A special glaze for titanium metal and titanium alloys containing rare earth oxides and its preparation method.

By preparing glazes containing rare earth oxides and zirconium oxide, the problems of thermal expansion mismatch and low bonding strength between the glaze and titanium metal/titanium alloy were solved. This resulted in good thermal expansion matching and high bonding strength between the glaze and titanium metal/titanium alloy, improving thermal shock resistance and extending service life.

CN123105989APending Publication Date: 2026-11-17AMBERS (WUXI) NEW MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611488281.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-23
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing glazes do not match the coefficient of thermal expansion of titanium metal/titanium alloys, resulting in low bonding strength and poor thermal shock resistance, which makes them prone to cracking and peeling in high-temperature or corrosive environments.

Method used

Feldspar glazes containing rare earth oxides, tin oxide, and zirconium oxide are used to prepare glazes that match the thermal expansion of titanium metal/titanium alloys, have high bonding strength, and are resistant to thermal shock. The process involves high-temperature melting, water quenching, grinding, and glaze slurry preparation, combined with firing in a vacuum or weak oxidizing atmosphere.

Benefits of technology

It achieves good thermal expansion matching between the glaze and titanium metal/titanium alloy, improves the bonding strength and thermal shock resistance, reduces high-temperature oxidation and corrosion, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105989A_ABST
    Figure CN123105989A_ABST
Patent Text Reader

Abstract

This invention discloses a special glaze for titanium metal and titanium alloys containing rare earth oxides and its preparation method. The raw materials include: potassium feldspar, quartz sand, aluminum hydroxide, alkali metal carbonates, alkaline earth metal carbonates, boric acid, rare earth oxides, tin oxide, and other oxides. The preparation method includes: S1, weighing the raw material powders (excluding rare earth oxides, tin oxide, and other oxides) according to the specified ratio and mixing them thoroughly; S2, melting the mixed powders at high temperature to form a glass melt; S3, water quenching; S4, preparing glass powder; S5, weighing the glass powder, rare earth oxides, tin oxide, and the other oxides according to the specified ratio and grinding them together to obtain glaze powder; S6, preparing glaze slurry; S7, glazing and firing. The glaze obtained by this invention achieves the effects of matching thermal expansion with titanium metal / titanium alloys, strong titanium-ceramic bonding, excellent resistance to thermal shock, lower firing temperature, and significantly improved oxidation resistance of titanium metal / titanium alloys after glazing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of inorganic non-metallic glazes, enamels, and enamel materials. It relates to a special glaze for titanium metal and titanium alloys containing rare earth oxides and its preparation method. It is particularly suitable as a protective, anti-oxidation, and decorative glaze for the surface of titanium metal and titanium alloy materials such as pure titanium, TA1, TA2, and TC4. It can be applied to the glazing of titanium-based industrial anti-corrosion components, titanium-based aerospace materials, titanium-based marine equipment, titanium-based handicrafts, titanium-based kitchenware, and titanium-based dental restorations. Background Technology

[0002] In aerospace and high-temperature environments, titanium and titanium alloys possess high specific strength, strong erosion resistance, and a weight significantly lower than alloy steel. They also exhibit good medium-temperature resistance; below 500℃, their strength, stiffness, creep resistance, and dimensional stability far surpass those of other alloy materials. However, their oxidation resistance at high temperatures is poor. Without protection, in air above 500℃, the surface of titanium-based materials rapidly oxidizes, forming a porous TiO2 oxide layer. This TiO2 oxide layer is easily peeled off, creating a new oxide layer. Therefore, the upper limit of the long-term operating temperature for titanium and titanium alloys is only around 500℃. For long-term use in higher temperature environments, a glaze must be sprayed onto the surface to isolate it from the air and prevent oxidation.

[0003] In the fields of fine chemicals, biomedicine, new energy, and semiconductor electronics, titanium metal and titanium alloys are widely used to store highly corrosive media due to their advantages such as resistance to chloride ion corrosion, resistance to strong oxidizing acids, non-toxicity, cleanliness, and high specific strength. These materials are used in the production of storage tanks for organic acids, inorganic acids, hydrogen peroxide, lithium hexafluorophosphate electrolyte, and lithium salt solutions; or in reaction vessels and receiving tanks for the production of chemical fibers, dyes, and pharmaceutical intermediates. However, prolonged use in such strong acid and oxidizing media will cause titanium metal to slowly corrode and deteriorate. Therefore, applying a glaze to the surface of titanium-based storage tanks and reaction vessels will significantly improve their durability.

[0004] In marine engineering, offshore oil platforms, and seawater desalination, titanium is one of the few metals that can withstand seawater corrosion for extended periods, with a lifespan far exceeding that of carbon steel and stainless steel. Therefore, it is widely used in seawater pretreatment tanks, concentrated brine storage tanks, seawater ballast tanks, oil and gas associated chemical storage tanks, and deep-sea mining corrosive media storage tanks. However, titanium-based devices are subjected to long-term seawater erosion in the marine environment, causing the titanium metal to corrode, thin, and eventually fail. Therefore, applying a glaze to the surface of titanium-based devices can significantly improve their corrosion and erosion resistance, thereby extending their service life.

[0005] In other fields, such as nuclear power, environmental protection, hydrometallurgy, and cryogenic and ultra-low temperature applications, titanium-based devices and titanium-based storage tanks are also widely used. If a layer of glaze can be sprayed on their surface, their durability will be greatly improved.

[0006] However, existing traditional glazes have the following prominent drawbacks when directly applied to titanium-based materials: 1. Mismatch in thermal expansion coefficients: The thermal expansion coefficients of conventional glazes and titanium-based materials differ greatly, making it easy for problems such as chipping, cracking, peeling, and coating detachment to occur during the glazing process; 2. Low bonding strength between titanium metal and ceramic: During high-temperature firing, the glaze components are prone to violent interfacial reactions with the titanium matrix, generating a large amount of brittle TiO2 reaction layer, which significantly reduces the bonding strength between titanium metal and ceramic. During use, the glaze layer is very easy to peel off from the surface of the titanium-based material. 3. Poor thermal shock resistance: Existing glazes are prone to cracking and chipping when the temperature fluctuates drastically, which damages the coating structure.

[0007] Therefore, if a special glaze can be developed that matches the thermal expansion of titanium / titanium alloy, has strong titanium-ceramic bonding, excellent resistance to thermal shock, and a low firing temperature, it would have very important engineering application value for fields that require the use of titanium / titanium alloy. Summary of the Invention

[0008] To overcome the above problems, this invention provides a special glaze for titanium metal and titanium alloy containing rare earth oxides, which has good thermal expansion matching with titanium metal / titanium alloy, strong titanium metal-ceramic bonding, excellent resistance to thermal shock, and low firing temperature, as well as its preparation method.

[0009] The technical solution adopted by this invention to solve the problems of the prior art is: A method for preparing a special glaze for titanium metal and titanium alloys containing rare earth oxides, wherein the glaze is essentially a feldspar glaze containing rare earth oxides (one or more of cerium oxide (CeO2), lanthanum oxide (La2O3), and yttrium oxide (Y2O3), tin oxide (SnO2), and other oxides (one or more of zirconium oxide (ZrO2) and titanium oxide (TiO2)). The raw materials for preparing the glaze, by weight, include: 35-45 parts potassium feldspar, 25-35 parts quartz sand, and aluminum hydroxide (Al(OH)3). 1-5 parts of alkali metal carbonate, 13-20 parts of alkali metal carbonate, wherein the alkali metal carbonate is one or more of sodium carbonate (Na₂CO₃), potassium carbonate (K₂CO₃), and lithium carbonate (Li₂CO₃); 2-8 parts of alkaline earth metal carbonate, wherein the alkaline earth metal carbonate is one or more of calcium carbonate (CaCO₃), barium carbonate (BaCO₃), and strontium carbonate (SrCO₃); 1-4 parts of boric acid; 3-15 parts of rare earth oxide, wherein the rare earth oxide is one or more of cerium oxide (CeO₂), lanthanum oxide (La₂O₃), and yttrium oxide (Y₂O₃); 0.1-2 parts of tin oxide (SnO₂); and 3-15 parts of other oxides, wherein the other oxides are one or more of zirconium oxide (ZrO₂) and titanium oxide (TiO₂); the preparation method of the glaze mainly includes the following steps: S1. Ingredient mixing: Weigh the raw material powders of each component except the rare earth oxides, tin oxides and other oxides according to the proportions, and put them into the mixer to mix thoroughly. S2. High-Temperature Melting: Place the mixed powder in a refractory crucible and heat to 1350–1450℃, holding for 60–120 minutes until the material is completely melted, forming a homogeneous glass melt. The reason for choosing 1350–1450℃ for 60–120 minutes is to ensure complete melting, the absence of raw material particles, and that the molten material can flow freely from the refractory crucible without abnormal crystallization or the risk of crucible detachment. If the temperature is too low, the material will not melt completely, potentially resulting in raw material particles, and the molten material may not be able to flow out of the refractory crucible. Conversely, if the temperature is too high, crystallization will occur, and the corrosion of the refractory crucible by the material will be exacerbated, leading to fluctuations in the chemical composition of the glass melt and consequently affecting the physical properties of the glaze.

[0010] S3, Water Quenching: Quickly immerse the molten glass in water for water quenching to obtain a glass ingot. Deionized water is preferred here; tap water, mineral water, or other contaminated water is not recommended. This is because tap water or mineral water contains small amounts of dissolved cations such as calcium, magnesium, sodium, and potassium, as well as anions such as chloride, carbonate, sulfate, and nitrate, which together constitute the total hardness. These inorganic salts enter the material after the glass ingot is dried, and their main effects include: (1) affecting the melting point of the glaze; (2) affecting the linear expansion coefficient of the glaze; (3) carbonates, nitrates, and sulfates release gases such as carbon oxides, nitrogen oxides, and sulfur oxides during glazing, generating bubbles and reducing the bonding strength between titanium and porcelain and the strength of the glaze itself. Moreover, tap water may also carry rust from the water pipes, affecting the color and melting point of the glaze. In addition to the above impurities, other unclean water may also carry organic matter. During glazing, organic matter oxidizes to generate carbon oxide gas. If the oxidation is insufficient to form carbon black, it will affect the color and strength of the glaze layer.

[0011] S4. Making glass powder: Crush and grind the dried glass frit to make glass powder; S5. Glaze powder preparation: Weigh the raw material powders of glass powder, rare earth oxide, tin oxide and other oxides according to the formula, grind the glass powder together with the rare earth oxide, tin oxide and other oxides, and control the preset particle size to produce glaze powder; preferably, the preset particle size is D50 3~10μm, D90 <30μm.

[0012] S6. Glaze Slurry Preparation: The glaze powder is stirred evenly with a mixing liquid to obtain a glaze slurry. The mixing liquid is one or more of water, propylene glycol, and butylene glycol. Glaze slurries prepared with water require a longer natural drying time after application. Glaze slurries prepared with propylene glycol and butylene glycol have a shorter natural drying time due to the higher volatility of the alcohol; however, for safety reasons, large-scale use in enclosed spaces is not recommended. As mentioned above, deionized water is preferred; tap water, mineral water, or other contaminated water is not recommended. If colored glaze is required, preferably, ceramic pigment is added to the glaze powder after preparation and before glaze slurry preparation, and mixed evenly to obtain colored glaze powder. During slurry preparation, the colored glaze powder is stirred evenly with the mixing liquid to obtain the glaze slurry.

[0013] S7. Glazing and firing: Titanium-based material pretreatment: The titanium-based material is degreased and sandblasted. During sandblasting, a large number of sparks should be avoided, otherwise it will lead to titanium oxidation. Then, the glazed surface of the titanium-based material is cleaned with alcohol or deionized water. Tap water and mineral water should not be used here, because impurities in tap water and mineral water will adhere to the surface of the titanium-based material, thus affecting the bonding strength between titanium and ceramic. Glazing is applied to the surface of titanium-based materials using spraying / dipping methods; After thorough drying, fire at 700–800℃ for 5–30 minutes under vacuum or a weak oxidizing atmosphere; then allow the furnace to cool naturally. Controlling the glazing process at a low temperature under vacuum or a weak oxidizing atmosphere, with a firing temperature of 700–800℃, can reduce surface oxidation of the titanium-based material.

[0014] Preferably, the potassium feldspar is potassium feldspar with a K2O content of 9% to 13%.

[0015] The present invention also discloses a special glaze for titanium metal and titanium alloy containing rare earth oxides, which is prepared by the above preparation method.

[0016] In this glaze, appropriate amounts of alkali metal oxides K2O, Na2O, and Li2O are introduced through potassium feldspar, potassium carbonate K2CO3, sodium carbonate Na2CO3, and lithium carbonate Li2CO3. During step "S2, high-temperature melting," sodium carbonate Na2CO3, potassium carbonate K2CO3, and lithium carbonate Li2CO3 decompose, generating Na2O, K2O, Li2O, and CO2 gas. The CO2 gas is discharged from the melt, leaving Na2O, K2O, and Li2O to react with other components such as potassium feldspar and quartz sand to form a glass melt. The beneficial effect of alkali metal oxides K2O, Na2O, and Li2O in this glaze is that they act as strong fluxes, significantly reducing the melting temperature and viscosity of the mixed powders, making it easier to melt the mixed powders into a homogeneous glass melt. However, Na₂O, K₂O, and Li₂O each play different roles: Na₂O has a strong fluxing ability, which can significantly reduce the melting temperature and the viscosity of the melt, and significantly increase the coefficient of thermal expansion; K₂O is also a flux, but its fluxing ability is slightly weaker than that of Na₂O, and its increase in the coefficient of thermal expansion is also less than that of Na₂O; Li₂O has the strongest fluxing ability, and a small amount can significantly reduce the melting temperature, and an appropriate amount can reduce the coefficient of thermal expansion. Therefore, in step "S1, ingredient mixing", this invention incorporates potassium feldspar and alkali metal carbonates (one or more of potassium carbonate K₂CO₃, sodium carbonate Na₂CO₃, and lithium carbonate Li₂CO₃), and by controlling the total alkali content in the glaze (the sum of K₂O, Na₂O, and Li₂O) and adjusting the ratio between K₂O, Na₂O, and Li₂O, the mixed alkali effect is used to balance the melting performance of the glass phase and effectively adjust the coefficient of thermal expansion of the glaze, thereby achieving the purpose of matching different grades of titanium metal and titanium alloys.

[0017] In this glaze, B2O3 is introduced by adding boric acid (H3BO3). During step "S2, high-temperature melting," boric acid (H3BO3) decomposes, generating B2O3 and H2O gas. The H2O gas is expelled from the melt, leaving B2O3 to react with other components such as potassium feldspar and quartz sand to form a glass melt. The beneficial role of B2O3 in this glaze is that it acts as a glass network former, significantly reducing the melting temperature and viscosity of the glass melt, making it easier for the mixed powders to melt into a homogeneous glass phase. An appropriate amount of B2O3 can also reduce the coefficient of thermal expansion of the glaze, improve its wetting properties, and allow it to spread more easily on the surface of the titanium-based material during sintering, which is beneficial for interfacial bonding and thus enhances the bonding strength between titanium metal and ceramic.

[0018] Specifically, in this glaze, by controlling the total alkali content (the sum of K2O, Na2O, and Li2O), the alkali metal composition ratio (the proportion between K2O, Na2O, and Li2O), and the B2O3 content, the sintering temperature and coefficient of thermal expansion of the glaze can be flexibly adjusted according to the titanium-based material to be glazed, so as to match the glaze with the titanium-based material to be glazed. The coefficient of linear expansion of different grades of titanium metal / titanium alloy from room temperature to 500℃ is typically 9.2~10.5×10. -6 / K. In this invention, the specific control mechanism of the sintering temperature and thermal expansion coefficient of the glaze is as follows: (1) Total alkali content is a primary regulator. K2O, Na2O, and Li2O can significantly disrupt the silicon-oxygen network in the glass phase. Increasing the total alkali content will exacerbate the breaking of Si-O bonds in the silicon-oxygen network, making the silicon-oxygen network loose and weakening the interatomic bonding force. Macroscopically, this manifests as a decrease in the melting point and viscosity of the glass melt. At the same time, alkali metal cations (K2O, Na2O, and Li2O) can also cause the silicon-oxygen network to become loose and the interatomic bonding force to weaken. + Na + Li + Located in the gaps of the silicon-oxygen network, the silicon-oxygen framework becomes loose due to the breakage of Si-O bonds after heating, making it easier to expand, resulting in an increase in volume and macroscopically manifested as an increase in the coefficient of thermal expansion.

[0019] (2) When the total alkali content remains constant, adjusting the relative proportions of K2O, Na2O, and Li2O can achieve secondary fine-tuning of the glass phase melting temperature and thermal expansion coefficient: This is influenced by the cation radius Li... + <Na + <K + The K₂O, Na₂O, and Li₂O components exhibit certain differences in their effects on the glass phase melting temperature and thermal expansion. This glaze uses potassium feldspar as its base material; in this system, Li… + With the smallest radius and highest electric field strength, Li₂O has the strongest ability to disrupt the silicon-oxygen network, thus exhibiting the strongest fluxing power. Even a small amount added can significantly lower the melting temperature of the glass phase. However, Li… + Due to its strong electric field and small radius, it is easier for it to enter the Si-O network for coordination, thus contributing the least to the coefficient of thermal expansion; adding a small amount may even lower the overall coefficient of thermal expansion. Compared with Li... + Correspondingly, Na + It also has a strong ability to disrupt silicon-oxygen networks, but Na + With a large radius, it cannot enter the Si-O network for coordination, resulting in a more relaxed non-bridged Si-O structure, which significantly increases the coefficient of thermal expansion; K + Although it has the largest radius, its entry into the voids of the non-bridged Si-O structure network actually provides some "support" to the structure, resulting in its contribution to the coefficient of thermal expansion being smaller than that of Na. + .

[0020] (3) B2O3, as a network former, works synergistically with alkali metal ions, exhibiting a "boron anomalous" phenomenon in its effect on the coefficient of thermal expansion. That is, in this glaze system, due to the presence of a large amount of alkali metal ions, boron-oxygen trigonometric bodies will transform into boron-oxygen tetrahedra and participate in the construction of the glass network. When the B2O3 content is low and the alkali metal ions are excessive, as the B2O3 content increases, the proportion of boron-oxygen tetrahedra increases, the glass phase network tends to be denser, and the coefficient of thermal expansion tends to decrease. Therefore, in this glaze system, an appropriate amount of B2O3 can reduce the coefficient of thermal expansion of the glaze.

[0021] In summary, in this glaze system, the total alkali content (the sum of K2O, Na2O, and Li2O) is controlled first to reduce the melting temperature of the glass phase and obtain a suitable coefficient of thermal expansion. Then, the alkali metal composition ratio (the ratio between K2O, Na2O, and Li2O) is optimized to further fine-tune the melting temperature and coefficient of thermal expansion. Finally, by introducing B2O3, the melting characteristics and thermal expansion value of the glass phase are synergistically optimized. At the same time, the superimposed effects of rare earth oxides, tin oxide, and other oxides in step "S5, glaze powder preparation" are taken into account. The overall sintering temperature and coefficient of thermal expansion of the glaze can be precisely controlled according to the performance requirements of the titanium-based material to be coated, so as to match the thermal expansion properties of different grades of titanium metal and titanium alloy.

[0022] In this glaze, appropriate amounts of alkaline earth metal oxides CaO, BaO, and SrO are introduced through calcium carbonate (CaCO3), barium carbonate (BaCO3), and strontium carbonate (SrCO3). This is because these oxides decompose during step "S2, high-temperature melting," generating CaO, BaO, SrO, and CO2 gas. The CO2 gas is expelled from the melt, leaving CaO, BaO, and SrO to react with other components such as potassium feldspar and quartz sand to form a glass melt. The beneficial effects of the alkaline earth metal oxides (CaO, BaO, SrO) in this glaze are to regulate its melting point and viscosity, enhance its chemical stability, and improve its strength. BaO also enhances its resistance to acid and alkali corrosion, while SrO inhibits feldspar crystallization, thereby significantly improving the chemical stability of the glaze.

[0023] In this glaze, Al2O3 is introduced through potassium feldspar and aluminum hydroxide (Al(OH)3). The introduction of Al2O3 via aluminum hydroxide (Al(OH)3) is due to the decomposition of aluminum hydroxide during step "S2, high-temperature melting," generating Al2O3 and H2O gas. The H2O gas is expelled from the melt, leaving Al2O3 to react with potassium feldspar, quartz sand, and other components to form a glass melt. The beneficial role of Al2O3 in this glaze is to improve the integrity of the glass network, thus enhancing the structural strength of the glaze and significantly improving its chemical stability and corrosion resistance.

[0024] In addition to the above, the present invention also has the following technical innovations: I. In this glaze, rare earth oxides, B2O3, and SnO2 significantly improve the bonding strength between titanium metal and ceramics. However, under vacuum or weak oxidizing atmosphere firing conditions, SnO2... 4+ Will be restored to Sn 2+ This will cause the glaze to turn gray or black. At the same time, the released oxygen will increase the risk of titanium metal oxidation, so the amount added should not be too large.

[0025] II. The rare earth oxides (one or more of cerium oxide CeO2, lanthanum oxide La2O3 and yttrium oxide Y2O3), tin oxide SnO2 and other oxides (one or more of zirconium oxide ZrO2 and titanium oxide TiO2) in this invention are added in the form of oxides, which can produce four beneficial effects: (1) greatly improve the bonding strength between titanium metal and ceramic; (2) effectively release thermal stress, greatly improve the thermal shock resistance of the glaze layer, and improve the thermal shock resistance; (3) greatly improve the strength of the glaze body, and improve the erosion resistance and wear resistance of the glaze layer; (4) adjust the coefficient of thermal expansion and accurately match the thermal expansion properties of titanium metal and titanium alloy such as TA1, TA2, and TC4.

[0026] The specific principle is as follows: 1. The addition of rare earth oxides in this invention can reduce the TiO2 oxide layer at the titanium-ceramic interface.

[0027] Titanium is readily oxidized to form a porous TiO2 oxide layer, which is easily peeled off. Ordinary glazes struggle to dissolve, break down, or penetrate the TiO2 oxide layer to directly wet the titanium substrate, resulting in poor adhesion between the glaze and the titanium matrix – a primary cause of titanium-based glaze peeling. Rare earth elements, with their higher affinity for oxygen, can preferentially capture free oxygen at the titanium-ceramic interface, inhibiting continuous oxygen diffusion to the titanium substrate surface. This inevitably reduces the thickness and extent of the oxide layer on the titanium surface, allowing the glaze melt more opportunities to directly contact the titanium matrix, thereby improving glaze adhesion and the bonding strength between titanium and ceramic.

[0028] 2. This invention adds rare earth oxides. Rare earth elements are surface-active components, which can improve the surface activity of the glaze. During glazing, they can reduce the interfacial energy between the melt and titanium metal, reduce the wetting contact angle, promote the spread of the glaze melt on the titanium surface, and improve the bonding strength between titanium and ceramic.

[0029] 3. The glaze of this invention contains B2O3. During glazing, B2O3 has a certain destructive and dissolving effect on the TiO2 oxide film on the titanium surface. It can locally destroy the TiO2 oxide layer, allowing the glaze melt to have more opportunities to directly contact the titanium body, thereby promoting the bonding between the glaze and the titanium body and improving the adhesion of the glaze.

[0030] 4. The glaze of this invention contains rare earth oxides, B2O3 and SnO2, which can react chemically with the titanium interface to generate a composite transition phase, build chemical bonds, and greatly improve the bonding strength between titanium and ceramic.

[0031] During the high-temperature glazing process, rare earth oxides, B2O3, and SnO2 in the glaze react chemically with titanium to generate Ti-rare earth-oxygen composite transition phase, titanium-boron alloy phase TiB / TiB2, and Ti-Sn-O composite oxide phase. This continuous, thin composite phase transition layer acts as a "bridging" layer for chemical bonds, reducing interfacial energy and improving the spreading performance of the glaze on the titanium surface on the one hand; and establishing a strong metallurgical bond on the other hand, enhancing interfacial bonding strength.

[0032] In this glaze system, B2O3, rare earth oxides, and SnO2 play a synergistic regulatory role in the interfacial reaction, jointly promoting the reaction of rare earth elements, B elements, and Sn elements with titanium at the interface to form Ti-B, Ti-rare earth-O, and Ti-Sn-O transition phases, constructing chemical bonds, which are embedded between the glaze layer and the titanium matrix like nails, thereby improving the toughness and bonding strength of the titanium-ceramic interface.

[0033] 5. It forms a diffuse toughening effect, eliminates thermal stress, and improves thermal shock resistance.

[0034] Rare earth oxides, zirconium oxide (ZrO2), and titanium dioxide (TiO2) exhibit high chemical stability and low reactivity. Added in oxide form, they do not chemically react with the glassy phase of the glaze during firing. This is equivalent to introducing dispersed second-phase solid particles into the brittle glassy matrix, creating a dispersion-based toughening effect, eliminating thermal stress, and improving the glaze's thermal shock resistance. The specific mechanism is as follows: Temperature changes generate thermal stress in the glass phase of the glaze. When the thermal stress reaches a critical value, cracks will appear. The cracks continue to spread, grow, connect, and penetrate, eventually leading to cracking and peeling of the glaze, which macroscopically manifests as poor thermal shock resistance.

[0035] In this invention, glass powder and oxides are ground together, and these oxides are dispersed in the glass phase in large quantities. This is equivalent to introducing a dispersed second phase into the brittle glass phase matrix. When the crack extends to the solid particles of the second phase, it will be deflected, bridged or pinned, which prolongs the crack propagation path and consumes more energy, thereby preventing crack propagation and growth, reducing the risk of glaze cracking and peeling, and macroscopically manifesting as good thermal shock resistance.

[0036] The main toughening mechanism is achieved through the following methods: (1) Crack deflection and bridging: The crack is blocked by the second phase oxide particles with high hardness and high elastic modulus, and it needs to detour to propagate. This prolongs the propagation path, consumes more energy, and can reduce the crack from continuing to grow.

[0037] (2) Pinning and line tension: When a crack in the glass phase extends to a solid particle, the solid particle pins the crack tip, causing it to bend. The crack requires more additional energy to pass through the particle, which in turn prevents the crack from extending.

[0038] (3) Residual stress field: The thermal expansion coefficients of the glass phase matrix and oxide particles are quite different. This mismatch in thermal expansion coefficients will generate a residual stress field, which can hinder the generation and propagation of cracks.

[0039] (4) Suppressing crack growth: A large number of dispersed second phase particles can effectively suppress crack propagation and growth. The smaller the particle spacing, the smaller the crack can be controlled within a smaller range, and the more obvious the toughening effect is. Macroscopically, this manifests as stronger thermal shock resistance.

[0040] 6. The reinforcement of the second-phase solid particles can improve the hardness and strength of the glaze layer.

[0041] High-hardness, high-elasticity rare earth oxides, ZrO2, TiO2, SnO2 and other solid particles are uniformly dispersed in the glass continuous phase, playing a supporting role in the skeleton. During the glazing process, the glass phase and oxide particles interlock with each other due to sintering, forming a strong bonding force, which can greatly improve the overall strength and hardness of the glaze.

[0042] 7. Fine-tune the coefficient of thermal expansion to improve the stress state at the titanium-ceramic interface.

[0043] Rare earth oxides, ZrO2, TiO2, and SnO2 have different coefficients of thermal expansion, which also differ significantly from those of the glass phase. By adding them in different proportions, the overall coefficient of thermal expansion of the glaze can be precisely controlled. By matching different grades of titanium metal and titanium alloys, the difference in thermal expansion between the glaze and the titanium matrix can be reduced, the interfacial thermal stress during heating and cooling can be reduced, the cracking and peeling of the glaze layer due to thermal stress can be reduced, and the thermal shock resistance and peeling resistance of the glaze layer can be improved.

[0044] The beneficial effects of this invention are: This invention discloses a method for preparing a special glaze for titanium metal and titanium alloys containing rare earth oxides. The process is ingenious, simple, and controllable. The resulting glaze achieves optimal thermal expansion matching with titanium metal / titanium alloys, strong titanium-ceramic bonding, excellent resistance to thermal shock, and a relatively low firing temperature. It is particularly advantageous due to its strong practicality and is worthy of widespread application. 1. By adding rare earth elements, the oxidation of titanium metal during the glazing process can be effectively inhibited and the formation of TiO2 reaction layer at the interface can be controlled, resulting in a strong titanium-ceramic bond. 2. By combining rare earth elements with B2O3, the surface activity of the glaze can be improved, the TiO2 oxide film can be destroyed and dissolved, the wettability of the glaze on the titanium-based material during firing can be improved, and the bonding strength between titanium and ceramic can be increased. 3. By combining rare earth elements with B2O3 and SnO2, a composite transition phase can be generated through a chemical reaction with the titanium interface, forming a chemical bond and improving the bonding strength between titanium and ceramic. 4. By combining the glass phase with rare earth oxides, ZrO2, TiO2, and SnO2 solid particles, a dispersion toughening effect is formed, which eliminates thermal stress and improves thermal shock resistance, making the glaze layer less prone to cracking and peeling when subjected to thermal shock. 5. By adding second-phase rare earth oxides, ZrO2, and TiO2 solid particles to the glass phase, a skeletal support can be provided; during the glazing process, the glass phase and oxide particles interlock with each other due to sintering, thus improving the hardness and strength of the glaze layer. 6. By combining the glass phase with different proportions of rare earth oxides, ZrO2, TiO2, and SnO2 solid particles, the thermal expansion coefficient of the glaze can be precisely controlled to match the thermal expansion properties of different grades of titanium metal and titanium alloys, thereby reducing thermal stress and improving thermal shock resistance. 7. By using deionized water to quench the glass frit and prepare the glaze slurry, the influence of dissolved substances in water on the physical and chemical properties of the glaze can be eliminated; 8. Avoid generating a lot of sparks when sandblasting and polishing the titanium substrate before glazing to prevent titanium oxidation; use alcohol or deionized water to clean the glazed surface of the titanium-based material to reduce contamination of the glazed surface. 9. By firing the glaze at 700–800°C in a vacuum or weak oxidizing atmosphere, the oxidation of the surface of titanium-based materials can be reduced; 10. By applying glaze to the surface of titanium-based materials, air can be effectively isolated, thereby improving the oxidation resistance of titanium-based materials in high-temperature air. Attached Figure Description

[0045] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein: Figure 1 This is a schematic flowchart of the preparation method of titanium metal and titanium alloy special glaze according to an embodiment of the present invention; Figure 2 Images of specimens used to test the bonding strength between titanium and ceramic; Figure 3 Images of the sample after glaze removal; Figure 4 Images of samples used to measure antioxidant properties. Detailed Implementation

[0046] All features disclosed in this specification, or all steps in all disclosed methods or processes, may be combined in any way, except for mutually exclusive features and / or steps.

[0047] Any feature disclosed in this specification (including any appended claims, abstract, and drawings) may be replaced by other equivalent or similar features for a similar purpose, unless specifically stated otherwise. That is, unless specifically stated otherwise, each feature is merely one example of a series of equivalent or similar features.

[0048] As shown below, a method for preparing a special glaze for titanium metal and titanium alloys containing rare earth oxides, wherein the raw materials for preparing the glaze, by weight, include: 35-45 parts potassium feldspar, 25-35 parts quartz sand, 1-5 parts aluminum hydroxide Al(OH)3, 13-20 parts alkali metal carbonate, wherein the alkali metal carbonate is one or more of sodium carbonate Na2CO3, potassium carbonate K2CO3, and lithium carbonate Li2CO3, 2-8 parts alkaline earth metal carbonate, wherein the alkaline earth metal carbonate is one or more of calcium carbonate CaCO3, barium carbonate BaCO3, and strontium carbonate SrCO3, 1-4 parts boric acid, 3-15 parts rare earth oxides, wherein the rare earth oxides are one or more of cerium oxide CeO2, lanthanum oxide La2O3, and yttrium oxide Y2O3, and tin oxide SnO2. 0.1 to 2 parts, and other oxides 3 to 15 parts, wherein the other oxides are one or more of zirconium oxide (ZrO2) and titanium dioxide (TiO2); the preparation method of the glaze mainly includes the following steps: S1. Ingredient mixing: Weigh the raw material powders of each component except the rare earth oxides, tin oxides and other oxides according to the proportions, and put them into the mixer to mix thoroughly. S2. High-temperature melting: Place the mixed powder in a refractory crucible, heat it to 1350-1450℃ and hold it for 60-120 minutes until the material is completely melted to form a homogeneous glass melt. S3, Water quenching: The molten glass is rapidly immersed in deionized water for water quenching to obtain glass frit; S4. Making glass powder: Crush and grind the dried glass frit to make glass powder; S5. Glaze powder preparation: Weigh the raw material powders of glass powder, rare earth oxide, tin oxide and other oxides according to the formula, grind the glass powder together with the rare earth oxide, tin oxide and other oxides, and control the preset particle size to produce glaze powder. The preset particle size is D50 3~10μm and D90 <30μm.

[0049] S6. Glaze Slurry Preparation: The glaze powder and the mixing liquid are stirred evenly to obtain the glaze slurry. The mixing liquid is one or more of deionized water, propylene glycol, and butylene glycol. If it is necessary to prepare colored glaze, preferably, ceramic pigments are added to the glaze powder after preparation and before glaze slurry preparation, and mixed evenly to obtain colored glaze powder. During slurry preparation, the colored glaze powder is stirred evenly with the mixing liquid to obtain the glaze slurry.

[0050] S7. Glazing and firing: Titanium-based material pretreatment: The titanium-based material is degreased and sandblasted, and excessive sparks should be avoided during sandblasting; then the glazed surface of the titanium-based material is cleaned with alcohol or deionized water. Glazing is applied to the surface of titanium-based materials using spraying / dipping methods; After thorough drying, fire at 700–800℃ for 5–30 minutes under vacuum or a weak oxidizing atmosphere; then allow to cool naturally in the furnace.

[0051] The potassium feldspar is potassium feldspar with a K2O content of 9% to 13%. Example

[0052] A special glaze for titanium metal and titanium alloys containing rare earth oxides is prepared according to steps S1-S7, as follows: S1 Ingredient Mixing: Weigh the following by weight: 40 parts potassium feldspar, 32 parts quartz sand, 3 parts aluminum hydroxide, 12 parts sodium carbonate, 3 parts potassium carbonate, 2.5 parts lithium carbonate, 3 parts calcium carbonate, 0.5 parts strontium carbonate, and 3 parts boric acid; add the prepared materials to a mixer and mix thoroughly. The potassium feldspar is potassium feldspar with a K2O content of 10.6%.

[0053] Glass powder is obtained through steps S2, S3, and S4.

[0054] S5 Glaze Powder: Weigh 100 parts glass powder, 10 parts CeO2, 1 part SnO2, 5 parts TiO2, and 5 parts ZrO2 by weight, and grind them together to obtain glaze powder. The particle size of the glaze powder is D50 7μm and D90 28μm.

[0055] The glaze slurry is prepared through step S6.

[0056] The S7 step involves glazing and firing: glazes are applied to titanium-based materials of grades TA2 and TC4 respectively, and after drying, they are placed in an atmosphere furnace. Argon is used to replace the air, and the oxygen partial pressure is controlled to be less than 0.1 Pa to create a weak oxidizing environment. The glazing temperature is 760℃. Example

[0057] A special glaze for titanium metal and titanium alloys containing rare earth oxides is prepared according to the glaze preparation steps S1-S7, as follows: S1 Ingredient Mixing: Weigh the following by weight: 40 parts potassium feldspar, 32 parts quartz sand, 3 parts aluminum hydroxide, 15 parts sodium carbonate, 5 parts potassium carbonate, 2.5 parts calcium carbonate, 1.5 parts barium carbonate, 0.5 parts strontium carbonate, and 3 parts boric acid. The potassium feldspar is potassium feldspar with a K2O content of 9.1%.

[0058] Glass powder is obtained through steps S2, S3, and S4.

[0059] S5 Glaze Powder: Weigh out 100 parts by weight of glass powder, 3 parts by weight of CeO2, 3 parts by weight of La2O3, 6 parts by weight of yttrium oxide (Y2O3), 0.5 parts by weight of SnO2, and 10 parts by weight of ZrO2, and grind them together to obtain glaze powder. The particle size of the glaze powder is D50 6μm and D90 26μm.

[0060] The glaze slurry is prepared through step S6.

[0061] The process involves glazing and firing via step S7: glazing is applied to TC4 titanium alloy and fired under vacuum conditions at a vacuum level of 100 kPa and a firing temperature of 780°C.

[0062] Comparative Example Comparative Example 1-1 (Example 1 without rare earth oxides, tin oxide and other oxides): The glass powder obtained in steps S1 to S4 of Example 1 was directly ground to a particle size of D50 7 μm and D90 28 μm. A glaze slurry was prepared in step S6. Glazing and firing were then carried out in step S7: the glaze was applied to a titanium-based material of grade TA2, dried, and placed in an atmosphere furnace. Air was replaced with argon gas to control the oxygen partial pressure to less than 0.1 Pa, creating a weakly oxidizing environment. The firing temperature was 740℃.

[0063] Comparative Examples 1-2 (Example 1 without tin oxide): Example 1: Glass powder obtained in steps S1 to S4; glaze powder preparation in step S5: Weigh 100 parts of glass powder, add 10 parts of CeO2, 5 parts of TiO2, and 5 parts of ZrO2, and grind them together to obtain glaze powder with a particle size of D50 7μm and D90 28μm. Glaze slurry is obtained in step S6. Glazing and firing are carried out in step S7: Glaze is applied to titanium-based material of grade TA2, dried, and placed in an atmosphere furnace. The air is replaced with argon gas to control the oxygen partial pressure to be less than 0.1 Pa, creating a weak oxidizing environment. The glaze firing temperature is 760℃.

[0064] Comparative Examples 1-3 (Example 1 without the addition of other oxides): Example 1: Glass powder obtained in steps S1 to S4; glaze powder preparation in step S5: Weigh 100 parts of glass powder, add 10 parts of CeO2 and 1 part of SnO2, and grind them together to obtain glaze powder with a particle size of D50 7μm and D90 28μm. Glaze slurry is obtained in step S6. Glazing and firing are carried out in step S7: Glaze is applied to titanium-based material of grade TA2, dried, and placed in an atmosphere furnace. The air is replaced with argon gas to control the oxygen partial pressure to be less than 0.1 Pa, creating a weak oxidizing environment. The glazing temperature is 760℃.

[0065] Comparative Examples 1-4 (The amount of rare earth oxide CeO2 added in Example 1 was increased from 10 parts to 20 parts): Example 1: Glass powder obtained in steps S1 to S4; glaze powder preparation in step S5: Weigh 100 parts of glass powder, add 20 parts of CeO2, 1 part of SnO2, 5 parts of TiO2, and 5 parts of ZrO2, and grind them together to obtain glaze powder with a particle size of D50 7μm and D90 28μm. Glaze slurry is obtained in step S6. Glazing and firing are carried out in step S7: Glaze is applied to titanium-based material of grade TA2, dried, and placed in an atmosphere furnace. The air is replaced with argon gas to control the oxygen partial pressure to be less than 0.1 Pa, creating a weak oxidizing environment. The glazing temperature is 770℃.

[0066] Comparative Example 2 (Example 2 without rare earth oxides, tin oxide and other oxides): In Example 2, the glass powder obtained in steps S1 to S4 was directly ground to a particle size of D50 6 μm and D90 26 μm. A glaze slurry was prepared in step S6. Glazing and firing were then carried out in step S7: the glaze was applied to TC4 titanium alloy and fired under vacuum at a vacuum degree of 100 kPa and a firing temperature of 760°C.

[0067] Performance verification The physical properties of the glaze powder and glazed titanium sheets prepared in the examples and comparative examples were tested, including the coefficient of linear expansion, flexural strength, titanium-ceramic bonding strength, thermal shock resistance, and oxidation resistance, as detailed below: Sample preparation and experimental methods were performed in accordance with YY 0621-2025 "Test for compatibility of dental metal-ceramic and ceramic-ceramic systems" and GB 30367-2025 "Ceramic materials in dentistry".

[0068] The performance comparison is as follows: 1. Linear expansion coefficient, flexural strength, and titanium-ceramic bond strength properties

[0069] Therefore, it can be seen that: (1) Comparing Comparative Example 1-1 and Comparative Example 2, Comparative Example 1-1 added 2.5 parts of lithium carbonate and 15 parts of sodium carbonate and potassium carbonate, while Comparative Example 2 did not have lithium carbonate and had 20 parts of sodium carbonate and potassium carbonate. The glazing temperature and coefficient of linear expansion of the glass powder were slightly different. The glazing temperature and coefficient of linear expansion of Comparative Example 1-1 with added lithium carbonate were lower, indicating that in this system, adding a small amount of lithium carbonate can significantly reduce the melting temperature of the glass and lower the coefficient of thermal expansion. (2) Comparing Example 1 and Comparative Example 1-1, Example 2 and Comparative Example 2, the addition of rare earth oxides and zirconium oxide ZrO2, titanium oxide TiO2 and tin oxide SnO2 can adjust the linear expansion coefficient of the glaze powder.

[0070] (3) Comparing Example 1 and Comparative Example 1-1, Example 2 and Comparative Example 2, the Example 1 has higher flexural strength and titanium-ceramic bond strength; (4) Comparing Example 1 and Comparative Examples 1-2, the addition of rare earth oxides and tin oxide resulted in a higher bonding strength between titanium and ceramic. (5) Comparing Example 1 and Comparative Examples 1-3, the flexural strength of the glaze was higher after adding other oxides; (6) Comparing Example 1 and Comparative Examples 1-4, the amount of rare earth oxide CeO2 added was increased from 10 parts to 20 parts. The improvement effect on the strength of the glaze itself and the bonding strength between titanium and ceramic was not obvious. However, in terms of raw material price, adding a large amount of rare earth oxide would lead to an increase in the cost of the glaze.

[0071] 2. Thermal shock resistance Samples were prepared according to "6.4.2 Sample Preparation" of YY 0621-2025 "Tests for Compatibility of Metal-Ceramic and Ceramic-Ceramic Systems in Dentistry". The samples were held in a furnace at 300℃ for 30 minutes, then removed and cooled to room temperature in air, constituting one thermal shock. This process was repeated. The strength before and after thermal shock was measured according to "6.4.3 Determination of Fracture Force" of the same standard. The retention rate R of the titanium-ceramic bond strength after thermal shock was calculated. R = (Fracturing strength after thermal shock / Fracturing strength before thermal shock) × 100% The results of thermal shock resistance of Example 1 and Comparative Example 1-1 are as follows:

[0072] It is evident that the thermal shock resistance of the embodiment is significantly improved.

[0073] 3. Antioxidant properties TA2 and TC4 titanium materials were used to prepare thin sheets of approximately 40mm × 40mm × 1mm. These were divided into two groups: one group was unglazed (bare sheets), and the other group was glazed according to Example 1, with a maximum glaze thickness of approximately 0.5mm (glazed sheets). The weights of both groups before firing were measured. They were then placed in an 800℃ furnace and held for 10 hours, followed by natural cooling to room temperature. The weights after firing were measured, and the weight gain per unit area δG was calculated. δG = (Weight after burning (mg) - Weight before burning (mg)) / Area (cm²) 2 / Time: 10 hours.

[0074] The results are as follows:

[0075] Therefore, it can be seen that the weight gain per unit area of ​​the glazed titanium sheet in Example 1 is only 2% to 3.5% of that of the bare sheet during the oxidation resistance test, indicating that the oxidation resistance of the glazed sheet is much greater than that of the bare sheet without glaze protection.

[0076] This invention is not limited to the specific embodiments described above. The invention extends to any new feature or combination disclosed in this specification, as well as any new method or process step or combination disclosed herein.

Claims

1. A method for preparing a special glaze for titanium metal and titanium alloys containing rare earth oxides, characterized in that, The raw materials for preparing the glaze, by weight, include: 35-45 parts potassium feldspar, 25-35 parts quartz sand, 1-5 parts aluminum hydroxide Al(OH)3, 13-20 parts alkali metal carbonate, wherein the alkali metal carbonate is one or more of sodium carbonate Na2CO3, potassium carbonate K2CO3, and lithium carbonate Li2CO3; 2-8 parts alkaline earth metal carbonate, wherein the alkaline earth metal carbonate is one or more of calcium carbonate CaCO3, barium carbonate BaCO3, and strontium carbonate SrCO3; 1-4 parts boric acid; 3-15 parts rare earth oxide, wherein the rare earth oxide is one or more of cerium oxide CeO2, lanthanum oxide La2O3, and yttrium oxide Y2O3; 0.1-2 parts tin oxide SnO2; and 3-15 parts other oxides, wherein the other oxides are one or more of zirconium oxide ZrO2 and titanium oxide TiO2. The preparation method of the glaze mainly includes the following steps: S1. Ingredient mixing: Weigh the raw material powders of each component except the rare earth oxides, tin oxides and other oxides according to the proportions, and put them into the mixer to mix thoroughly. S2. High-temperature melting: Place the mixed powder in a refractory crucible, heat it to 1350-1450℃ and hold it for 60-120 minutes until the material is completely melted to form a homogeneous glass melt. S3, Water quenching: The molten glass is rapidly immersed in water for water quenching to obtain glass frit; S4. Making glass powder: Crush and grind the dried glass frit to make glass powder; S5. Glaze powder preparation: Weigh the raw material powders of glass powder, rare earth oxide, tin oxide and other oxides according to the formula, grind the glass powder together with the rare earth oxide, tin oxide and other oxides, control the preset particle size for discharge, and obtain glaze powder. S6. Preparation of glaze slurry: The glaze powder is mixed with the blending liquid to obtain the glaze slurry. The blending liquid is one or more of water, propylene glycol and butanediol. S7. Glazing and firing: Titanium-based material pretreatment: The titanium-based material is degreased and sandblasted, and then the glazed surface of the titanium-based material is cleaned with alcohol or deionized water; Glazing is applied to the surface of titanium-based materials using spraying / dipping methods; After thorough drying, fire at 700–800℃ for 5–30 minutes under vacuum or a weak oxidizing atmosphere; then allow to cool naturally in the furnace.

2. The preparation method according to claim 1, characterized in that, In step S1, the potassium feldspar is potassium feldspar with a K2O content of 9% to 13%.

3. The preparation method according to claim 1, characterized in that, In step S3, the water used for water quenching is deionized water.

4. The preparation method according to claim 1, characterized in that, In step S5, the particle size of the glaze powder is controlled to be D50 3~10μm and D90 <30μm when the glaze powder is discharged.

5. The preparation method according to claim 1, characterized in that, In step S6, the water used to prepare the glaze slurry is deionized water.

6. The preparation method according to claim 1, characterized in that, If it is necessary to prepare colored glaze, ceramic pigments are added to the glaze powder after it is made and before it is made into glaze slurry. The mixture is stirred evenly to obtain colored glaze powder. When making glaze slurry, the colored glaze powder is stirred evenly with the mixing liquid to obtain glaze slurry.

7. The preparation method according to claim 1, characterized in that, In step S7, when sandblasting and polishing the titanium-based material, a large number of sparks should be avoided.

8. A special glaze for titanium metal and titanium alloys containing rare earth oxides, characterized in that, Prepared by the preparation method according to any one of claims 1-7.