A lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite slurry, its preparation method and application
By using a lead-free barium aluminum borosilicate-zinc borosilicate dual glass powder composite dielectric slurry, combined with TiO2 modification, the crack resistance and density problems of existing glass powder-based lead-free dielectric slurries have been solved, achieving the stable use requirements of high-end thick-film electronic components and showing good industrial application prospects.
Patent Information
- Application Number
- CN202611459350.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-18
- Publication Date
- 2026-11-17
AI Technical Summary
Existing glass powder-based lead-free dielectric slurries cannot simultaneously meet the multiple requirements of crack resistance, high density, and strong adhesion, and therefore cannot meet the needs of high-end thick-film electronic components.
A lead-free barium aluminum borosilicate-zinc borosilicate dual glass powder composite medium slurry is used. By mixing barium aluminum borosilicate glass powder and zinc borosilicate glass powder, and adding an appropriate amount of TiO2, the component ratio and process parameters are optimized to form a highly dense and strong adhesion.
It achieves good crack resistance and high density of the dielectric layer, strong adhesion to alumina substrate, is suitable for high-end thick film electronic components, complies with lead-free environmental protection standards, has good process stability, and is suitable for industrial production.
Smart Images

Figure CN123106003A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electronic paste technology, and in particular to a lead-free barium aluminum borosilicate-zinc borosilicate dual glass powder composite dielectric paste, its preparation method, and its application. Background Technology
[0002] Dielectric pastes are one of the core raw materials for the fabrication of electronic components. Their comprehensive performance directly determines the structural stability, insulation performance, and service life of electronic components, and they are widely used in the dielectric layer fabrication process of various electronic devices. In the field of electronic pastes, glass powder-based dielectric pastes have become the mainstream choice for thick-film dielectric materials due to their advantages such as strong substrate compatibility, controllable preparation costs, and mature sintering processes.
[0003] Currently, most conventional lead-free dielectric slurries based on glass powder in the industry use a single glass system formulation, which makes it difficult to simultaneously achieve sintering density, interfacial adhesion, and thermal expansion matching. This fails to meet the core requirements of high-end thick-film electronic components for high-density, crack-free, and high-adhesion dielectric layers. Specifically, barium aluminum borosilicate (BABS) glass slurries are stable during sintering, form dense films, and have excellent insulation properties, but their high coefficient of thermal expansion results in poor thermal matching with 96% alumina substrates, easily generating thermal stress during sintering and causing film cracking. Even if cracking defects are improved through component control, it will still cause an increase in the glass softening point and induce glaze formation, resulting in a narrowing of the conventional thick-film sintering process window and a deterioration in the interfacial bonding and re-firing stability of multilayer thick films. Zinc borosilicate (ZBS) glass systems have a low coefficient of thermal expansion, which can effectively buffer sintering thermal stress and avoid film cracking defects, but their own high-temperature melt spreading ability is weak, resulting in relatively low sintering density and weak interfacial adhesion. Even if the formulation is optimized to improve density, it is impossible to achieve a simultaneous match between high density and strong adhesion.
[0004] In summary, current glass powder-based lead-free media slurries cannot simultaneously meet the multiple requirements of crack resistance, high density, and strong adhesion. Summary of the Invention
[0005] In view of this, the present invention provides a lead-free barium aluminum borosilicate-zinc borosilicate dual glass powder composite dielectric slurry, its preparation method, and its application. The present invention composites lead-free barium aluminum borosilicate and zinc borosilicate dual glass powders, resulting in a dielectric slurry with good crack resistance, high density, and strong adhesion to alumina substrates, which can meet the long-term stable use requirements of high-end thick-film electronic components.
[0006] To achieve the above-mentioned objectives, the present invention provides the following technical solution: A lead-free barium aluminum borosilicate-zinc borosilicate dual glass powder composite slurry includes mixed glass powder, organic carrier and dispersant; The mixed glass powder comprises the following components in parts by weight: 75-88 parts of barium aluminum borosilicate glass powder, 12-24 parts of zinc borosilicate glass powder, and 20-10 parts of TiO. The mass ratio of the mixed glass powder, organic carrier, and dispersant is (70~80):(15~28):(0.3~2).
[0007] Preferably, the softening point of the barium aluminum borosilicate glass powder is 700~800℃; the softening point of the zinc borosilicate glass powder is 580~680℃; and the average particle size of the barium aluminum borosilicate glass powder and the zinc borosilicate glass powder is independently 1~4μm.
[0008] Preferably, the molar ratio of BaO, Al2O3, B2O3 and SiO2 in the barium aluminum borosilicate glass powder is (40~60):(3~12):(8~20):(15~35).
[0009] Preferably, the zinc borosilicate glass powder comprises the following components in molar fractions: ZnO 53~70 mol%, B2O3 12~20 mol%, SiO2 15~30 mol%; the molar ratio of ZnO to B2O3 in the zinc borosilicate glass powder is 3.2~4.8.
[0010] Preferably, the organic carrier comprises a binder and an organic solvent, wherein the binder comprises one or more of ethyl cellulose, phenolic resin and polymethacrylic acid resin; the organic solvent comprises at least two of terpineol, dodecyl alcohol, butyl carbitol and butyl carbitol acetate; and the mass ratio of the binder to the organic solvent is (3~17):(83~97).
[0011] Preferably, the dispersant includes one or more of hydrogenated castor oil, oleic acid, polyamide dispersants, and polyacrylic acid dispersants.
[0012] This invention also provides a method for preparing the lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite dielectric slurry described above, comprising the following steps: (1) Mix barium aluminum borosilicate glass powder and zinc borosilicate glass powder, or mix barium aluminum borosilicate glass powder, zinc borosilicate glass powder and TiO2 to obtain mixed glass powder; (2) The mixed glass powder, organic carrier and dispersant are mixed to obtain a premixed slurry; (3) The premixed slurry is rolled and dispersed to obtain the lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite medium slurry.
[0013] Preferably, the stirring speed in step (2) is 700~1500 r / min and the stirring time is 10~40 min; The rolling and dispersing speed in step (3) is 100~200 r / min, the number of rolling times is ≥7, and the fineness of the slurry after rolling is ≤12μm.
[0014] The present invention also provides the application of the lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite dielectric slurry described in the above-described scheme or the lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite dielectric slurry prepared by the preparation method described in the above-described scheme in the preparation of dielectric layers.
[0015] Preferably, the method for preparing the dielectric layer includes: printing the lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite dielectric paste onto a substrate, followed by drying and sintering to obtain the dielectric layer; the drying temperature is 100~140℃ and the time is 10~30min; the sintering temperature is 800~900℃ and the time is 10~40min.
[0016] This invention provides a lead-free barium aluminum borosilicate-zinc borosilicate dual-glass powder composite slurry, comprising mixed glass powders, an organic carrier, and a dispersant; the mixed glass powders comprise the following components by weight: 75-88 parts barium aluminum borosilicate glass powder, 12-24 parts zinc borosilicate glass powder, and 20-10 parts TiO2; the mass ratio of the mixed glass powders, organic carrier, and dispersant is (70-80):(15-28):(0.3-2). The beneficial effects of this invention are: 1. Excellent crack resistance and superior adhesion to substrates. This invention combines BABS glass powder and ZBS dual glass powder, neutralizing the extreme thermal expansion characteristics of the two glass systems. This ensures that the overall thermal expansion coefficient of the composite system is precisely matched with the 96% alumina substrate, significantly eliminating interfacial thermal stress during sintering heating and cooling. It solves the film cracking problem caused by BABS thermal expansion mismatch and improves the weak interfacial bonding of the ZBS system. The sintered film adheres firmly and has good integrity, making it suitable for mainstream ceramic substrate systems.
[0017] 2. Excellent film density and wide adjustable performance range. This invention, through the composite of BABS and ZBS double glass, effectively improves the relatively loose sintering and high porosity defects of the ZBS system, thereby enhancing the basic density of the film. Furthermore, the introduction of an appropriate amount of TiO2 additive further modifies the glass sintering network, promotes denser grain arrangement, effectively strengthens the film structure, reduces porosity defects, and significantly optimizes the film density effect. By adjusting the amount of TiO2 added, this invention enables graded control of film density performance, adapting to application scenarios with different density levels and insulation requirements, significantly improving product adaptability and overall insulation performance.
[0018] 3. Lead-free and environmentally friendly, with stable process and high industrial value. This invention adopts a completely lead-free formula, which complies with the lead-free and environmentally friendly standards of the electronics industry; the preparation process is a conventional process in the industry, with a simple flow, strong controllability, and good repeatability. It is suitable for high-temperature sintering processes of 800~900℃, with a wide process window, and the resulting dielectric layer has excellent performance, possessing good industrial adaptability and engineering practical value.
[0019] In summary, the lead-free barium aluminum borosilicate-zinc borosilicate dual glass powder composite dielectric slurry provided by this invention solves the technical problems of poor thermal compatibility between BABS glass powder and alumina substrate, relatively poor density of ZBS glass powder, and weak interfacial adhesion. It effectively balances the sintering density, interfacial adhesion performance, and crack resistance of the slurry, resulting in a thick-film isolation dielectric slurry with excellent comprehensive performance. It can meet the long-term stable use requirements of high-end thick-film electronic components and has broad application prospects. Attached Figure Description
[0020] Figure 1 The DSC curve of the BABS glass powder prepared in Example 1; Figure 2 This is a SEM image of the dielectric layer obtained after sintering the dielectric slurry in Example 2; Figure 3 This is a SEM image of the dielectric layer obtained after sintering the dielectric slurry in Example 3; Figure 4 This is a SEM image of the dielectric layer obtained after sintering the dielectric slurry in Example 4; Figure 5 This is a SEM image of the dielectric layer obtained after sintering the dielectric slurry in Example 5; Figure 6 This is a SEM image of the dielectric layer obtained after sintering the dielectric slurry in Comparative Example 1. Figure 7 This is a SEM image of the dielectric layer obtained after sintering the dielectric slurry in Comparative Example 2. Figure 8 This is a SEM image of the dielectric layer obtained after sintering the dielectric slurry in Comparative Example 3. Figure 9 This is a SEM image of the dielectric layer obtained after sintering the dielectric slurry in Comparative Example 4. Figure 10 The image shows the SEM image of the dielectric layer after the dielectric slurry and silver paste were sintered together, as obtained in Example 3. The curves represent the results of EDS silver element line scans. Detailed Implementation
[0021] This invention provides a lead-free barium aluminum borosilicate-zinc borosilicate dual glass powder composite medium slurry, comprising mixed glass powder, organic carrier and dispersant; The mixed glass powder comprises the following components in parts by weight: 75-88 parts of barium aluminum borosilicate glass powder, 12-24 parts of zinc borosilicate glass powder, and 20-10 parts of TiO. The mass ratio of the mixed glass powder, organic carrier, and dispersant is (70~80):(15~28):(0.3~2).
[0022] The lead-free barium aluminum borosilicate-zinc borosilicate dual glass powder composite slurry provided by the present invention comprises mixed glass powder; the mixed glass powder comprises the following components in parts by weight: 75-88 parts of barium aluminum borosilicate glass powder, specifically 75, 78, 78.2, 79, 80.6 or 82.5 parts; 12-24 parts of zinc borosilicate glass powder, specifically 14.5, 18, 18.5, 18.8, 19 or 19.4 parts; and 0-10 parts of TiO2, specifically 0, 3, 4, 5, 6 or 7 parts, more preferably 3 parts; the TiO2 specifically refers to TiO2 powder.
[0023] In this invention, the softening point of the barium aluminum borosilicate glass powder is preferably 700~800℃; the molar ratio of BaO, Al2O3, B2O3 and SiO2 in the barium aluminum borosilicate glass powder is preferably (40~60):(3~12):(8~20):(15~35), specifically 50:8:10:32. The preferred method for preparing the barium aluminum borosilicate glass powder includes: mixing BaCO3, Al2O3, H3BO3 and SiO2, followed by sequential melting, water quenching and ball milling to obtain the barium aluminum borosilicate glass powder; the melting temperature is preferably 1300℃, and the melting time is preferably 2 hours.
[0024] In this invention, the softening point of the zinc borosilicate glass powder is preferably 580~680℃; the zinc borosilicate glass powder comprises the following molar fractions: ZnO 53~70 mol%, specifically 55%, 60%, 65% or 68%; B2O3 12~20 mol%, specifically 15%, 16% or 18%; SiO2 15~30 mol%, specifically 26%, 20%, 25% or 28%; the molar ratio of ZnO to B2O3 in the zinc borosilicate glass powder is preferably 3.2~4.8, specifically 3.2, 3.4, 3.6, 3.8, 4.0 or 4.2. In a specific embodiment of this invention, the zinc borosilicate glass powder is prepared according to the method in patent ZL202310882597.6.
[0025] In this invention, the average particle size of the barium aluminum borosilicate glass powder and the zinc borosilicate glass powder is independently 1~4μm, specifically 1, 2, 3 or 4μm.
[0026] The lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite slurry provided by this invention includes an organic carrier. In this invention, the organic carrier preferably includes a binder and an organic solvent. The binder preferably includes one or more of ethyl cellulose, phenolic resin, and polymethyl methacrylate resin. The organic solvent preferably includes at least two of terpineol, dodecyl alcohol ester, butyl carbitol, and butyl carbitol acetate, specifically two or three. In a specific embodiment of this invention, the organic solvent is preferably a mixed solvent of terpineol, butyl carbitol, and butyl carbitol acetate, and the mass ratio of terpineol, butyl carbitol, and butyl carbitol acetate in the mixed solvent is preferably 1:1:2.
[0027] In this invention, the preferred mass ratio of the adhesive to the organic solvent is (3~17):(83~97), specifically 8:92.
[0028] The lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite slurry provided by this invention includes a dispersant. In this invention, the dispersant preferably includes one or more of hydrogenated castor oil, oleic acid, polyamide dispersants, and polyacrylic acid dispersants; the polyamide dispersant preferably includes at least one of polyamide wax and Dispano 6900; and the polyacrylic acid dispersant preferably includes at least one of BYK110, BYK2025, and ammonium polyacrylate.
[0029] In this invention, the mass ratio of the mixed glass powder, organic carrier and dispersant is (70~80):(15~28):(0.3~2), preferably 75.1:24.3:0.6, 75.5:23.9:0.6, 75.7:23.7:0.6 or 75.3:24.1:0.6.
[0030] This invention also provides a method for preparing the lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite dielectric slurry described above, comprising the following steps: (1) Mix barium aluminum borosilicate glass powder and zinc borosilicate glass powder, or mix barium aluminum borosilicate glass powder, zinc borosilicate glass powder and TiO2 to obtain mixed glass powder; (2) The mixed glass powder, organic carrier and dispersant are mixed to obtain a premixed slurry; (3) The premixed slurry is rolled and dispersed to obtain the lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite medium slurry.
[0031] This invention mixes barium aluminum borosilicate glass powder and zinc borosilicate glass powder, or mixes barium aluminum borosilicate glass powder, zinc borosilicate glass powder and TiO2 to obtain a mixed glass powder. This invention does not have special requirements for the mixing conditions; simply mixing all the raw materials evenly is sufficient.
[0032] After obtaining the mixed glass powder, the present invention mixes the mixed glass powder, organic carrier, and dispersant to obtain a premixed slurry. In the present invention, the stirring speed during mixing is preferably 700~1500 r / min, specifically 1000 r / min, and the stirring time is preferably 10~40 min, specifically 15 min.
[0033] After obtaining the premixed slurry, the present invention further disperses the premixed slurry by rolling to obtain the lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite medium slurry. In the present invention, the rolling speed is preferably 100~200 r / min, specifically 150 r / min, the rolling number is preferably ≥7 times, specifically 7~12 times, and the fineness of the slurry after rolling is ≤12μm.
[0034] The present invention also provides the application of the lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite dielectric slurry described in the above-described scheme or the lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite dielectric slurry prepared by the preparation method described in the above-described scheme in the preparation of dielectric layers.
[0035] In this invention, the preferred method for preparing the dielectric layer includes: printing the lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite dielectric paste onto a substrate, followed by drying and sintering to obtain the dielectric layer; the substrate is preferably an alumina substrate; the drying temperature is preferably 100~140℃, specifically 120℃, and the drying time is preferably 10~30min, specifically 15min; the sintering temperature is preferably 800~900℃, specifically 850℃, and the sintering time is preferably 10~40min, specifically 15min.
[0036] The technical solutions of this invention will be clearly and completely described below with reference to the embodiments thereof. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0037] In the following examples, ZBS glass powder was prepared according to the formula and process disclosed in patent ZL202310882597.6, wherein: ZnO 58.33mol%, B2O3 17.16mol%, SiO2 24.51mol%, the molar ratio of ZnO to B2O3 was 3.4, the softening point of ZBS glass powder was 643℃, and the coefficient of thermal expansion was 3.97×10⁻⁶. -6 / ℃ (25~700℃). All examples and comparative examples maintained consistent raw material specifications, preparation equipment, and process parameters to ensure unique experimental variables and reliable comparison results.
[0038] Example 1 This embodiment describes the preparation of BABS glass powder, and the specific steps are as follows: BaCO3, Al2O3, H3BO3, and SiO2 were weighed and thoroughly mixed according to the oxide molar ratio BaO:Al2O3:B2O3:SiO2 = 50:8:10:32. The mixture was then placed in a high-temperature furnace and melted at 1300℃ for 2 hours, followed by rapid water quenching to obtain microcrystalline glass. The microcrystalline glass was then ball-milled, sieved, and dried to obtain BABS glass powder with a softening point of 770℃, which was then set aside. Testing showed that the average particle size of the BABS glass powder was 3 μm, and its coefficient of thermal expansion was 13.71 × 10⁻⁶. -6 / ℃ (25~700℃). Figure 1 The DSC curve of the BABS glass powder prepared in Example 1 is shown.
[0039] The BABS glass powder prepared in this embodiment will be used in subsequent embodiments.
[0040] Example 2 In this embodiment, BABS glass powder and ZBS glass powder were blended to investigate the basic film-forming performance of the dual-glass blend system with a fixed BABS / ZBS ratio.
[0041] S1. Mix 80.6 parts of BABS glass powder and 19.4 parts of ZBS glass powder to obtain a mixed glass powder. S2. Weigh the mixed glass powder, organic carrier (the binder is ethyl cellulose, and the solvent is terpineol, butyl carbitol and butyl carbitol acetate mixed in a mass ratio of 1:1:2, with a binder to solvent mass ratio of 8:92), and dispersant (hydrogenated castor oil) in a homogenizer at a mass ratio of 75.3:24.1:0.6, and stir at 1000 r / min for 15 min to obtain a premixed slurry; S3. Transfer the premixed slurry to a three-roll mill and roll it 12 times at 150 r / min to obtain a medium slurry with a fineness ≤12μm; S4. Print the dielectric paste onto a 96% alumina substrate, level it at room temperature for 15 min, dry it in an oven at 120℃ for 15 min, and sinter it at a peak temperature of 850℃ for 15 min to obtain the dielectric layer.
[0042] Example 3 In this embodiment, the ratio of BABS glass powder to ZBS glass powder remains unchanged, and 3 parts of TiO2 additive are introduced to investigate the film formation of the medium slurry under this TiO2 dosage.
[0043] S1. Take 78.2 parts of BABS glass powder, 18.8 parts of ZBS glass powder and 3 parts of TiO2 additive and mix them initially to obtain mixed glass powder; S2. Weigh the mixed glass powder, organic carrier (the binder is ethyl cellulose, and the solvent is terpineol, butyl carbitol and butyl carbitol acetate mixed in a mass ratio of 1:1:2, with a binder to solvent mass ratio of 8:92), and dispersant (hydrogenated castor oil) in a homogenizer according to a mass ratio of 75.7:23.7:0.6, and stir at 1000 r / min for 15 min to obtain a premixed slurry; S3. Transfer the premixed slurry to a three-roll mill and roll it 12 times at 150 r / min to obtain a medium slurry with a fineness ≤12μm; S4. Print the dielectric paste onto a 96% alumina substrate, level it at room temperature for 15 min, dry it in an oven at 120℃ for 15 min, and sinter it at a peak temperature of 850℃ for 15 min to obtain the dielectric layer.
[0044] Example 4 In this embodiment, the amount of TiO2 added is kept constant, and the mass ratio of BABS glass powder to ZBS glass powder is changed to investigate the effect of the change in the glass powder ratio on the performance of the dielectric layer.
[0045] S1. Take 82.5 parts of BABS glass powder, 14.5 parts of ZBS glass powder and 3 parts of TiO2 additive and mix them initially to obtain mixed glass powder; S2. Weigh the mixed glass powder, organic carrier (the binder is ethyl cellulose, and the solvent is terpineol, butyl carbitol and butyl carbitol acetate mixed in a mass ratio of 1:1:2, with a binder to solvent mass ratio of 8:92), and dispersant (hydrogenated castor oil) in a homogenizer at a mass ratio of 75.1:24.3:0.6, and stir at 1000 r / min for 15 min to obtain a premixed slurry; S3. Transfer the premixed slurry to a three-roll mill and roll it 12 times at 150 r / min to obtain a medium slurry with a fineness ≤12μm; S4. Print the dielectric paste onto a 96% alumina substrate, level it at room temperature for 15 min, dry it in an oven at 120℃ for 15 min, and sinter it at a peak temperature of 850℃ for 15 min to obtain the dielectric layer.
[0046] Example 5 In this embodiment, the ratio of BABS glass powder to ZBS glass powder was kept basically unchanged, and the amount of TiO2 added was increased to investigate the effect of the additive dosage on the film-forming performance.
[0047] S1. Take 75 parts of BABS glass powder, 18 parts of ZBS glass powder and 7 parts of TiO2 additive and mix them initially to obtain mixed glass powder; S2. Weigh the mixed glass powder, organic carrier (the binder is ethyl cellulose, and the solvent is terpineol, butyl carbitol and butyl carbitol acetate mixed in a mass ratio of 1:1:2, with a binder to solvent mass ratio of 8:92), and dispersant (hydrogenated castor oil) in a homogenizer according to a mass ratio of 75.5:23.9:0.6, and stir at 1000 r / min for 15 min to obtain a premixed slurry; S3. Transfer the premixed slurry to a three-roll mill and roll it 12 times at 150 r / min to obtain a medium slurry with a fineness ≤12μm; S4. Print the dielectric paste onto a 96% alumina substrate, level it at room temperature for 15 min, dry it in an oven at 120℃ for 15 min, and sinter it at a peak temperature of 850℃ for 15 min to obtain the dielectric layer.
[0048] Comparative Example 1 This comparative example uses a single BABS glass system without adding ZBS glass powder and TiO2 to characterize the film-forming defects and sintering compatibility of a single high-expansion BABS glass.
[0049] S1. Weigh out BABS glass powder, organic carrier (binder is ethyl cellulose, solvent is terpineol, butyl carbitol and butyl carbitol acetate mixed in a mass ratio of 1:1:2, the mass ratio of binder to solvent is 8:92), and dispersant (hydrogenated castor oil) in a homogenizer according to a mass ratio of 75.1:24.3:0.6, and stir at 1000 r / min for 15 min to obtain a premixed slurry; S2. Transfer the premixed slurry to a three-roll mill and roll it 12 times at 150 r / min to obtain a medium slurry with a fineness ≤12μm; S3. Print the dielectric paste onto a 96% alumina substrate, level it at room temperature for 15 min, dry it in an oven at 120℃ for 15 min, and sinter it at a peak temperature of 850℃ for 15 min to obtain the dielectric layer.
[0050] Comparative Example 2 This comparative example uses a single ZBS glass system without adding BABS glass powder or TiO2 to characterize the inherent performance defects of single ZBS glass powder, such as loose sintering and weak adhesion.
[0051] S1. Weigh ZBS glass powder, organic carrier (binder is ethyl cellulose, solvent is terpineol, butyl carbitol and butyl carbitol acetate mixed in a mass ratio of 1:1:2, the mass ratio of binder to solvent is 8:92), and dispersant (hydrogenated castor oil) in a homogenizer according to a mass ratio of 75.1:24.3:0.6, and stir at 1000 r / min for 15 min to obtain a premixed slurry; S2. Transfer the premixed slurry to a three-roll mill and roll it 12 times at 150 r / min to obtain a medium slurry with a fineness ≤12μm; S3. Print the dielectric paste onto a 96% alumina substrate, level it at room temperature for 15 min, dry it in an oven at 120℃ for 15 min, and sinter it at a peak temperature of 850℃ for 15 min to obtain the dielectric layer.
[0052] Comparative Example 3 This comparative example uses a low-dosage ZBS compound system without TiO2 addition to investigate the effect of low-dosage ZBS on the film-forming properties of BABS matrix.
[0053] S1. Take 89 parts of BABS glass powder and 11 parts of ZBS glass powder and mix them initially to obtain mixed glass powder; S2. Weigh the mixed glass powder, organic carrier (the binder is ethyl cellulose, and the solvent is terpineol, butyl carbitol and butyl carbitol acetate mixed in a mass ratio of 1:1:2, with a binder to solvent mass ratio of 8:92), and dispersant (hydrogenated castor oil) in a homogenizer according to a mass ratio of 76.8:22.6:0.6, and stir at 1000 r / min for 15 min to obtain a premixed slurry; S3. Transfer the premixed slurry to a three-roll mill and roll it 12 times at 150 r / min to obtain a medium slurry with a fineness ≤12μm; S4. Print the dielectric paste onto a 96% alumina substrate, level it at room temperature for 15 min, dry it in an oven at 120℃ for 15 min, and sinter it at a peak temperature of 850℃ for 15 min to obtain the dielectric layer.
[0054] Comparative Example 4 This comparative example uses a high-dosage ZBS compound system without TiO2 addition to investigate the negative issues such as sintering porosity and reduced insulation caused by the high proportion of ZBS glass powder, and to determine the suitable mixing ratio range of the two glass components.
[0055] S1. Take 72.5 parts of BABS glass powder and 27.5 parts of ZBS glass powder and mix them initially to obtain mixed glass powder; S2. Weigh the mixed glass powder, organic carrier (the binder is ethyl cellulose, and the solvent is terpineol, butyl carbitol and butyl carbitol acetate mixed in a mass ratio of 1:1:2, with a binder to solvent mass ratio of 8:92), and dispersant (hydrogenated castor oil) in a homogenizer at a mass ratio of 75:24.4:0.6, and stir at 1000 r / min for 15 min to obtain a premixed slurry; S3. Transfer the premixed slurry to a three-roll mill and roll it 12 times at 150 r / min to obtain a medium slurry with a fineness ≤12μm; S4. Print the dielectric paste onto a 96% alumina substrate, level it at room temperature for 15 min, dry it in an oven at 120℃ for 15 min, and sinter it at a peak temperature of 850℃ for 15 min to obtain the dielectric layer.
[0056] Performance testing 1. Morphological test The microstructure of the dielectric layer surface was observed using a tungsten filament scanning electron microscope at 500x magnification, with a focus on observing the film cracking, number of pores and pore size to determine the coating density level.
[0057] 2. Adhesion test The cross-cut test was used. After cutting, the coating was peeled off by sticking and tearing with tape, and the adhesion level was determined (0 is the best and 5 is the worst).
[0058] 3. Insulation resistance test A high insulation resistance tester was used, with the test voltage set to DC 100V, and the test environment temperature at 25℃ and relative humidity at 50%. The steady-state insulation resistance of the sintered dielectric layer was tested, and each sample was tested three times and the average value was taken to ensure data accuracy.
[0059] The performance test results of Examples 2-5 and Comparative Examples 1-4 are shown in Table 1.
[0060] Table 1 Test Results
[0061] Figures 2-9 SEM images of the dielectric layers obtained after sintering the dielectric slurry in Examples 2-5 and Comparative Examples 1-4; Figure 10 This is a SEM image of the dielectric layer after the dielectric paste and silver paste were sintered together, as obtained in Example 3.
[0062] Combining the performance results of each embodiment and comparative example in Table 1, it can be seen that the single BABS system (Comparative Example 1) exhibits significant cracking defects after sintering (see Table 1). Figure 6 The single ZBS system (Comparative Example 2) exhibits relatively low density (see...). Figure 7 Problems such as poor interfacial adhesion and deteriorated insulation performance exist, meaning that neither can achieve a qualified dielectric layer when used alone. In the binary compound system without added modifiers (Example 2), adjusting the ratio of BABS glass powder to ZBS glass powder can effectively improve the thermal expansion mismatch problem and solve the film cracking defect, but the film still has relatively many pores (see...). Figure 2 The problem is that the overall performance has a clear upper limit.
[0063] The introduction of TiO2 functional additives has a significant synergistic modification effect on the double-glass composite system. Appropriate amounts of TiO2 can optimize the sintering microstructure of the system, fill the micropores in the film layer, promote uniform and dense grain arrangement, and simultaneously strengthen the interfacial bonding between the dielectric layer and the alumina substrate, thereby improving the density and insulation performance of the dielectric layer. Experimental results show that there is an optimal range for TiO2 doping amounts, with 3% doping yielding the best modification effect. The dielectric layers prepared in Examples 3-4 exhibit good density and are virtually pore-free (see...). Figures 3-4 Excessive doping may hinder the melting and spreading of powder during sintering, resulting in more micropores (see...). Figure 5 This, on the contrary, caused a decrease in the density and insulation performance of the film layer. Furthermore, in Comparative Example 3, the ZBS glass powder content was low, resulting in a severely cracked dielectric layer with poor density and a small number of micropores (see...). Figure 8 In Comparative Example 4, the ZBS glass powder content was relatively high, and the resulting dielectric layer did not crack, but had a small number of large pores (see...). Figure 9 Furthermore, the adhesion decreased. This indicates that the ratio of BABS to ZBS is the core key to the thermal expansion matching of the system, and the optimal ratio can synergistically balance the film's crack resistance, sintering density, and adhesion strength to the substrate.
[0064] Combined with the surface SEM and EDS silver element line scan results of the silver paste after sintering with the dielectric slurry in Example 3 ( Figure 10 This method can verify the interfacial compatibility between the dielectric layer and the silver electrode, as well as the resistance to silver ion diffusion. Under optimal formulation, the interface between the dielectric layer and the silver paste is smooth and clear, and the film is dense and complete, without diffusion defects such as pores or cracks. The Ag element line scan signal shows a steep boundary without tailing or dispersion, confirming that there is no silver ion diffusion or interfacial element migration during high-temperature sintering. The dielectric paste provided by this invention can form a dense sintered network, effectively blocking silver electrode ion migration, avoiding interlayer leakage risks, and significantly improving the interfacial stability and service reliability of multilayer thick film devices.
[0065] In summary, this invention, through a formulation design combining high and low softening point BABS and ZBS dual glass powders coupled with an appropriate amount of TiO2 modification, effectively solves the technical problems of easy cracking during sintering of some barium aluminum borosilicate glass pastes and poor density and adhesion of zinc borosilicate glass pastes in alumina substrate systems. The dielectric paste obtained by the optimal ratio of BABS:ZBS:TiO2 = 78.2:18.8:3 is suitable for high-temperature sintering processes of 800~900℃, and the sintered film is crack-free, has high density, strong adhesion, and excellent insulation performance. Furthermore, this invention uses a lead-free environmentally friendly formulation, has a simple preparation process, good stability and repeatability, and can meet the batch preparation needs of high-end thick-film circuit interlayer isolation media, possessing good market application value and promotion prospects.
[0066] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite dielectric slurry, characterized in that, Includes mixed glass powder, organic carrier and dispersant; The mixed glass powder comprises the following components in parts by weight: 75-88 parts of barium aluminum borosilicate glass powder, 12-24 parts of zinc borosilicate glass powder, and 0-10 parts of TiO2; The mass ratio of the mixed glass powder, organic carrier, and dispersant is (70~80):(15~28):(0.3~2).
2. The lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite medium slurry according to claim 1, characterized in that, The softening point of the barium aluminum borosilicate glass powder is 700~800℃; the softening point of the zinc borosilicate glass powder is 580~680℃; and the average particle size of the barium aluminum borosilicate glass powder and the zinc borosilicate glass powder is independently 1~4μm.
3. The lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite dielectric slurry according to claim 1, characterized in that, In the barium aluminum borosilicate glass powder, the molar ratio of BaO, Al2O3, B2O3 and SiO2 is (40~60):(3~12):(8~20):(15~35).
4. The lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite medium slurry according to claim 1, characterized in that, The zinc borosilicate glass powder comprises the following components in molar fractions: ZnO 53~70 mol%, B2O3 12~20 mol%, SiO2 15~30 mol%; the molar ratio of ZnO to B2O3 in the zinc borosilicate glass powder is 3.2~4.
8.
5. The lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite medium slurry according to claim 1, characterized in that, The organic carrier includes a binder and an organic solvent. The binder includes one or more of ethyl cellulose, phenolic resin and polymethyl methacrylate resin. The organic solvent includes at least two of terpineol, dodecyl alcohol, butyl carbitol and butyl carbitol acetate. The mass ratio of the binder to the organic solvent is (3~17):(83~97).
6. The lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite medium slurry according to claim 1, characterized in that, The dispersant includes one or more of hydrogenated castor oil, oleic acid, polyamide dispersants, and polyacrylic acid dispersants.
7. The method for preparing the lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite dielectric slurry according to any one of claims 1 to 6, characterized in that, Includes the following steps: (1) Mix barium aluminum borosilicate glass powder and zinc borosilicate glass powder, or mix barium aluminum borosilicate glass powder, zinc borosilicate glass powder and TiO2 to obtain mixed glass powder; (2) The mixed glass powder, organic carrier and dispersant are mixed to obtain a premixed slurry; (3) The premixed slurry is rolled and dispersed to obtain the lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite medium slurry.
8. The preparation method according to claim 7, characterized in that, The mixing speed in step (2) is 700~1500 r / min, and the mixing time is 10~40 min; The rolling and dispersing speed in step (3) is 100~200 r / min, the number of rolling times is ≥7, and the fineness of the slurry after rolling is ≤12μm.
9. The application of the lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite dielectric slurry according to any one of claims 1 to 6 or the lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite dielectric slurry prepared by the preparation method according to any one of claims 7 to 8 in the preparation of dielectric layers.
10. The application according to claim 9, characterized in that, The method for preparing the dielectric layer includes: printing the lead-free barium aluminum borosilicate-zinc borosilicate double glass powder composite dielectric paste onto a substrate, followed by drying and sintering to obtain the dielectric layer; the drying temperature is 100~140℃ and the time is 10~30min; the sintering temperature is 800~900℃ and the time is 10~40min.
Citation Information
Patent Citations
A low-temperature co-fired ceramic material of zinc-boron-silicate system and its preparation method