Glass microsphere modification equipment and modification methods

By designing hot air ducts and guide plates in the modification equipment, combined with a heating supply unit, uniform modification and rapid reaction of glass microspheres were achieved, solving the problems of long production cycles and easy agglomeration, and improving the utilization efficiency and storage performance of the modifier.

CN123106008APending Publication Date: 2026-11-17ZHENGZHOU HOLLOWLITE MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611361486.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for modifying glass microspheres suffer from problems such as long production cycles, easy agglomeration, and low utilization efficiency of modifiers. In particular, modified glass microspheres prepared by airflow dryers are prone to agglomeration during storage, and dry modification may lead to breakage of glass microspheres.

Method used

A modification device is used, which includes a modification chamber, a hot air source, and a modifier nozzle. The design of the hot air pipe and the guide plate makes the glass microspheres spin and form turbulence in the modification chamber. Combined with the temperature control of the heating supply unit, the modifier is uniformly sprayed and reacted quickly, avoiding the introduction of moisture and shortening the static curing time.

Benefits of technology

This method achieves uniform distribution of the modifier, reduces the amount of modifier used, shortens the production cycle, improves the long-term storage performance of modified glass microspheres, avoids clumping, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106008A_ABST
    Figure CN123106008A_ABST
Patent Text Reader

Abstract

This invention discloses a glass microsphere modification device and method. The bottom surface of the modification chamber of the device is equipped with a heating supply unit. Several guide plates and at least two pairs of modifier nozzles are alternately installed in the modification chamber, with each guide plate having a free end and forming a microsphere flow channel with the inner wall of the modification chamber. Each pair of modifier nozzles is arranged opposite to each other and installed on adjacent guide plates. At least one ring of hot air pipe outlets is provided above each modifier nozzle, and the outlet direction of the hot air pipes intersects with the movement direction of the glass microspheres along the microsphere flow channel, causing the glass microspheres to spin. This results in a more uniform distribution of the silanizing modifier on the surface of the glass microspheres. Furthermore, since no moisture is introduced, the amount of modifier used can be reduced, and the static curing time is short. In addition, since no moisture is introduced during the glass microsphere modification process, the final modified glass microspheres are less prone to clumping even after long-term storage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of glass microsphere modification technology, specifically to a glass microsphere modification device and modification method. Background Technology

[0002] Hollow glass microspheres are lightweight, high-strength, and have good flowability, making them a common filler widely used in industries such as plastics, adhesives, rubber, and coatings. However, as glass microspheres are inorganic materials, their interfacial bonding with some organic materials is relatively poor. To optimize the overall performance of materials after adding glass microspheres, surface modification treatment is generally required before use. Common modification methods include liquid-phase and dry methods. Liquid-phase methods generate large amounts of wastewater during modification, causing pollution. Furthermore, some reactive substances readily react with each other in the liquid phase. Additionally, because some modifiers do not adhere to the powder surface in the liquid phase, a large amount of modifier remains dispersed in the liquid, failing to function effectively. This requires adding a significant amount of modifier to achieve good results. Moreover, since the modifier can react on its own in the liquid phase, imprecise process control can lead to significant variations in the modification effect. Existing dry methods involve mixing the powder and modifier uniformly under high-speed stirring conditions. However, this method can cause glass microsphere breakage and is unsuitable for glass microsphere modification.

[0003] To address the aforementioned issues, Chinese patent application CN117466542A discloses a method for modifying glass microspheres, comprising the following steps: mixing glass microspheres with hot air and introducing the mixture into an airflow drying pipeline for airflow drying; during the airflow drying process, spraying a silanizing modifier and water sequentially onto the glass microspheres; obtaining glass microsphere powder from the outlet of the airflow drying pipeline; and then curing to obtain modified glass microspheres. This patent application CN117466542A employs a combination of dry and wet methods to modify glass microspheres. The dry method involves spraying the silanizing modifier onto the surface of the glass microspheres in a hot air environment, while the wet method involves spraying water to moisten the surface of the glass microspheres coated with the silanizing modifier and induce modification. Finally, the modified glass microspheres are dried again with hot air to become powder and directly discharged without additional dehydration and drying. This method has high utilization efficiency of the silanizing modifier, is simple to operate, and is easy to scale up for industrial production. However, CN117466542A mainly uses an airflow dryer to prepare modified glass microspheres, which requires a long curing time (25-30℃, 26-28h, for further reaction), resulting in a long production cycle and low production efficiency. Moreover, the modified glass microspheres prepared by this method are prone to clumping during storage.

[0004] Therefore, there is a need to propose an equipment for modifying glass microspheres and a method for mass-producing modified glass microspheres using the equipment, which can not only shorten the production cycle of modified glass microspheres, but also effectively improve the performance of modified glass microspheres and give them better long-term storage performance. Summary of the Invention

[0005] Regarding the issue of clumping in modified glass microspheres prepared using CN117466542A during long-term storage, research analysis suggests that this may be due to the water spraying process during microsphere preparation. Since the dryer only has one heat source at the front end, subsequent water spraying may result in heat loss and difficulty in evaporation, leaving excessive residue on the microsphere surface. This leads to the slow precipitation of soluble substances such as free sodium ions during storage, ultimately causing clumping. Furthermore, the large heat dissipation area of ​​the airflow dryer's pipes results in rapid heat loss, requiring a curing time of 26–28 hours at 25–30℃ (for a more complete modification reaction) to ensure sufficient reaction between the glass microspheres and the modifier. This long production cycle hinders industrial-scale application.

[0006] To this end, in a first aspect, the present invention provides a glass microsphere modification device, comprising a modification chamber, a hot air source, and at least two pairs of modifier nozzles. The left and right sides of the modification chamber are respectively provided with an outlet and an inlet. A heating and supply unit is installed on the bottom surface of the modification chamber. A plurality of guide plates are alternately installed on the top and bottom surfaces of the modification chamber, each guide plate having a free end and forming a microsphere flow channel with the inner wall of the modification chamber. The hot air channel is located near the inlet and can blow hot air to allow the glass microspheres to flow along the microsphere flow channel within the modification chamber. Each pair of modifier nozzles is arranged opposite to each other and respectively installed on adjacent guide plates. At least one ring of hot air pipe is arranged 20-30 cm above the modifier nozzles, with the outlet direction of the hot air pipe facing downwards and intersecting the movement direction of the glass microspheres along the microsphere flow channel, causing the glass microspheres to spin.

[0007] In this invention, the "free end" of the guide plate refers to the end of the guide plate that is suspended in the air and is not connected to the bottom or top surface of the modified cavity; the end of the guide plate that is fixed to the top or bottom surface of the modified cavity is the fixed end, which is arranged opposite to the free end.

[0008] Furthermore, the modification chamber is equipped with 2-3 pairs of modifier nozzles, which not only facilitates more uniform application of the modifier but also reduces the amount of modifier used. Preferably, with the bottom surface of the modification chamber as a reference, the height of the modifier nozzles is 1 / 3 to 2 / 3 of the height of the modification chamber; more preferably, it is 1 / 2 of the height of the modification chamber; all modifier nozzles are located on the same horizontal line. This allows for more uniform mixing of the glass microspheres and the modifier.

[0009] In this invention, the height of the modified cavity refers to the distance between its top and bottom surfaces; the length of the modified cavity is defined as the distance between its left and right sides; and the width of the modified cavity is defined as the distance between its front and rear sides. The modified cavity can be a cuboid or similar shape. Preferably, the modified cavity has a height of 2-3 m, a length of 2.5-4.2 m, and a width of 0.6-0.8 m. Specifically, the modified cavity is a cuboid formed by its front and rear sides, left and right sides, top surface, and bottom surface.

[0010] Furthermore, the guide plate divides the total length of the left and right sides of the modified cavity into several single channels. Each single channel is the spacing between two adjacent, staggered guide plates. The free end of the guide plate is spaced apart from the top or bottom surface of the opposing modified cavity to form a narrow channel for the microsphere flow. The length of this narrow channel is 50%-60% of the length of the single channel. This allows for instantaneous acceleration and rapid deceleration of the microspheres, which is beneficial for changing the position of the glass microspheres within the flow channel. Preferably, the length of a single channel is 0.5-0.6 m.

[0011] Furthermore, the outlet directions of the hot air ducts in the same ring are both clockwise or counterclockwise, and they are respectively arranged on the adjacent and intersecting guide plates and the front and rear side surfaces; the angle between the outlet direction of the hot air duct and the horizontal plane is 30°-45° downwards, the angle between the outlet direction of the hot air duct on the guide plate and the front and rear vertical planes is 45°-60° counterclockwise or clockwise, and the angle between the outlet direction of the hot air duct on the front and rear side surfaces and the left and right vertical planes is 45°-60° counterclockwise or clockwise; wherein, the horizontal plane is parallel to the top and bottom surfaces, the front and rear vertical planes are parallel to the front and rear side surfaces, and the left and right vertical planes are parallel to the left and right side surfaces; this is more conducive to the spin of the glass microspheres.

[0012] Furthermore, at least two heating and replenishing units are provided in the modification chamber. The heating temperature of the heating and replenishing units is 130-150℃, which allows the modifier to undergo a bonding reaction with the surface of the glass microspheres; at the same time, it also ensures that the discharge temperature is not lower than 100℃, which helps to shorten the subsequent static curing time of the modified glass microspheres. Preferably, the heating and replenishing unit is located on the bottom surface of the modification chamber directly below the center of the spacing between each pair of modifier nozzles; more preferably, the distance between the heating and replenishing unit and each adjacent pair of modifier nozzles is 1-1.5 m.

[0013] Furthermore, an elastic layer is provided on the guide plate to minimize the breakage of glass microspheres caused by collisions with the guide plate during movement within the modified cavity. Preferably, an elastic layer is also provided inside the modified cavity. The thickness of the elastic layer is 2-3 mm, and the material of the elastic layer can be an elastic material such as high-temperature resistant silicone rubber. The high-temperature resistant silicone rubber includes methyl vinyl silicone rubber (VMQ), methyl vinyl phenyl silicone rubber (PVMQ), phenylene / phenyl ether silicone rubber, and modified fluorosilicone rubber, etc.

[0014] Secondly, the present invention provides a method for modifying glass microspheres, comprising the steps of:

[0015] Provide the above-mentioned modification equipment;

[0016] First, the temperature of the modification chamber is heated to 130-150℃ by the hot air source and heating supply unit. Then, hot air is blown out by the hot air pipe. Next, glass microspheres are added and modified by spraying a modifier onto the glass microspheres. During the modification process, the glass microspheres flowing in the flow channel move along the flow channel under the action of the hot air blown out by the hot air pipe. At the same time, turbulence is formed under the action of each pair of modifier nozzles, so that the modifier is evenly sprayed on the surface of the glass microspheres, forming a modified glass microsphere semi-finished product, which is discharged from the outlet and left to cure to obtain the modified glass microsphere finished product.

[0017] The temperature inside the modified cavity is maintained at 130-150°C, which is beneficial for promoting the bonding reaction between the modifier and the surface of the glass microspheres and keeping the temperature fluctuation inside the modified cavity relatively small.

[0018] Furthermore, the spraying pressure of each modifier nozzle is 0.4–0.5 MPa; this facilitates the formation of turbulence in the hollow glass microspheres under the counter-spraying of each pair of modifier nozzles. Furthermore, the glass microspheres are hollow glass microspheres with a D90 particle size of 30–110 μm; the initial velocity of the hot air blown from the hot air source is 6–8 m / s, and the initial velocity of the hot air blown from the hot air pipe is 5–6 m / s. Thus, as the glass microspheres move along the flow channel within the modification cavity, they not only form turbulence but also spin, with a spin angle greater than 0°, resulting in a more uniform coating of the modifier on the surface of the glass microspheres. Preferably, the hollow glass microspheres have a D90 particle size of 30–80 micrometers and a true density of 0.15–0.7 g / cm³. 3 .

[0019] Furthermore, the mass ratio of the modifier to the glass microspheres is (4-13):1000.

[0020] Furthermore, the modifier is sprayed at least twice. In one specific embodiment, the modifier is sprayed three times, and the mass ratio of the first, second, and third sprays of the modifier to the mass of the glass microspheres is (2-5):(1-5):(1-3):1000.

[0021] The modifier is one or more silanizing modifiers selected from aminopropyltrimethoxysilane, aminopropyltriethoxysilane, glycidyl etheroxypropyltrimethoxysilane, glycidyl etheroxypropyltriethoxysilane, vinyltrimethoxysilane, and vinyltriethoxysilane.

[0022] To ensure a more complete reaction between the modifier and the glass microspheres, the static curing method includes: the temperature of the modified glass microsphere semi-finished product discharged from the outlet is not lower than 100°C, and it is statically cured at room temperature for 4–6 hours. Preferably, the room temperature is 25–30°C.

[0023] Thirdly, the present invention provides a modified glass microsphere prepared by the above method. Preferably, the modified glass microsphere can be used in the preparation of polyurethane adhesives, silicone rubber, etc., so that the polyurethane adhesives, silicone rubber, and other materials have good tensile strength and elongation at break. The amount of the modified glass microsphere added to the polyurethane adhesive or silicone rubber is 1-20 wt%, such as 1 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, etc.

[0024] Therefore, the technical solution provided by this invention can achieve dry modification of glass microspheres. During the modification process, the glass microspheres can move along the feed airflow in the drying chamber, and their movement path can be disturbed by subsequent airflows, and their position can be changed by the gap changes between the guide plate and the top or bottom surface. This makes the modifier more evenly distributed on the surface of the glass microspheres. At the same time, since no water is introduced, the amount of modifier used can be reduced (when water comes into contact with silane coupling agents, the silane coupling agents are more likely to hydrolyze, and also because of the rapid formation of excess silanol groups, they are prone to self-polymerization, thus weakening the modification effect). The static curing time is short. In addition, no water is introduced during the modification process of the glass microspheres, so that the final modified glass microspheres are not prone to clumping even after long-term storage. At the same time, since only the outermost ring of the invention is in contact with air, heat loss is minimal. Attached Figure Description

[0025] Figure 1 This is a front view of the glass microsphere modification device provided in an embodiment of the present invention; wherein, the dotted curve with arrows is the microsphere flow channel, and the arrows on the channel represent the overall flow direction of the glass microspheres;

[0026] Figure 2 The glass microsphere modification equipment provided in this embodiment of the invention is along Figure 1 A cross-sectional view with the dashed line AA in the middle;

[0027] Figure 3 The graph shows the evaluation of the long-term storage performance of the modified glass microsphere powder using Comparative Example 2 (left) and Example 2 (right);

[0028] The component symbols in each figure are as follows: 1-modified cavity, 11-left side, 12-right side, 13-top, 14-bottom, 15-hot air pipe, 16-front side, 17-rear side, 110-outlet, 120-inlet, 2-hot air source, 3-guide plate, 31-free end, 4-modifier nozzle, 5-heating supply unit. Detailed Implementation

[0029] The present invention will be further described in detail below with reference to the embodiments and accompanying drawings, but the embodiments of the present invention are not limited thereto.

[0030] To make the objectives, technical solutions, and advantages of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.

[0031] The endpoints and any values ​​of the ranges disclosed in this invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this invention.

[0032] In this invention, terms such as "up," "down," "left," "right," "front," and "back" used to describe location refer to relative positional relationships, not actual positional relationships, unless otherwise specified.

[0033] In this invention, unless otherwise specified and / or stated, all numerical values ​​involving component amounts are "by weight". Unless otherwise specified, the terminology used in this invention are common terms in the relevant field. Unless otherwise specified, the preparation processes, testing methods, etc., used in the various embodiments are conventional methods well known to those skilled in the art, and the raw materials and equipment used can be obtained from publicly available commercial sources.

[0034] Example 1

[0035] Please see Figure 1 and 2This embodiment provides a glass microsphere modification device, including a modification chamber 1, a hot air source 2, several guide plates 3, at least two pairs of modifier nozzles 4, and at least one ring of hot air pipes 15. The modification chamber is a cuboid, with an outlet 110 and an inlet 120 respectively on its left and right sides 11 and 12. The several guide plates 3 are evenly and alternately installed on the top surface 13 and bottom surface 14 of the modification chamber. One end of each guide plate 3 is fixed to the top surface 13 or bottom surface 14 of the modification chamber, and the opposite end is a free end 31. Thus, the several guide plates 3 and the inner wall of the modification chamber form a microsphere channel for movement. The hot air source 2 is located near the inlet 2, providing the main heat source for the modification chamber 1, while the blown hot air can carry the glass microspheres along the microsphere flow channel. Several heating supply units 5 are installed on the bottom surface 14 of the modification chamber to ensure that the temperature inside the modification chamber is relatively stable during modification and to promote the smooth progress of the modification reaction. Each pair of modifier nozzles 4 is arranged opposite to each other and respectively mounted on adjacent guide plates 3. At least one ring of hot air pipe 15 is arranged 20-30 cm above the modifier nozzle 4. The outlet direction of the hot air pipe 15 intersects the movement direction of the glass microspheres along the flow channel of the microspheres, causing the glass microspheres to spin.

[0036] In this embodiment, the modified cavity 1 is a cuboid with a height of 2 m (distance between the top surface 13 and the bottom surface 14), a length of 4.2 m (distance between the left and right side surfaces 11 and 12), and a width of 0.6 mm. There are six guide plates 3, each 1.7 m long. The free end of each guide plate 3 is spaced 0.3 m from the top surface 13 or bottom surface 14 of the opposing modified cavity to form a narrow channel for the flow of the microspheres. The spacing between adjacent guide plates on the same side is equal, and the spacing between two staggered adjacent guide plates forms a single channel, with each single channel approximately 0.6 meters long. The six guide plates in the modified cavity 1 are divided into three groups, each group consisting of a pair of adjacent, alternately arranged guide plates 3. Each guide plate in each group is equipped with a pair of modifier nozzles 4, with the nozzles in each pair of modifier nozzles 4 facing opposite directions; that is, the modified cavity 1 is equipped with three pairs of modifier nozzles 4. With the bottom surface 14 of the modified cavity as a reference, the height of the modifier nozzle 4 is half the height of the modified cavity, and all modifier nozzles 4 are located on the same horizontal line; this allows for a more uniform mixing of glass microspheres and modifier. Viewed from above, the outlet direction of the hot air pipes 15 in the same ring faces downwards, forming a downward angle of 30° with the horizontal plane (parallel to the top surface 13 and bottom surface 14 of the modified cavity); when the hot air pipe 15 is located on the guide plate 3, the angle between the outlet direction of the hot air pipe 15 and the front and rear vertical planes (parallel to the front and rear sides 16 and 17 of the modified cavity) is 45° clockwise; when the hot air pipe 15 is located on the front and rear sides, the angle between the outlet direction of the hot air pipe 15 and the left and right vertical planes (parallel to the left and right sides 11 and 12 of the modified cavity) is 45° clockwise, which is more conducive to the spin of the glass microspheres. Preferably, the hot air duct 15 is located approximately 25 cm above the modifier nozzle 4. Three heating supply units 5 are installed inside the modification cavity 1, positioned directly below the center of the spacing between each pair of modifier nozzles 4 on the bottom surface 14 of the modification cavity, with each heating supply unit approximately 1 m away from its adjacent pair of modifier nozzles. A VMQ elastic layer approximately 2 mm thick is fixed to each guide plate 3 and the inner wall of the modification cavity 1 to minimize the breakage of glass microspheres caused by collisions with the guide plates 3 during movement within the modification cavity 1.

[0037] To prepare silanized modified microspheres using the aforementioned glass microsphere modification equipment, firstly, the hot air source 2 and heating supply unit 5 are started to heat the temperature of the modification chamber 1 to 130-150℃; then, the hot air pipe 15 is started, and glass microspheres are added from the feed inlet 120. Under the carrying action of the hot air blown from the hot air source 2, the microspheres move along the flow channel within the modification chamber 1; simultaneously, silanization modification is performed. During the modification process, a silanizing modifier is sprayed onto the glass microspheres, and the glass microspheres flow along the microsphere flow channel. During the channel movement, hot air at 130-150°C is blown out from the hot air pipe 15. The glass microspheres spin under the action of the hot air blown out from the hot air pipe 15, and the spin angle is greater than 0°. At the same time, the glass microspheres form turbulence under the action of the opposing spray of each pair of modifier nozzles 4, so that the silanizing modifier is evenly sprayed on the surface of the glass microspheres, forming a modified glass microsphere semi-finished product, which is discharged from the discharge port 110. The discharge temperature is not lower than 100°C, and it is left to stand and cure in an environment of 25-30°C for 4-6 hours to obtain the modified glass microsphere finished product.

[0038] The heating temperature of the heating supply unit is 130-150℃, and the hot air temperature blown out by the hot air source 2 and hot air pipe 15 is also 130-150℃. This ensures a relatively stable temperature within the modification chamber 1, allowing the silanizing modifier to bond with the surface of the glass microspheres. Simultaneously, it ensures that the discharge temperature at the outlet is not lower than 100℃, which helps shorten the subsequent static curing time of the modified glass microspheres. Preferably, the glass microspheres suitable for the above-mentioned glass microsphere modification equipment are hollow glass microspheres with a D90 particle size of 30-110 μm and a true density of 0.15-0.7 g / cm³. 3 The initial velocity of the hot air blown out by the hot air source 2 is 6-8 m / s, the initial velocity of the hot air at the hot air pipe 15 is 5-6 m / s, and the spraying pressure of each modifier nozzle 4 is 0.4-0.5 MPa. In this way, as the glass microspheres move along the flow channel of the microspheres in the modification cavity 1, they not only form turbulence, but also spin, and the spin angle is greater than 0°, so that the modifier is sprayed more evenly on the surface of the glass microspheres.

[0039] Example 2

[0040] This embodiment provides a modified glass microsphere and its preparation method. The modified glass microsphere is prepared using the modification equipment provided in Example 1. The specific preparation method includes: a method for modifying glass microspheres, including the following steps: first, start the hot air source 2 and the heating supply unit 5 to heat the temperature of the modification chamber 1 to 150°C; then start the hot air pipe 15 to blow out hot air at 150°C, and then uniformly introduce glass microspheres from the feed port 120 for silanization modification treatment. Under the action of the 8 m / s hot air blown out by the hot air source 2, the glass microspheres move along the microsphere flow channel. At the same time, under the counter-spraying action of the modifier nozzle 4 with a nozzle pressure of 0.4 MPa, a vortex is formed, and the microspheres spin under the action of the 5 m / s hot air. A semi-finished modified glass microsphere is formed and discharged from the discharge port 110. The discharge temperature is not lower than 100°C. The microspheres are then left to stand and cure at room temperature for 6 hours to obtain the finished modified glass microsphere. The glass microspheres were HL38, and the modifier was aminopropyltrimethoxysilane. During the modification and drying process, the glass microspheres were sprayed with the silanizing modifier three times, and the mass ratio of the first silanizing modifier sprayed, the second silanizing modifier sprayed, the third silanizing modifier sprayed, and the glass microspheres was 3:2:1:1000.

[0041] Example 3

[0042] This embodiment provides a modified glass microsphere and its preparation method, which is basically the same as the modified glass microsphere and its preparation method provided in Embodiment 2. The main differences are: the heating temperature of the heating supply unit 5, the temperature of the hot air blown out by the hot air source 2 and the hot air pipe 15 are all 140°C, the initial velocity of the hot air blown out by the hot air source 2 is 6 m / s, the initial velocity of the hot air blown out by the hot air pipe 15 is 5 m / s, the spraying pressure of the modifier nozzle 4 is 0.5 MPa, the discharge temperature is not lower than 100°C, and the static curing time is 4 h; the spraying mass of the first silanization modifier, the spraying mass of the second silanization modifier, the spraying mass of the third silanization modifier, and the mass ratio of the glass microspheres are 5:2:1:1000.

[0043] Example 4

[0044] This embodiment provides a modified glass microsphere and its preparation method, which is basically the same as the modified glass microsphere and its preparation method provided in Example 2. The main difference is that the mass ratio of the first silanization modifier spraying mass, the second silanization modifier spraying mass, the third silanization modifier spraying mass, and the glass microsphere mass is 2:1:1:1000.

[0045] Example 5

[0046] This embodiment provides a modified glass microsphere and its preparation method, which is basically the same as the modified glass microsphere and its preparation method provided in Embodiment 2. The main differences are: the heating temperature of the heating supply unit 5, the temperature of the hot air blown out by the hot air source 2 and the hot air pipe 15 are all 130 ℃, the initial velocity of the hot air blown out by the hot air source 2 is 8 m / s, the initial velocity of the hot air blown out by the hot air pipe 15 is 6 m / s, the spraying pressure of the modifier nozzle 4 is 0.5 MPa, the discharge temperature is not lower than 100 ℃, and the static curing time is 5 h; and the mass ratio of the first silanization modifier spraying mass, the second silanization modifier spraying mass, the third silanization modifier spraying mass, and the glass microsphere mass is 5:5:3:1000. The silanization modifier is vinyltrimethoxysilane, and the glass microsphere is hollow glass microsphere of model HS38 from Saint-Léite.

[0047] Example 6

[0048] This embodiment provides a modified glass microsphere and its preparation method, which is basically the same as the modified glass microsphere and its preparation method provided in Embodiment 2. The main differences are: the heating temperature of the heating supply unit 5, the temperature of the hot air blown out of the hot air source 2 and the outlet 15 of the hot air pipe are all 150 ℃, the initial velocity of the hot air blown out of the hot air source 2 is 7 m / s, the initial velocity of the hot air blown out of the hot air pipe 15 is 5 m / s, the spraying pressure of the modifier nozzle 4 is 0.5 MPa, the discharge temperature is not lower than 100 ℃, and the static curing time is 6 h; and the mass ratio of the first silanization modifier spraying mass, the second silanization modifier spraying mass, the third silanization modifier spraying mass, and the glass microsphere mass is 5:4:1:1000. The silanization modifier is vinyltrimethoxysilane, and the glass microsphere is hollow glass microsphere of model HL50 from Saint-Léite.

[0049] Comparative Example 1

[0050] This comparative example provides a modified glass microsphere, the preparation method of which includes: placing HL38 hollow glass microspheres, deionized water, and aminopropyltrimethoxysilane in a reaction vessel at a weight ratio of 1000:5000:8, mixing them evenly at 25°C, stirring for 1 h, dehydrating them, and drying them in a forced-air drying oven at 105°C for 4 h.

[0051] Comparative Example 2

[0052] This comparative example provides a modified glass microsphere, which is prepared according to the scheme of Example 1 in CN117466542B, using aminopropyltrimethoxysilane to modify HL38 hollow glass microspheres.

[0053] Comparative Example 3

[0054] This comparative example provides a modified glass microsphere and its preparation method. Based on Example 2, the main differences are: the length of each guide plate 3 is 1.4 m; the hot air pipe 15 faces downward, with an angle of 70° downward to the horizontal plane and an angle of 70° clockwise to the vertical plane; the initial velocity of the hot air blown out by the hot air source 2 is 10 m / s; the initial velocity of the hot air blown out by the hot air pipe 15 is 3 m / s; the spraying pressure of the modifier nozzle 4 is 0.4 MPa; the discharge temperature is greater than 100 ℃, and the static curing time is 4 h.

[0055] Comparative Example 4

[0056] This comparative example provides a modified glass microsphere and its preparation method. Based on Example 2, the main difference is that: the length of each guide plate 3 is 1.5 m, the hot air pipe 15 faces downward, the angle between the hot air pipe 15 and the horizontal plane is 50° downward and the angle between the hot air pipe 15 and the vertical plane is 30° clockwise, the initial velocity of the hot air blown out by the hot air source 2 is 6 m / s, the initial velocity of the hot air blown out by the hot air pipe 15 is 6 m / s, and the static curing time is 5 h.

[0057] Comparative Example 5

[0058] This comparative example provides a modified glass microsphere, the preparation method of which refers to the scheme of Example 3 in CN117466542B, the difference being: this comparative example uses vinyltrimethoxysilane to modify HS38 hollow glass microspheres, and the mass ratio of the first vinyltrimethoxysilane, the second vinyltrimethoxysilane, the third vinyltrimethoxysilane, water and glass microspheres is 5:5:3:5:1000.

[0059] application

[0060] The modified glass microspheres provided in Examples 2-4 and Comparative Examples 1-4 were used in the preparation of polyurethane adhesives, and the modified glass microspheres provided in Examples 5-6 and Comparative Example 5 were used in low-density silicone rubber. The tensile strength, elongation at break, and long-term storage performance of the corresponding polyurethane adhesives or silicone rubbers were measured, and the results are shown in Table 1.

[0061] 1) The method for determining the tensile strength and elongation at break of polyurethane adhesive is as follows: Components A and B are mixed evenly at a mass ratio of 100:830 to prepare a dumbbell-shaped sheet with a thickness of 2 mm. After curing under standard conditions for 7 days, its tensile strength and elongation at break are tested using a universal tensile testing machine at a speed of 500 mm / min. The polyurethane adhesive includes:

[0062] Component A: PAPI (polymethylene polyphenyl polyisocyanate);

[0063] Component B: Composed of the following components in parts by weight: 7 parts polyether polyol YD305, 90 parts polyether polyol 330n,

[0064] 15 parts glass microspheres, 2 parts fumed silica, and 0.07 parts dibutyltin dilaurate.

[0065] The processing of component B is as follows: polyether polyol YD305 and polyether polyol 330n are added to a dehydration reactor and dehydrated for 2 h at a pressure below -0.095 MPa and a temperature of 100°C. Then, the temperature is lowered to 35°C, and the dehydrated modified glass microspheres, fumed silica and dibutyltin dilaurate are added to the dehydration reactor respectively. The mixture is then stirred under vacuum for 10 min to obtain component B.

[0066] 2) Low-density silicone rubber comprises: 70 parts by weight of vinyl silicone rubber (60A, vinyl content 1%), 3 parts by weight of methyl silicone oil (200 cps), 18 parts by weight of calcium carbonate, and 0.5 parts by weight of silane coupling agent vinyltrimethoxysilane. The mixture is then kneaded for 18 min at 113°C under vacuum below -0.095 MPa using a vacuum kneader. 7 parts by weight of modified glass microspheres are added, and kneading is continued for 8 min. Finally, 1.2 parts by weight of vulcanizing agent bis(2,5-dimethyl)sulfurizing agent is added at room temperature on an open mill, and the mixture is kneaded for 8 min to obtain the low-density silicone rubber product. This product is then pressed into 2 mm thick sheets and vulcanized for 4.2 min on a flat vulcanizing machine at 180°C. After curing the vulcanized sheets under standard conditions for 7 days, they are cut into dumbbell-shaped pieces for testing their tensile strength and elongation at break. The testing speed is 500 mm / min.

[0067] 3) Evaluation method for long-term storage performance: The prepared modified glass microspheres were placed in a sealed package and placed in an environment of 70°C and 90% humidity. After 15 days, it was observed whether there was clumping.

[0068] Table 1 Performance Test Results

[0069] Modified glass microspheres in adhesives Tensile strength (MPa) Elongation at break (%) Long-term storage performance Example 2 5.5 368 No clumps Comparative Example 1 4.9 333 No clumps Comparative Example 2 5.5 370 There are clumps Comparative Example 3 5.2 358 No clumps Comparative Example 4 5.3 362 No clumps Example 3 5.7 371 No clumps Example 4 5.4 363 No clumps Example 5 3.4 286 No clumps Comparative Example 5 3.2 265 There are clumps Example 6 3.3 279 No clumps

[0070] From Table 1 and Figure 3It can be seen that the technical solution provided by the embodiments of the present invention achieves dry modification of glass microspheres. During the modification and drying process, the glass microspheres can move along the feed airflow in the modification chamber, and can not only spin under the action of hot air, but also form turbulence under the spraying action of the modifier nozzle, so that the silanizing modifier is more evenly distributed on the surface of the glass microspheres, reducing the amount of coupling agent used (comparative Examples 2 and 3 and Comparative Example 2). In addition, since no water is introduced, the amount of silanizing modifier used can be reduced; at the same time, due to the control of the discharge temperature, the static curing time is short. Furthermore, since no water is introduced during the modification process of the glass microspheres, the final modified glass microspheres are not prone to agglomeration even after long-term storage. Figure 3 As shown (Comparative Example 2, Comparative Example 2, Example 5 and Comparative Example 5).

[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them; although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications can still be made to the specific implementation of the present invention or equivalent substitutions can be made to some technical features without departing from the spirit of the technical solutions of the present invention, and all such modifications and substitutions should be covered within the scope of the technical solutions claimed in the present invention.

Claims

1. A glass microsphere modification device, characterized in that, The device includes a modification chamber, a hot air source, and at least two pairs of modifier nozzles. The left and right sides of the modification chamber are respectively provided with an outlet and an inlet. A heating and supply unit is installed on the bottom surface of the modification chamber. Several guide plates are alternately installed on the top and bottom surfaces of the modification chamber, each guide plate having a free end and forming a microsphere flow channel with the inner wall of the modification chamber. The hot air channel is located near the inlet and can blow hot air to carry glass microspheres along the microsphere flow channel within the modification chamber. Each pair of modifier nozzles is arranged opposite each other and installed on adjacent guide plates. At least one ring of hot air pipe is arranged 20-30 cm above the modifier nozzles, with the outlet direction of the hot air pipes facing downwards and intersecting the movement direction of the glass microspheres along the microsphere flow channel, causing the glass microspheres to spin.

2. The modification equipment according to claim 1, characterized in that, With the bottom surface of the modified cavity as a reference, the height of the modifier nozzle is 1 / 3 to 2 / 3 of the height of the modified cavity.

3. The modification equipment according to claim 1 or 2, characterized in that, The guide plate divides the total length of the left and right sides of the modified cavity into several single channels. The single channel is the spacing formed between two adjacent staggered guide plates. The free end of the guide plate is spaced apart from the top or bottom surface of the opposite modified cavity to form a narrow channel for the flow of microbeads. The length of the narrow channel is 50%-60% of the length of the single channel.

4. The modification equipment according to claim 1 or 2, characterized in that, The modified cavity also includes front and rear sides, which, together with the left and right sides, the top surface, and the bottom surface, form a cuboid shape. The outlet direction of the hot air ducts in the same ring is either clockwise or counterclockwise, and they are respectively arranged on the adjacent and intersecting guide plates and the front and rear sides. The angle between the outlet direction of the hot air duct and the horizontal plane is 30°-45° downwards. The angle between the outlet direction of the hot air duct located on the guide plate and the front and rear vertical planes is 45°-60° counterclockwise or clockwise. The angle between the outlet direction of the hot air duct located on the front and rear sides and the left and right vertical planes is 45°-60° counterclockwise or clockwise. The horizontal plane is parallel to the top and bottom surfaces, the front and rear vertical planes are parallel to the front and rear sides, and the left and right vertical planes are parallel to the left and right sides.

5. The modification equipment according to claim 1, characterized in that, At least two heating supply units are provided in the modified cavity, and the heating supply units are located on the bottom surface of the modified cavity directly below the center of the spacing between each pair of modifier nozzles.

6. The modification equipment according to claim 1, characterized in that, An elastic layer is provided on the flow guide plate.

7. A method for modifying glass microspheres, comprising the following steps: Provide the modified device according to any one of claims 1 to 6; First, the temperature of the modified cavity is heated to 130-150°C using the hot air source and heating supply unit. Then, hot air is blown out through the hot air pipe. Next, glass microspheres are added, and modification is achieved by spraying a modifier onto the glass microspheres. As the glass microspheres move along the flow channel under the influence of the hot air blown out of the hot air channel, during the modification process, the glass microspheres flowing in the flow channel spin under the action of the hot air blown out of the hot air pipe, and at the same time form turbulence under the action of each pair of modifier nozzles, so that the modifier is evenly sprayed on the surface of the glass microspheres, forming a modified glass microsphere semi-finished product, which is discharged from the outlet and left to stand for curing to obtain the modified glass microsphere finished product.

8. The modification method according to claim 7, characterized in that, The spraying pressure of each modifier nozzle is 0.4 to 0.5 MPa, and the temperature of the hot air blown out by the hot air pipe is 130 to 150°C.

9. The modification method according to claim 7 or 8, characterized in that, The glass microspheres are hollow glass microspheres with a D90 particle size of 30-110 μm. The initial velocity of the hot air blown out by the hot air source is 6-8 m / s, the initial velocity of the hot air blown out by the hot air pipe is 5-6 m / s, and the spin angle of the glass microspheres is greater than 0°.

10. The modification method according to claim 7 or 8, characterized in that, The mass ratio of the modifier to the glass microspheres is (4-13):1000.

11. The modification method according to claim 10, characterized in that, The modifier is sprayed three times, and the mass ratio of the first, second, and third sprays of the modifier to the mass of the glass microspheres is (2-5):(1-5):(1-3):1000.

12. The modification method according to claim 7 or 8, characterized in that, The static curing method includes: the temperature of the modified glass microsphere semi-finished product discharged from the outlet is not lower than 100°C, and it is statically cured at room temperature for 4 to 6 hours.

13. A modified glass microsphere prepared by the modification method according to any one of claims 7 to 10.

Citation Information

Patent Citations

  • Modification method of glass beads

    CN117466542A