned liquid level constant.

[0241] Next, the removal of the glass from the through-hole outlet will be explained.

[0242] As a method for removing glass from the through-hole outlet, any method can be used, such as pulling the glass out of the through-hole outlet by utilizing its own weight to move downwards, or applying a traction force to pull the glass out in addition to the gravity acting on it. Furthermore, since the glass does not substantially stretch during removal, the removal speed of the glass is equivalent to the moving speed of the glass molded body 11 described above. Controlling the removal speed refers to controlling the force pulling out the glass molded body in a way that achieves a desired removal speed; if the glass moves downwards at a speed greater than the desired speed due to its own weight, a force is applied to decelerate the glass molded body, thereby controlling the removal speed to the desired speed.

[0243] If the glass is removed from the through-hole at too high or too low a speed, the height of the molten glass 9 inside the through-hole will be inconsistent, creating a gap between the inner wall of the through-hole and the glass, resulting in unstable dimensions of the glass mold. In extreme cases, the molten glass 9 may overflow from the mold 2, or the glass mold may have a poor shape. Therefore, it is preferable to control the removal speed.

[0244] As an example of controlling the removal speed of the glass molded body, such as Figure 1As shown, a method can be described that holds the side surface 6 formed by the inner wall of the through-hole of the glass being taken out from the outlet of the through-hole and controls the speed at which the glass molded body 11 is taken out from the outlet. For example, the side surface 6 of the solid glass 10 is held by multiple rollers 3, and the rotational speed of the rollers 3 is controlled to control the downward movement speed of the glass molded body without causing the rollers 3 to slip with the glass side surface 6. Preferably, multiple sets of the rollers 3 are arranged along the movement path of the glass molded body, and the weight acting on the glass molded body is supported by multiple sets of rollers in a distributed manner. With this arrangement, the problem of the glass molded body 11 slipping between the rollers 3 and the inability to control the extraction speed can be prevented more reliably. The rollers 3 are preferably arranged in the forming furnace 7. The strain of the glass molded body in the forming furnace 7 is reduced, and the glass molded body below the rollers 3 is in a suspended state due to the holding of the rollers 3. Therefore, even if the glass molded body below the rollers 3 is separated from the glass above, it will not adversely affect the control of the glass extraction speed. Furthermore, since the strain of the glass molded body leaving the forming furnace 7 is reduced, the glass will not break due to the separation of the glass molded body. In addition, if the annealed glass molded body is cut or severed at a position after passing the aforementioned holding position, the flow of molten glass into the mold can be uninterrupted, which is therefore advantageous. If this is done, the weight of the glass molded body to be held will not be excessive, which is advantageous in controlling the glass removal speed. Moreover, the cut glass molded body can be fed into the next process while the glass molded body is being formed, which also improves the productivity of the glass molded body.

[0245] On the other hand, in methods that hold the glass side and control the extraction speed, if the force clamping the glass is too great, the glass will break; therefore, a force exceeding a given value cannot be applied. Consequently, if the glass forming body becomes heavy, it will slip between the rollers, making speed control difficult. To avoid this, a method can be used to control the extraction speed of the glass from the through-hole by supporting the front end of the glass being extracted from the outlet of the through-hole. An example of this is shown below. Figure 2 This method differs from methods that retain the sides because it does not utilize friction to hold the glass molded body, making it suitable for molding heavy glass molded bodies.

[0246] In any of the above-mentioned extraction speed control methods, the extraction speed can be controlled as follows: the height of the molten glass 9 in the mold 2 is monitored by the liquid level sensor 4. Based on the monitoring signal, the extraction speed is increased when the liquid level is higher than the reference height, and decreased when the liquid level is lower than the reference height. For example, the monitoring signal is input to the controller 5 that controls the extraction speed. The controller 5 compares the reference height with the monitored liquid level height and feeds back the result as the extraction speed. When using roller 3 (refer to...) Figure 1In the method of controlling the extraction speed by clamping the side of the glass, the control signal output by the controller 5 can be input to the controller of the motor that rotates the roller 3 to control the rotation speed of the roller 3. In the method of controlling the extraction speed by supporting the front end of the glass being extracted from the through-hole outlet (see...),... Figure 2 In this process, the control signal output by controller 5 can be input to the actuator of the structure supporting the front end (support structure 8) to control the moving speed of the component supporting the front end of the glass to reach the desired speed. There is no particular limitation on the method for monitoring the height of the molten glass surface within the mold; methods such as using a thermometer or laser sensor can be exemplified.

[0247] Furthermore, increasing the angle between the central axis of the through-hole and the vertical line increases the friction between the through-hole of the mold and the side of the glass molded body. Even if the glass molded body is heavy, the removal speed can be controlled by maintaining the side of the glass molded body. Therefore, in the case of making heavy glass molded bodies from glass with not extremely low viscosity at the time of flow, the mold can be configured with the central axis of the through-hole tilted relative to the vertical line.

[0248] Next, the method for separating the glass molded body during removal will be explained.

[0249] For glass removed from the through-hole outlet, by bringing the internal and side temperatures closer together, the risk of internal stress reduction, explosive failure, or breakage due to minor thermal or mechanical shocks is eliminated. Furthermore, to cool the glass to room temperature, it must be pulled out of the mold at a considerable length. This requires a large space under the mold and poses a risk of difficulty in precisely controlling the removal speed due to the excessive weight of the glass mold. Therefore, it is preferable to cut the glass mold when its temperature reaches near its glass transition temperature.

[0250] The specific example of the segmentation method is shown below. Figures 3-5 The preferred method is as follows: Figure 3 As shown, at a given position, on a portion of the side of the glass molded body, a scribing line (gradation line) is formed in a direction perpendicular to the removal direction of the glass molded body by scribing. A fulcrum for local support is provided on the side opposite to the position where the scribing was performed, sandwiched between the central axis of the glass molded body. This fulcrum restricts the movement of the glass molded body above the fulcrum. Simultaneously, pressure is applied horizontally below the scribing position on the side of the glass molded body. Figure 4 As shown, with the fulcrum as the center, the glass molded body is broken from the part where the scribing process has been performed, thus cutting the glass molded body in half.

[0251] In addition, when cutting glass moldings with large outer diameters, the following methods are preferred: Figure 5As shown, a metal sleeve with internal water channels comes into partial contact with the scribing area. Thermal shock generates a crack from the scribing into the glass. The side opposite the scribing, which is sandwiched between the central axis of the glass molded body and supported by a fulcrum, applies force to the glass molded body below the scribing. The torque is applied in such a way that the crack grows towards the part supported by the fulcrum, thus cutting the glass molded body.

[0252] The magnitude of internal stress generated during cooling varies depending on the shape and size of the glass molded body. For example, in the case of extremely thin glass molded bodies such as optical fibers, it is not easy to generate a temperature difference between the interior and the surface. Similarly, for extremely thin sheet glass, it is also not easy to generate a temperature difference between the interior and the surface. Conversely, for rod-shaped glass with a large outer diameter or thick plate-shaped glass, the temperature difference between the interior and the surface increases, making it easier to generate large internal stresses during cooling. Such glass molded bodies include plate-shaped glass with a thickness of 3 mm or more, or rod-shaped glass with an outer diameter of 3 mm or more. Therefore, this invention is suitable for molding plate-shaped glass with a thickness of 3 mm or more, and more suitable for molding plate-shaped glass with a thickness of 5 mm or more. Furthermore, it is suitable for molding rod-shaped glass with an outer diameter of 3 mm or more, more suitable for molding rod-shaped glass with an outer diameter of 5 mm or more, further suitable for molding rod-shaped glass with an outer diameter of 10 mm or more, and even more suitable for molding rod-shaped glass with an outer diameter of 10 mm or more.

[0253] The method described above involves continuously feeding molten glass from a pipe into a mold. This method enables the continuous forming of glass bodies by placing a mold below the outlet of the pipe from which the molten glass flows out.

[0254] Next, we will explain the method of using multiple molds.

[0255] In one approach, the following steps can be repeated: preparing multiple molds and placing one of them below the tube; continuously flowing molten glass into the mold placed below the tube to form a glass molded body; then, interrupting the flow of molten glass into the mold, removing the mold containing the molten glass from below the tube, and removing the glass molded body from the removed mold; after the removal, moving a mold different from the mold containing the molten glass into the tube and placing it below the tube, and then flowing molten glass into the moved-in mold.

[0256] This method is suitable for molding heavy glass bodies made from glass with low viscosity at the time of flow. While this method requires multiple molds, a mechanism for sequentially moving these molds below the tube, and a mechanism for interrupting the flow of molten glass into the molds, it has the advantage of allowing the flow of molten glass into the molds and the complete removal of the glass body from the same mold to occur at different times. Therefore, by interrupting the flow of molten glass into the mold at a given point in time when the length of the glass body reaches a given length, the glass body and mold are removed together from below the tube, allowing it to be removed from the mold without cutting or severing it. Thus, the removal speed of the glass body can be controlled by supporting the front end (lower end), thereby enabling high-precision control of the removal speed of heavy glass bodies, unlike methods that rely on friction to hold the sides of the glass body.

[0257] To interrupt the flow of molten glass, for example, the following method can be used: a cutting blade made of a single blade, suitable for cutting off the low-viscosity molten glass flow during outflow, is inserted between the outlet of the pipe and the inlet of the through hole, cutting off the flow of molten glass. The cutting blade is then removed at the point when the mold is removed from or removed from the mold, restarting the flow of molten glass. In addition to interrupting the flow of molten glass, this method also preferably involves continuously allowing the molten glass flowing out of the pipe to flow into the mold.

[0258] The transfer of the mold can be carried out, for example, by using two molds and alternately moving the molds into and out of the pipe outlet; or by placing three or more molds on a structure such as a turntable that simultaneously transfers multiple molds, and by making the turntable rotate in stages, the molds stop sequentially below the pipe outlet.

[0259] In any method using one mold or multiple molds, it is preferable to arrange the mold such that the pipe is arranged vertically and the center of the molten glass surface within the mold is vertically below the center of the pipe outlet. This arrangement allows the molten glass to flow neatly from the inlet side to the outlet side within the mold, resulting in an optically uniform glass molded body, which is preferable from this perspective.

[0260] According to the above-described method for manufacturing glass molded articles, the contact area between the glass and the inner wall of the through-hole can be increased, allowing for rapid heat dissipation from the glass and thus enabling rapid cooling. This, in turn, prevents devitrification of the glass.

[0261] When the primary objective is to reduce or prevent ripples in the glass molded body, the following method is effective: Using a mold with a straight central axis (inlet and outlet connected in a straight line), the mold is positioned vertically with the central axis of the through-hole, and molten glass continuously flows in from the inlet of the through-hole to form the glass molded body. The shape and size of the through-hole and the material of the mold can be directly applied as described above. Furthermore, it is preferable that the entire circumference of the glass side contacts the inner wall of the through-hole to remove heat from the glass. In this method, as mentioned above, it is preferable to make the pipe from which the molten glass flows out vertical. This arrangement ensures that the flow of glass in the pipe, the direction of movement of glass in the mold, and the direction of gravity acting on the glass are aligned. This prevents mixing between the glass surface and the interior, further reducing or preventing ripples. From the viewpoint of further reducing or preventing ripples, it is preferable to adjust the positional relationship between the pipe and the mold so that the central axis of the pipe is aligned with the central axis of the through-hole during the inflow of molten glass.

[0262] According to the above-described method for manufacturing glass molded bodies, corrugations can be locally present on the surface layer of the glass molded body, enabling the production of optically uniform glass molded bodies without internal corrugations over a large volume range. As described later, the glass molded body obtained in this way can be processed into glass raw materials for pressing, or into optical elements, or the glass raw materials for pressing can be heated and then pressed to produce optical element blanks, optical elements, or the optical element blanks can be processed to produce optical elements.

[0263] Thus, according to the above-described method for manufacturing glass molded articles, optically uniform glass molded articles can be manufactured with high productivity and without breakage.

[0264] [Optical Components]

[0265] One aspect of the present invention relates to an optical element made of the aforementioned optical glass. Specific examples of optical elements include various lenses such as spherical lenses, aspherical lenses, and microlenses, as well as prisms. Furthermore, from an application perspective, the aforementioned optical element is suitable as an interchangeable lens for SLR cameras, a lens for digital cameras, a lens for digital video cameras, a lens for projectors, etc. The surface of these optical elements can be coated with optical thin films such as anti-reflective films as needed.

[0266] The aforementioned optical element can be manufactured using an optical element manufacturing method that includes a process of heating and softening glass raw material made of the aforementioned optical glass and then shaping it.

[0267] Alternatively, the aforementioned optical element can also be manufactured by an optical element manufacturing method comprising the following steps: producing glass raw material from a glass mold made by the aforementioned glass molding method, heating and softening the glass raw material, and molding it.

[0268] Examples of forming methods in the process of heating and softening glass raw materials and shaping them include: a method of pressing softened glass raw materials using a pressing mold; and a method of clamping glass raw materials between rotating rollers using multiple rollers and applying pressure to shape them into rod-shaped glass bodies.

[0269] Compression molding can be further classified into two methods.

[0270] The first method involves heating and softening raw glass, then pressing it into a molding die. After the pressed product is slowly cooled, it is ground and polished to finally produce an optical element. In this method, the raw glass is pressed into a shape that incorporates grinding and polishing allowances for the optical element. The heating and softening process, followed by slow cooling, can be carried out in atmospheric conditions. In another method, raw glass with its entire surface roughened by tumbling or similar processes is used. A powdered release agent, such as boron nitride, is uniformly coated onto the entire surface of the raw glass. It is then heated and softened in a furnace before being placed into a molding die. After being pressed and shaped using upper and lower dies, the die is opened, the pressed product is removed, and placed in a slow cooling furnace to reduce strain and ensure the glass's refractive index precisely matches the target value. After the product cools to room temperature, it is ground and polished using known methods for manufacturing glass optical elements, ultimately producing the optical element. This method can be used to manufacture various optical elements such as spherical lenses and prisms. Anti-reflective coatings and other optical multilayer films can be formed on the surface of optical components as needed.

[0271] The second method involves heating and precision pressing a glass raw material with a smooth surface to create an optical element. Precision pressing, also known as mold optical forming, involves using a pressing mold to shape the entire optical element and precisely transferring the shaped surface onto the glass to form optical functional surfaces. The pressing mold comprises mold components with precision-machined shaped surfaces, and these components are assembled with high precision. In this method, the positional accuracy of multiple optical functional surfaces can be achieved with high precision. For example, it is possible to form a lens that suppresses the tilt and decentering of the central axis of the optical functional surfaces on both sides of the lens. In this second method, the surface of an optical element capable of optical functional surfaces, including those that refract, diffract, reflect, and transmit light, can be formed without relying on machining processes such as grinding and polishing. Therefore, it is possible to manufacture optical elements such as aspherical lenses, which require significant time and cost in machining, with high productivity. Precision pressing can be performed using known methods. For example, a film such as a carbon film, which improves demolding properties and enhances the sliding properties between the glass and the mold forming surface, is formed on the entire surface of the glass raw material for pressing. The glass raw material is heated in a non-oxidizing gas atmosphere and then precision pressed in this atmosphere. Next, the pressing mold is opened, the pressed product is removed, and it is slowly cooled to obtain an optical element. The optical element obtained in this way can be machined as needed, such as for lens centering, around the optical functional surfaces. This method enables the high-volume production of optical elements such as aspherical lenses, spherical lenses, lens arrays, microlenses, diffraction gratings, and prisms. Anti-reflective coatings and other optical multilayer films can be formed on the surface of the optical element as needed.

[0272] Alternatively, as a method for manufacturing optical elements, the following method can be exemplified: The glass molded body is precision annealed to precisely match the refractive index to the desired value, while simultaneously reducing strain in the glass. The glass molded body is then cut or slit to produce a cutting disc. Examples of glass molded body shapes include rod-shaped glass. When cutting the glass perpendicular to the central axis of the rod-shaped glass, the known side-pressure cutting method is preferably used.

[0273] Next, the cutting disc is ground to create an optical element blank with an increased polishing allowance for the shape of the optical element. The blank is then polished to finally produce the optical element. When using rod-shaped glass, it is preferable to make the outer diameter of the rod-shaped glass the same as the outer diameter of the optical element, or to shape it to have an outer diameter with increased grinding and polishing allowances for the outer diameter of the optical element.

[0274] This enables the high-volume manufacturing of various optical components such as lenses, prisms, and filters. Anti-reflective coatings and other multi-layered optical films can be formed on the surface of these components.

[0275] Example

[0276] The present invention will now be described in further detail through embodiments. However, the present invention is not limited to the implementation methods shown in the embodiments.

[0277] [Example 1]

[0278] <Examples No. 1~69>

[0279] Using nitrates, sulfates, carbonates, hydroxides, oxides, boric acids, etc., respectively, as raw materials for introducing each component, in a manner that forms the glass composition shown in the table below, the raw materials are weighed and thoroughly mixed to prepare the blending raw materials.

[0280] The raw materials were placed in a platinum crucible and heated and melted in a melting furnace set at 1400℃~1450℃ for 2 hours. After the molten glass was stirred to homogenize it, it was poured into a preheated mold and allowed to cool naturally to near the glass transition temperature. Then it was immediately placed in an annealing furnace and held at the glass transition temperature for about 30 minutes. It was then slowly cooled at a rate of -30℃ / hour for 4 hours and then allowed to cool naturally to room temperature in the furnace. This yielded the optical glasses No. 1~69 shown in the table below.

[0281] The physical properties of the optical glass thus obtained are shown in the following table.

[0282] The physical properties of optical glass were determined by the methods shown below.

[0283] <Evaluation of the physical properties of optical glass>

[0284] (1) Refractive index nd, Abbe number νd

[0285] The refractive index nd and Abbe number νd of the obtained glass were determined by the refractive index measurement method standard of the Japan Optical Glass Manufacturers Association.

[0286] (2) Glass transition temperature Tg

[0287] The glass was thoroughly pulverized in a mortar to prepare a sample. A platinum box was used as the sample container. The glass transition temperature Tg was determined using a differential scanning calorimeter (DSC3300SA) manufactured by NETZSCH JAPAN with a heating rate of 10 °C / min.

[0288] (3) Specific gravity sg

[0289] The specific gravity was determined using the Archimedes method.

[0290] <Evaluation of Melting Properties>

[0291] Using 50-150g of glass with the glass composition shown in the table below, respectively, nitrates, sulfates, carbonates, hydroxides, oxides, boric acids, etc. are used as raw materials to introduce each component. The raw materials are weighed and thoroughly mixed to prepare the blending raw materials.

[0292] The prepared raw material was placed in a platinum crucible and heated and melted in a melting furnace set at 1400℃~1500℃ for 2 hours. The changes in the raw material immediately after being removed from the melting furnace were evaluated. The state that would become molten glass was marked as "○"; the state that was clearly not molten glass was marked as "×".

[0293] <Evaluation of thermal stability>

[0294] Using 50-150g of glass with the glass composition shown in the table below, respectively, nitrates, sulfates, carbonates, hydroxides, oxides, boric acids, etc. are used as raw materials to introduce each component. The raw materials are weighed and thoroughly mixed to prepare the blending raw materials.

[0295] The raw materials were placed in a platinum crucible and heated and melted in a furnace set at 1400℃~1500℃ for 2 hours to obtain molten glass. 5cc of the molten glass was added to the platinum crucible. The crucible was covered and kept in a furnace heated to 1400℃~1450℃ for 2 hours. It was then quickly removed and rapidly cooled using water or air cooling. When observing the cooled glass, vitrified glass was marked with "○", and opaque glass (cloudy) was marked with "×". In the "○" state, it does not need to be entirely glass; some crystals may be present.

[0296] If both the meltability and thermal stability evaluation results are "○", the rod-shaped glass molded body can be manufactured using the molding method described above. In contrast, if one or both of the meltability and thermal stability evaluation results are "×", it is difficult to apply the molding method described above, and a containerless solidification method must be used.

[0297] [Comparative Example]

[0298] An optical glass having the composition of Example 7 of Japanese Patent Application Publication No. 2016-011228 (Patent Document 1) was manufactured using the previously described method, and its meltability and thermal stability were evaluated using the previously described method. The refractive index and Abbe number of Example 7 shown in Table 1 of Japanese Patent Application Publication No. 2016-011228 (Patent Document 1) are shown in the table described below.

[0299] The results are shown in the table below. In the table, "wt%" represents mass%.

[0300]

[0301]

[0302]

[0303]

[0304]

[0305]

[0306]

[0307]

[0308]

[0309]

[0310]

[0311]

[0312]

[0313]

[0314]

[0315]

[0316]

[0317]

[0318]

[0319]

[0320]

[0321]

[0322]

[0323]

[0324]

[0325]

[0326]

[0327]

[0328] Regarding meltability, Figure 6 The comparison results of the melt properties of the comparative example and Example 1 No. 60 are shown.

[0329] Using a glass composition similar to that of a comparative example, corresponding nitrates, sulfates, carbonates, hydroxides, oxides, and boric acids were used as raw materials for introducing each component. The raw materials were weighed and thoroughly mixed to prepare a formulation. The formulation was added to a platinum crucible and heated in a melting furnace set to 1500°C for 2 hours. The resulting image is Photo A.

[0330] Using the glass composition of Example 1 No. 60, corresponding nitrates, sulfates, carbonates, hydroxides, oxides, boric acid, etc., were used as raw materials for introducing each component, respectively. The raw materials were weighed and thoroughly mixed to prepare a blending material. The blending material was added to a platinum crucible and heated in a melting furnace set to 1400°C for 2 hours. The photograph of the contents of the crucible is Photo B.

[0331] In Photo B, the glass raw material has completely melted and has become molten. This confirms that all the glass from Example 1 shown in the table above exhibits the same melting properties as in Photo B.

[0332] In contrast, in Photo A, despite being heated to a temperature 100°C higher, the glass material did not melt and remained.

[0333] [Example 2]

[0334] Glass raw materials were weighed in a manner that yielded optical glasses identical to those produced in Example 1. After thorough mixing, the mixture was introduced into a melting vessel and heated for melting. Next, the thoroughly clarified and homogenized molten glass was continuously and uninterruptedly fed into a container arranged in a vertically positioned outlet at a constant flow rate. Figure 1The inlet of the through-hole is located at the center of the carbon mold shown. The inner diameter of the through-hole is 20 mm, with the central axis of the through-hole aligned with the vertical direction, and the central axis of the tube aligned with the central axis of the through-hole. The length of the through-hole is set to several hundred mm, and a strip heater (not shown in the figure) is wound around the mold to heat it, thereby appropriately controlling the temperature of the inner wall of the through-hole to achieve good molding. The side of the cylindrical glass rod taken out from the through-hole outlet is held by two rollers, and the removal speed of the cylindrical glass rod is controlled. The height of the molten glass in the through-hole of the mold is monitored using a liquid level sensor (laser sensor), and the monitoring signal output by the sensor is input to the roller controller to control the electrical input to the motor that rotates the roller, so that the liquid level is kept constant. In this embodiment, the removal speed of the cylindrical glass rod is controlled as follows: that is, the rotation speed of the roller is fed back according to the change in the liquid level, so that the liquid level remains constant.

[0335] Thus, cylindrical glass rods with an outer diameter of 20 mm are continuously removed from the through-hole outlet. A forming furnace is positioned directly below the mold, allowing the cylindrical glass rods removed from the mold to be immediately moved into the forming furnace. A heater (not shown in the figure) is positioned inside the forming furnace to maintain the temperature of the gas atmosphere within the furnace at a temperature range that prevents the cylindrical glass rods from breaking. The aforementioned rollers are positioned inside the forming furnace. As the cylindrical glass rods pass through the forming furnace over time, the temperature of the center and surface of the rod tends to approach each other, thus preventing the generation of internal stresses that could cause explosive breakage of the rod itself, and enabling the glass to be formed into cylindrical shapes without breakage.

[0336] Next, a scribing process is performed on a portion of the side of the cylindrical glass sample delivered from the forming furnace, along a direction perpendicular to the central axis of the cylindrical glass. Then, a metal sleeve containing water flowing within the internal water channels is brought into contact with the scribing to locally cool the scribed area, causing a crack to extend from the scribing towards the center. At this time, the metal sleeve follows the movement of the cylindrical glass, maintaining contact with the scribing. At the point where the crack has propagated, the opposite side of the scribed portion is supported by a fulcrum relative to the central axis of the cylindrical glass, and the side of the glass sample below the scribing is pressed, separating the cylindrical glass sample above the height of the scribing from the cylindrical glass sample below. It should be noted that the outer diameter of the cylindrical glass sample in this embodiment is relatively small, at 20 mm, therefore, good separation can be achieved even without applying thermal shock from the contact with the metal sleeve.

[0337] During separation, a robotic arm holds the sides of the cylindrical glass to be separated. After separation, the cylindrical glass, still held by the robotic arm, is transferred to the inlet of a continuous slow cooling furnace located next to the casting and forming furnace. A heater and a conveyor belt for transporting the glass are installed inside the continuous slow cooling furnace. In the furnace, where the temperature distribution is controlled, the cylindrical glass, carried on the conveyor belt, is slowly cooled to remove strain as it moves.

[0338] The cylindrical glass, taken from a continuous slow cooling furnace, was cut, the cut surface was polished, and the interior was observed. The results showed that ribs were only visible in a very shallow layer from the surface; no ribs were identified in deeper layers. That is, most of the cylindrical glass was optically homogeneous.

[0339] [Example 3]

[0340] Using the slowly cooled cylindrical glass prepared in Example 2, glass raw materials for pressing were produced. First, scribing was performed on the cut-off portion of the cylindrical glass. Then, the cylindrical glass was inserted into a high-pressure vessel with the scribing portion positioned in the center of the vessel. The cylindrical glass was clamped at the opening of the vessel using a rubber seal, allowing for movement without restricting the central axis direction. Water was then injected into the vessel, filling it completely to prevent air bubbles from entering.

[0341] In this state, the water pressure inside the container is increased, and the cylindrical glass is cut perpendicular to the central axis at the marked position. Thus, the cylindrical glass is cut at given intervals, producing a cutting disc.

[0342] Next, the cutting disc is tumbled and ground to a weight equal to that of the target pressed product. At the same time, the sharp edges are rounded and the surface is roughened to produce glass raw material for pressing.

[0343] In addition, the aforementioned cutting discs were ground and polished to produce a smooth-surfaced glass raw material for precision pressing and molding.

[0344] [Example 4]

[0345] In Example 3, the entire surface of the glass raw material for pressing and molding was uniformly coated with a powdered release agent made of boron nitride, and then placed in a heating furnace. While being moved inside the furnace, it was heated and softened in the atmosphere.

[0346] The softened glass raw material is fed into a pressing mold consisting of an upper mold, a lower mold, and a mold body. It is pressed and formed in the atmosphere. The mold is opened and the pressed product is taken out and placed in a slow cooling furnace for precision annealing. After cooling to room temperature, it is made into an optical component blank.

[0347] Next, the blanks were ground and polished to produce spherical lenses made of various optical glasses. No devitrification or ridges were observed inside the lenses, resulting in optically uniform optical elements.

[0348] [Example 5]

[0349] In Example 3, a carbon film was formed on the entire surface of the glass raw material for precision pressing. The material was heated in a mixed atmosphere of nitrogen and hydrogen, and precision pressing was performed using a pressing mold with the carbon film attached to the forming surface of a SiC profile as a release film. The precision-pressed product was then slowly cooled to obtain an aspherical lens made of various optical glasses.

[0350] No devitrification or ridges were observed inside the lens, resulting in an optically uniform element.

[0351] [Example 6]

[0352] The cylindrical glass prepared in Example 2, which had undergone precision annealing, was cut perpendicularly to its central axis using a side-pressure cutting method to create a cutting disc. The cutting disc was then ground and polished to fabricate a spherical lens made of various optical glasses. No devitrification or ridges were observed inside the lens, resulting in an optically uniform element.

[0353] It should be understood that the embodiments disclosed herein are exemplary in all respects and do not constitute a limitation. The scope of the invention is defined by the claims, not by the foregoing description, and is intended to include all modifications within the meaning and scope of the claims.

[0354] For example, by adjusting the composition described in the specification, an optical glass according to one aspect of the present invention can be obtained from the glass composition exemplified above.

[0355] In addition, of course, any combination of two or more items described in the specification as examples or preferred options is possible.

Claims

1. An optical glass, wherein, Based on quality standards, The SiO2 content is above 2.50% and below 15.00%. The B2O3 content is above 2.00% and below 17.50%. The La2O3 content is above 40.00%. The Nb₂O₅ content is greater than 0.00% and less than 14.00%. The total content of SiO2 and B2O3 (SiO2+B2O3) is above 14.00% and below 20.00%. Rare earth oxides (La₂O₃, Gd₂O₃, Y₂O₃, and Yb₂O₃) are represented as Ln₂O₃. The Ln2O3 content is the total content of La2O3, Gd2O3, Y2O3, and Yb2O3 (La2O3+Gd2O3+Y2O3+Yb2O3). The Ln2O3 content is above 50.00%. The mass ratio of Ln2O3 content to the total content of SiO2 and B2O3 (Ln2O3 / (SiO2+B2O3)) is greater than 3.

41. The total content of Nb2O5, TiO2, WO3, and Ta2O5 (Nb2O5+TiO2+WO3+Ta2O5) is less than 14.00%. The mass ratio of TiO2 content to the total content of SiO2 and B2O3 (TiO2 / (SiO2+B2O3)) is less than 0.

17. The value obtained by subtracting the contents of Nb2O5, TiO2, WO3, and Ta2O5 from the Ln2O3 content (Ln2O3-Nb2O5-TiO2-WO3-Ta2O5) is over 49.00%, and... Let y be the mass ratio of Ln2O3 content to the total content of Ln2O3, SiO2, and B2O3 (Ln2O3 / (Ln2O3+SiO2+B2O3)). And with the mass ratio of Ln2O3 content to the total content of Ln2O3, Nb2O5, TiO2, WO3, and Ta2O5 (Ln2O3 / (Ln2O3+Nb2O5+TiO2+WO3+Ta2O5)) set as x, The condition y ≥ -0.7058x + 1.38 is satisfied.

2. The optical glass according to claim 1, wherein, The Ta2O5 content is above 0.00% and below 15.00%.

3. The optical glass according to claim 1, wherein, The total content of SiO2, B2O3 and P2O5 (SiO2+B2O3+P2O5) is above 14.00% and below 19.50%.

4. The optical glass according to claim 1, wherein, The mass ratio of Ln2O3 content to the total content of Ln2O3, Nb2O5, TiO2, WO3 and Ta2O5 (Ln2O3 / (Ln2O3+Nb2O5+TiO2+WO3+Ta2O5)) is greater than 0.

845.

5. The optical glass according to claim 1, wherein, The total content of ZnO, ZrO2, Nb2O5, TiO2, WO3 and Ta2O5 (ZnO+ZrO2+Nb2O5+TiO2+WO3+Ta2O5) is above 6.00%.

6. The optical glass according to claim 1, wherein y ≥ -0.2797x + 1.0181.

7. The optical glass according to claim 1, wherein, The refractive index nd and the Abbe number νd satisfy the following equation: nd≥-0.01000×νd+2.28500.

8. The optical glass according to claim 1, wherein, The Ta2O5 content is above 0.00% and below 15.00%. The total content of SiO2, B2O3, and P2O5 (SiO2+B2O3+P2O5) is above 14.00% and below 19.50%. The mass ratio of Ln2O3 content to the total content of Ln2O3, Nb2O5, TiO2, WO3, and Ta2O5 (Ln2O3 / (Ln2O3+Nb2O5+TiO2+WO3+Ta2O5)) is greater than 0.

845. The total content of ZnO, ZrO2, Nb2O5, TiO2, WO3, and Ta2O5 (ZnO+ZrO2+Nb2O5+TiO2+WO3+Ta2O5) is above 6.00%. It satisfies y ≥ -0.2797x + 1.0181, and The refractive index nd and the Abbe number νd satisfy the following equation: nd≥-0.01000×νd+2.28500.

9. An optical element made of the optical glass according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Optical glass

    JP2016011228A