An alkali-free glass for TFTs and its preparation method
By adjusting the composition of alkali-free glass, especially by reducing or removing MgO and optimizing the proportion of other oxides, alkali-free glass with low liquidus temperature and high mechanical strength was prepared, solving the crystallization problem of TFT alkali-free glass and improving the quality of display panels.
Patent Information
- Application Number
- CN202611212235.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-17
AI Technical Summary
The high liquidus temperature of existing TFT alkali-free glass increases the risk of crystallization, affecting the optical uniformity and surface flatness of the glass, and consequently impacting the quality of the display panel.
By adjusting the proportions of SiO2, Al2O3, B2O3, CaO, SrO, BaO, and ZnO, and combining them with a clarifying agent, an alkali-free glass without MgO was prepared, which lowered the liquidus temperature and improved the mechanical strength.
This significantly reduces the liquidus temperature of alkali-free glass, improves its resistance to crystallization, ensures its mechanical strength and optical uniformity, and enhances the performance of the display panel.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of glass substrate technology for displays, and specifically relates to an alkali-free glass for TFTs and its preparation method. Background Technology
[0002] TFT-LCD, or Thin Film Transistor Liquid Crystal Display, is a technology that cleverly combines microelectronics and liquid crystal display (LCD) technologies. It transfers the precision microelectronic processing techniques used on single-crystal glass to the fabrication of thin film transistor (TFT) arrays on large-area glass. This array substrate, along with another substrate containing a color filter, is then combined with mature LCD technology to form a liquid crystal cell. Subsequent processes, such as polarizer lamination, complete the liquid crystal display device. The manufacturing process of LCD panels is extremely complex, and the requirements for materials are very stringent. The glass substrate of a TFT-LCD is the core component of the LCD panel and a key strategic material in the electronic information display industry. Its performance directly determines the final quality, manufacturing cost, and product yield of the panel. First, the coefficient of thermal expansion of the glass substrate used in the manufacture of display devices must be strictly controlled to avoid stress problems caused by mismatch in the coefficient of thermal expansion during the manufacturing process. Second, the glass substrate must have excellent chemical resistance to avoid unnecessary damage to the glass substrate caused by the etching process during production. Third, the manufacturing process has high requirements for the heat resistance of the glass substrate, such as high strain point temperature and low thermal shrinkage, to avoid deformation of the glass due to heat treatment. Fourth, the glass used in the manufacture of display devices must have excellent uniformity and flatness.
[0003] The alkali-free glass system uses SiO2 as the network forging body and Al2O3 as the network intermediate, supplemented by B2O3 and alkaline earth metal oxides for performance regulation. Among these, magnesium oxide (MgO), as one of the most important alkaline earth metal components, plays an irreplaceable role in glass melting, structure regulation, and performance optimization, and is an indispensable key component in the alkali-free glass formulation. Because alkali-free glass does not contain strong fluxing components such as sodium and potassium, its melting temperature is significantly higher than that of ordinary soda-lime glass. MgO, as a network modifier, introduces magnesium... 2+ With its small ionic radius and high field strength, MgO can break some of the Si-O bonds in the silicon-oxygen network, reducing the high-temperature viscosity of the glass melt and making the batch more easily melted into a homogeneous glass phase. This not only directly reduces production costs but also mitigates the erosion of the furnace refractory materials by the high-temperature melt, significantly extending the furnace's service life. Compared with other alkaline earth metal oxides such as CaO, SrO, and BaO, MgO can effectively maintain the high strain point of glass without significantly increasing the coefficient of thermal expansion.
[0004] TFT alkali-free glass incorporates magnesium oxide to reduce melting difficulty and increase Young's modulus. However, magnesium oxide raises the liquidus temperature. The liquidus temperature of glass is the highest temperature at which the molten glass phase and the crystalline phase can coexist in equilibrium; that is, the lowest temperature at which the glass can melt without crystallization. TFT substrate glass is primarily produced using the overflow pull-down method. The forming process requires the molten glass to maintain a stable liquid phase state at the forming temperature, which must be significantly higher than the liquidus temperature. An increased liquidus temperature means the molten glass spends a longer time in the "crystallization-sensitive zone" during the cooling path, significantly increasing the probability of nucleation and crystal growth. Microcrystals precipitated inside the glass form defects, disrupting optical uniformity, causing light scattering and increased screen haze, directly leading to display defects such as bright spots and dark spots on the display panel. Furthermore, microcrystal protrusions on the substrate surface disrupt submicron-level surface flatness, causing pattern distortion and alignment deviations in subsequent photolithography processes.
[0005] Therefore, ensuring that alkali-free glass has good mechanical strength while also having a lower liquidus temperature is of great significance for improving the glass's resistance to crystallization during the glassmaking process and thus improving the quality of the glass. Summary of the Invention
[0006] To address the shortcomings of existing technologies, this invention provides a method for preparing alkali-free glass for TFTs. This alkali-free glass meets the requirements of TFT processes for glass substrates, exhibits a lower liquidus temperature, and possesses good mechanical strength, thus solving the technical problems mentioned in the background art. Specifically, the technical solution of this invention includes the following: One objective of this invention is to provide an alkali-free glass for TFTs, wherein the alkali-free glass comprises the following raw materials by weight percentage: 56%~63% SiO2; 15%~20% Al2O3; 9%~13% B2O3; 4%~8% CaO; 3.1%~5% SrO; 0%~6% BaO; 0%~1% ZnO; 0% MgO; 0.1-0.5% clarifying agent.
[0007] Furthermore, the clarifying agent includes tin oxide, but may also be sodium sulfate, sodium nitrate, potassium nitrate, sodium chloride, strontium chloride, calcium fluoride, or stannous oxide.
[0008] Furthermore, the ratio of SrO to (CaO+SrO+BaO) is 0.242~0.534.
[0009] Preferably, the ratio of SrO to (CaO+SrO+BaO) is 0.242~0.425.
[0010] Preferably, the alkali-free glass comprises the following raw materials by weight percentage: 59.00% SiO2; 17.00% Al2O3; 9.00% B2O3; 4.60% CaO; 4.20% SrO; 6.00% BaO; 0.20% clarifying agent.
[0011] Preferably, the alkali-free glass comprises the following raw materials by weight percentage: 60.90% SiO2; 18.10% Al2O3; 9.50% B2O3; 4.00% CaO; 4.50% SrO; 2.10% BaO; 0.60% ZnO; 0.30% clarifying agent.
[0012] Preferably, the alkali-free glass comprises the following raw materials by weight percentage: 56.05% SiO2; 20.00% Al2O3; 11.00% B2O3; 4.90% CaO; 3.10% SrO; 4.80% BaO; 0.15% clarifying agent.
[0013] A second objective of this invention is to provide a method for preparing alkali-free glass for TFTs, the method comprising the following steps: According to the mass percentage, 56%~63% SiO2, 15%~20% Al2O3, 9%~13% B2O3, 4%~8% CaO, 3.1%~5% SrO, 0%~6% BaO, 0%~1% ZnO and 0.1~0.5% clarifying agent are mixed and heated to obtain glass melt; The alkali-free glass is obtained by annealing the glass melt and then grinding and polishing it.
[0014] Furthermore, the process parameters for the mixed heating include a temperature of 1500℃~1650℃, a rotation speed of 50r / min~100r / min, and a processing time of 4h~8h.
[0015] Furthermore, the process parameters for the annealing treatment include a temperature of 700℃~750℃ and a treatment time of 1h~3h.
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: The alkali-free glass of this invention eliminates MgO, which easily leads to a high liquidus temperature. SiO2, an essential component for the network structure, improves the glass's heat resistance and chemical durability, allowing it to achieve higher strain points and strength. However, too little SiO2 deteriorates the glass's main network structure, increasing its dielectric constant and reducing its mechanical and heat resistance. Too much SiO2 raises the melting temperature, increases brittleness, and places excessive demands on the production process, making melting difficult. Conventional furnaces struggle to meet the demands of high-capacity melting techniques for batch material melting. Al2O3 acts as a network former, promoting the integrity of network connections and significantly improving the glass's heat resistance and mechanical stability. However, it also makes the glass structure more rigid, increasing its brittleness. B₂O₃, as a glass-forming oxide, can form glass on its own. Its addition enhances the chemical stability and mechanical properties of glass, reduces its coefficient of thermal expansion, and lowers its dielectric constant. B₂O₃ is also a good flux, significantly lowering the glass melting temperature and aiding the vitrification process. CaO, SrO, and BaO are all alkaline earth metal oxides. The addition of CaO and SrO helps optimize the chemical and mechanical properties of glass, while adjusting its physical characteristics to meet the high-performance glass requirements of the liquid crystal display industry. The addition of BaO helps lower the dielectric constant of glass, thereby reducing the impact of electron migration in liquid crystal displays and improving the performance of the display panel. ZnO has an 18-element outer-shell electron structure. Compared to alkaline earth metals, ZnO... 2+ Ions are more easily polarized, which can reduce glass viscosity at high temperatures and make it less prone to crystal nucleation, thus lowering the upper limit of glass crystallization temperature. However, when the ZnO content is too high, the destructive and depolymerizing effects of ZnO on the glass network structure increase, which is detrimental to improving glass performance. By adjusting the ratio between SiO2, Al2O3, B2O3, CaO, SrO, BaO, and ZnO, the prepared alkali-free glass not only has good mechanical strength but also a significantly lower liquidus temperature, resulting in excellent performance. Detailed Implementation
[0017] The technical solution of the present invention will be clearly and completely described below through embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0018] Unless otherwise stated, all raw materials and reagents used in this invention are commercially available or can be prepared by known methods.
[0019] Example 1 A method for preparing alkali-free glass for TFTs is shown below: According to the mass percentages, 61.00% SiO2, 16.00% Al2O3, 11.00% B2O3, 6.60% CaO, 5.00% SrO, 0.20% ZnO, and 0.20% SnO2 were mixed and stirred at 600 rpm for 30 minutes. The mixture was then poured into a crucible, heated to 1500℃, and stirred at 50 rpm for 4 hours to obtain a glass melt. The glass melt was then poured into a mold and transferred to an annealing furnace at 700℃ for 1 hour. After annealing, the glass was cooled to room temperature in the furnace and then polished to obtain alkali-free glass with a thickness of 0.7 mm.
[0020] Example 2 A method for preparing alkali-free glass for TFTs is shown below: According to the mass percentages, 61.60% SiO2, 15.00% Al2O3, 12.00% B2O3, 6.00% CaO, 5.00% SrO, 0.10% BaO, and 0.30% SnO2 were mixed and stirred at 600 rpm for 30 minutes. The mixture was then poured into a crucible, heated to 1500℃, and the stirring speed was controlled at 50 rpm. The mixture was stirred and melted at this temperature for 4 hours to obtain a glass melt. The glass melt was then poured into a mold and transferred to an annealing furnace at 700℃ for 1 hour of annealing. After annealing, the glass was cooled to room temperature in the furnace and then polished to obtain alkali-free glass with a thickness of 0.7 mm.
[0021] Example 3 A method for preparing alkali-free glass for TFTs is shown below: According to the mass percentages, 63.00% SiO2, 15.30% Al2O3, 10.00% B2O3, 5.60% CaO, 4.80% SrO, 0.90% BaO, 0.30% ZnO, and 0.1% SnO2 were mixed and stirred at 600 rpm for 30 minutes. The mixture was then poured into a crucible, heated to 1500℃, and the stirring speed was controlled at 50 rpm. The mixture was stirred and melted at this temperature for 4 hours to obtain a glass melt. The glass melt was then poured into a mold and transferred to an annealing furnace at 700℃ for 1 hour of annealing. After annealing, the glass was cooled to room temperature in the furnace and then polished to obtain alkali-free glass with a thickness of 0.7 mm.
[0022] Example 4 A method for preparing alkali-free glass for TFTs is shown below: According to the mass percentages, 56.05% SiO2, 20.00% Al2O3, 11.00% B2O3, 4.90% CaO, 3.10% SrO, 4.80% BaO, and 0.15% SnO2 were mixed and stirred at 600 rpm for 30 minutes. The mixture was then poured into a crucible, heated to 1550℃, and stirred at 50 rpm for 5 hours to obtain a glass melt. The glass melt was then poured into a mold and transferred to an annealing furnace at 710℃ for 1 hour. After annealing, the glass was cooled to room temperature in the furnace and then polished to obtain alkali-free glass with a thickness of 0.7 mm.
[0023] Example 5 A method for preparing alkali-free glass for TFTs is shown below: According to the mass percentages, 59.00% SiO2, 17.00% Al2O3, 9.00% B2O3, 4.60% CaO, 4.20% SrO, 6.00% BaO, and 0.20% SnO2 were mixed and stirred at 600 rpm for 30 minutes. The mixture was then poured into a crucible, heated to 1550℃, and stirred at 50 rpm for 5 hours to obtain a glass melt. The glass melt was then poured into a mold and transferred to an annealing furnace at 710℃ for 1 hour. After annealing, the glass was cooled to room temperature in the furnace and then polished to obtain alkali-free glass with a thickness of 0.7 mm.
[0024] Example 6 A method for preparing alkali-free glass for TFTs is shown below: According to the mass percentages, 61.00% SiO2, 16.00% Al2O3, 13.00% B2O3, 4.10% CaO, 4.70% SrO, 1.00% ZnO, and 0.20% SnO2 were mixed and stirred at 600 rpm for 30 minutes. The mixture was then poured into a crucible, heated to 1550℃, and stirred at 50 rpm for 6 hours to obtain a glass melt. The glass melt was then poured into a mold and transferred to an annealing furnace at 720℃ for 1 hour. After annealing, the glass was cooled to room temperature in the furnace and then polished to obtain alkali-free glass with a thickness of 0.7 mm.
[0025] Example 7 A method for preparing alkali-free glass for TFTs is shown below: According to the mass percentages, 61.00% SiO2, 16% Al2O3, 10.00% B2O3, 7.30% CaO, 5.00% SrO, 0.20% BaO, and 0.5% SnO2 were mixed and stirred at 600 rpm for 30 minutes. The mixture was then poured into a crucible, heated to 1550℃, and the stirring speed was controlled at 100 rpm. The mixture was stirred and melted at this temperature for 6 hours to obtain a glass melt. The glass melt was then poured into a mold and transferred to an annealing furnace at 720℃ for 2 hours of annealing. After annealing, the glass was cooled to room temperature in the furnace and then polished to obtain alkali-free glass with a thickness of 0.7 mm.
[0026] Example 8 A method for preparing alkali-free glass for TFTs is shown below: According to the mass percentage, 60.00% SiO2, 16.40% Al2O3, 11.00% B2O3, 8.00% CaO, 4.40% SrO, and 0.20% SnO2 were mixed and stirred at 600 rpm for 30 minutes. The mixture was then poured into a crucible, heated to 1550℃, and the stirring speed was controlled at 100 rpm. The mixture was stirred and melted at this temperature for 7 hours to obtain a glass melt. The glass melt was then poured into a mold and transferred to an annealing furnace at 730℃ for 2 hours of annealing. After annealing, the glass was cooled to room temperature in the furnace and then polished to obtain alkali-free glass with a thickness of 0.7 mm.
[0027] Example 9 A method for preparing alkali-free glass for TFTs is shown below: According to the mass percentages, 60.90% SiO2, 18.10% Al2O3, 9.50% B2O3, 4.00% CaO, 4.50% SrO, 2.10% BaO, 0.60% ZnO, and 0.30% SnO2 were mixed and stirred at 600 rpm for 30 minutes. The mixture was then poured into a crucible, heated to 1550℃, and stirred at 100 rpm for 7 hours to obtain a glass melt. The glass melt was then poured into a mold and transferred to an annealing furnace at 730℃ for 2 hours. After annealing, the glass was cooled to room temperature in the furnace and then polished to obtain alkali-free glass with a thickness of 0.7 mm.
[0028] Example 10 A method for preparing alkali-free glass for TFTs is shown below: According to the mass percentages, 61.00% SiO2, 16.00% Al2O3, 10.80% B2O3, 6.80% CaO, 5.00% SrO, 0.20% ZnO, and 0.20% SnO2 were mixed and stirred at 600 rpm for 30 minutes. The mixture was then poured into a crucible, heated to 1600℃, and stirred at 100 rpm for 7 hours to obtain a glass melt. The glass melt was then poured into a mold and transferred to an annealing furnace at 740℃ for 2 hours. After annealing, the glass was cooled to room temperature in the furnace and then polished to obtain alkali-free glass with a thickness of 0.7 mm.
[0029] Example 11 A method for preparing alkali-free glass for TFTs is shown below: According to the mass percentages, 61.00% SiO2, 16.50% Al2O3, 11.00% B2O3, 6.10% CaO, 5.00% SrO, 0.20% ZnO, and 0.20% SnO2 were mixed and stirred at 600 rpm for 30 minutes. The mixture was then poured into a crucible, heated to 1600℃, and stirred at 100 rpm for 8 hours to obtain a glass melt. The glass melt was then poured into a mold and transferred to an annealing furnace at 750℃ for 3 hours. After annealing, the glass was cooled to room temperature in the furnace and then polished to obtain alkali-free glass with a thickness of 0.7 mm.
[0030] Example 12 A method for preparing alkali-free glass for TFTs is shown below: According to the mass percentages, 59.30% SiO2, 17.00% Al2O3, 11.00% B2O3, 6.60% CaO, 5.00% SrO, 0.70% BaO, 0.20% ZnO, and 0.20% SnO2 were mixed and stirred at 600 rpm for 30 minutes. The mixture was then poured into a crucible, heated to 1650℃, and the stirring speed was controlled at 100 rpm. The mixture was stirred and melted at this temperature for 8 hours to obtain a glass melt. The glass melt was then poured into a mold and transferred to an annealing furnace at 750℃ for 3 hours of annealing. After annealing, the glass was cooled to room temperature in the furnace and then polished to obtain alkali-free glass with a thickness of 0.7 mm.
[0031] Comparative Example 1 A method for preparing alkali-free glass for TFTs is shown below: According to the mass percentages, 60.30% SiO2, 16.00% Al2O3, 10.00% B2O3, 3.00% MgO, 6.00% CaO, 4.30% SrO, 0.20% ZnO, and 0.20% SnO2 were mixed and stirred at 600 rpm for 30 minutes. The mixture was then poured into a crucible, heated to 1650℃, and the stirring speed was controlled at 100 rpm. The mixture was stirred and melted at this temperature for 8 hours to obtain a glass melt. The glass melt was then poured into a mold and transferred to an annealing furnace at 750℃ for 3 hours of annealing. After annealing, the glass was cooled to room temperature in the furnace and removed, then polished to obtain alkali-free glass with a thickness of 0.7 mm.
[0032] Comparative Example 2 A method for preparing alkali-free glass for TFTs is shown below: According to the mass percentages, 61.00% SiO2, 17.10% Al2O3, 12.00% B2O3, 4.50% CaO, 5.00% SrO, 0.20% ZnO, and 0.20% SnO2 were mixed and stirred at 600 rpm for 30 minutes. The mixture was then poured into a crucible, heated to 1650℃, and the stirring speed was controlled at 100 rpm. The mixture was stirred and melted at this temperature for 8 hours to obtain a glass melt. The glass melt was then poured into a mold and transferred to an annealing furnace at 750℃ for 3 hours of annealing. After annealing, the glass was cooled to room temperature in the furnace and then polished to obtain alkali-free glass with a thickness of 0.7 mm.
[0033] Comparative Example 3 A method for preparing alkali-free glass for TFTs is shown below: According to the mass percentages, 61.00% SiO2, 16.00% Al2O3, 11.00% B2O3, 6.60% CaO, 1.20% SrO, 3.80% BaO, 0.20% ZnO, and 0.20% SnO2 were mixed and stirred at 600 rpm for 30 minutes. The mixture was then poured into a crucible, heated to 1650℃, and the stirring speed was controlled at 100 rpm. The mixture was stirred and melted at this temperature for 8 hours to obtain a glass melt. The glass melt was then poured into a mold and transferred to an annealing furnace at 750℃ for 3 hours of annealing. After annealing, the glass was cooled to room temperature in the furnace and then polished to obtain alkali-free glass with a thickness of 0.7 mm.
[0034] The alkali-free glasses obtained in Examples 1-12 and Comparative Examples 1-3 were tested for relevant properties according to the following test methods: The density of glass was determined according to ASTM C-693, and the unit is g / cm³. 3 ; The coefficient of thermal expansion of glass between 50 and 350°C was determined using a horizontal dilatometer according to ASTM E-228, with units expressed as ×10⁻¹⁰. -7 / ℃; The Young's modulus of glass was determined using a mechanical testing machine according to ASTM C-623, with units of GPa. The strain point of glass was determined using an annealing point strain tester according to ASTM C-336, with the unit being °C. The temperature corresponding to an alkali-free glass with a viscosity of 200 P was determined using a rotational high-temperature viscometer according to ASTM C-965, and the unit is °C. The glass liquidus temperature TL was determined using the gradient furnace method according to ASTM C-829, with units in °C. The results are shown in Table 1.
[0035] Table 1. Performance Test Results of Alkali-Free Glass
[0036] The following conclusions can be drawn from Table 1 above: (1) As can be seen from Examples 1 to 12, the alkali-free glass prepared by the present invention has the following characteristics: density ≤ 3.5 g / cm³. 3 The coefficient of thermal expansion in the temperature range of 50-350℃ is less than 40×10. -7 / ℃; Young's modulus ≥72GPa; strain point >660℃; liquidus temperature ≤1130℃; temperature T200 corresponding to viscosity of 200P ≤1630℃; indicating that alkali-free glass not only has good mechanical properties, but also a significantly reduced liquidus temperature. In addition, it also achieves a low coefficient of thermal expansion and a high strain point temperature, demonstrating excellent performance.
[0037] (2) Through comparative examples 1 to 3, it can be found that the components of the alkali-free glass of the present invention have a synergistic promoting effect within a certain range. When the amount of certain raw materials is changed, its Young's modulus will be weakened, and the liquidus temperature and T200 will increase, which is not conducive to improving the performance of the alkali-free glass.
[0038] The embodiments described above provide a detailed explanation of the technical solutions and beneficial effects of the present invention. It should be understood that the above descriptions are merely specific embodiments of the present invention and are not intended to limit the present invention. Various changes and modifications can be made to the present invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed.
Claims
1. An alkali-free glass for TFTs, characterized in that, The alkali-free glass comprises the following raw materials by weight percentage: 56%~63% SiO2; 15%~20% Al2O3; 9%~13% B2O3; 4%~8% CaO; 3.1%~5% SrO; 0%~6% BaO; 0%~1% ZnO; 0% MgO; 0.1-0.5% clarifying agent.
2. The alkali-free glass for TFTs according to claim 1, characterized in that, The clarifying agent includes tin oxide.
3. The alkali-free glass for TFTs according to claim 1, characterized in that, The ratio of SrO to (CaO+SrO+BaO) is 0.242~0.
534.
4. The alkali-free glass for TFTs according to claim 3, characterized in that, The ratio of SrO to (CaO+SrO+BaO) is 0.242~0.
425.
5. The alkali-free glass for TFTs according to claim 1, characterized in that, The alkali-free glass comprises the following raw materials by weight percentage: 59.00% SiO2; 17.00% Al2O3; 9.00% B2O3; 4.60% CaO; 4.20% SrO; 6.00% BaO; 0.20% clarifying agent.
6. The alkali-free glass for TFTs according to claim 1, characterized in that, The alkali-free glass comprises the following raw materials by weight percentage: 60.90% SiO2; 18.10% Al2O3; 9.50% B2O3; 4.00% CaO; 4.50% SrO; 2.10% BaO; 0.60% ZnO; 0.30% clarifying agent.
7. The alkali-free glass for TFTs according to claim 1, characterized in that, The alkali-free glass comprises the following raw materials by weight percentage: 56.05% SiO2; 20.00% Al2O3; 11.00% B2O3; 4.90% CaO; 3.10% SrO; 4.80% BaO; 0.15% clarifying agent.
8. A method for preparing alkali-free glass for TFTs as described in any one of claims 1 to 7, characterized in that, The preparation method includes the following steps: According to the mass percentage, 56%~63% SiO2, 15%~20% Al2O3, 9%~13% B2O3, 4%~8% CaO, 3.1%~5% SrO, 0%~6% BaO, 0%~1% ZnO and 0.1~0.5% clarifying agent are mixed and heated to obtain glass melt; The alkali-free glass is obtained by annealing the glass melt and then grinding and polishing it.
9. The method for preparing alkali-free glass for TFTs according to claim 8, characterized in that, The process parameters for the mixed heating include a temperature of 1500℃~1650℃, a rotation speed of 50r / min~100r / min, and a processing time of 4h~8h.
10. The method for preparing alkali-free glass for TFTs according to claim 8, characterized in that, The process parameters for the annealing treatment include a temperature of 700℃~750℃ and a treatment time of 1h~3h.