A method for preparing alternative fuel for cement kilns using industrial waste residue
By compounding microsilica powder and slag with low-calorific-value coal gangue and carbide slag, alternative fuels for cement kilns are prepared, which solves the problem of crusting and blockage caused by direct feeding of low-calorific-value coal gangue into the kiln, improves combustion efficiency and kiln system stability, and expands its application in cement kilns.
Patent Information
- Application Number
- CN202611420189.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-17
AI Technical Summary
When low-calorific-value coal gangue is used directly as fuel in cement kilns, it is prone to incomplete combustion in the decomposition furnace, resulting in local high-temperature crusting that blocks the cyclone separator and feed pipe, thus limiting its utilization efficiency and proportion in cement kilns.
Alternative fuels are prepared by blending microsilica powder, slag, low-calorific-value coal gangue, and carbide slag. Microsilica powder is used to improve combustion mass transfer, and slag is used to regulate ash melting characteristics. Combined with dynamic monitoring and adjustment, the problem of crusting and blockage is solved.
It improves the combustion efficiency of low-calorific-value coal gangue, reduces crusting and blockage, expands its utilization rate in cement kilns, reduces preparation costs, and enhances the stability of the kiln system.
Smart Images

Figure CN123106038A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of cement industry technology, and in particular relates to a method for preparing alternative fuels for cement kilns using industrial waste residue. Background Technology
[0002] Coal gangue is a solid waste generated during coal mining and washing. Its annual emissions are enormous, with accumulated stockpiles exceeding 7 billion tons, occupying vast amounts of land and polluting the surrounding environment. Coal gangue contains a certain amount of fixed carbon and volatile matter, with a lower calorific value typically ranging from 800 to 3000 kcal / kg, demonstrating its potential as a fuel. Using coal gangue as an alternative fuel in cement production can both dispose of solid waste and reduce cement companies' reliance on high-quality coal, representing a crucial direction for energy conservation and emission reduction in the cement industry.
[0003] The precalciner in a cement kiln is the core equipment in the precalciner kiln system, responsible for fuel combustion and raw meal carbonate decomposition. Its internal temperature is typically controlled between 900-1100℃. Fuel burns and releases heat within the precalciner, which is then supplied to the raw meal powder in the kiln tail preheater system for endothermic decomposition. The gas flow at the precalciner outlet carries unburned fuel particles and raw meal dust, which undergo gas-solid separation in the lowest-level cyclone separator (usually a C5 cyclone). The normal operation of the C5 cyclone separator and its feed pipe directly impacts the stability and operating rate of the kiln system.
[0004] When low-calorific-value coal gangue (lower heating value below 1600 kcal / kg) is used directly as a substitute fuel in a decomposition furnace, its low volatile matter content, poor fixed carbon activity, high ignition temperature, and long burnout time result in a large number of carbon particles failing to burn completely within the furnace. These particles are carried by the airflow into the C5 cyclone zone. In this zone, the gas temperature remains between 800-900℃, and the oxygen content is relatively abundant. Unburned carbon particles undergo secondary combustion here, creating localized high temperatures. This localized high temperature softens or even partially melts the low-melting-point components in the material carried by the airflow, causing them to adhere to the conical part of the cyclone and the inner wall of the feed pipe, gradually thickening to form a crust. Once the crust reaches a certain thickness, it reduces the effective cross-sectional area of the feed pipe or even completely blocks it, forcing the production line to reduce output or shut down for cleaning. This problem directly limits the substitution ratio and utilization efficiency of low-calorific-value coal gangue in cement kilns.
[0005] Currently, cement companies primarily address this issue by limiting the proportion of coal gangue (usually controlled below 10% of the total fuel calorific value), increasing the frequency of manual or mechanical cleaning of the crust, or adding some high-grade coal to the coal gangue to improve the average calorific value of the mixed fuel. Some companies have also attempted to adjust the type and amount of alumina corrective raw materials in the raw meal formula to try to change the sintering characteristics of the materials entering the kiln, but due to the limitations of raw meal ratio control requirements, the adjustment range is limited, and the effect on alleviating the crusting problem is not significant. In addition, although various combustion aids are available on the market, their costs are high and their effects are unstable, failing to gain widespread acceptance in the industry.
[0006] The Wuhai area and surrounding regions of Inner Mongolia are home to large-scale calcium carbide-based PVC production enterprises, ferrosilicon alloy smelting enterprises, and coal chemical enterprises. Cement plants also have stable sources of various industrial wastes, including calcium carbide slag, microsilica powder, and furnace slag. Local cement production lines have long used calcium carbide slag as a calcareous raw material to replace limestone, achieving mature operational experience. However, when utilizing the abundant low-calorific-value coal gangue in the region as a substitute fuel on a large scale, the aforementioned scaling and clogging problems become prominent. Therefore, the following solutions are proposed to address these issues. Summary of the Invention
[0007] The purpose of this invention is to provide a method for preparing alternative fuels for cement kilns using industrial waste residue. The method involves preparing alternative fuels by compounding silica powder, slag, low-calorific-value coal gangue, and carbide slag. Silica powder is used to improve combustion mass transfer, and slag is used to adjust ash melting characteristics, making the fuel combustion characteristics suitable for the decomposition furnace operating conditions. This solves the problem of scale formation and blockage caused by directly feeding low-calorific-value coal gangue into the kiln, leading to forced production reductions and kiln shutdowns.
[0008] To solve the above-mentioned technical problems, the present invention is achieved through the following technical solution: This invention discloses a method for preparing alternative fuel for cement kilns using industrial waste residue, comprising the following steps: Raw material pretreatment: Low-calorific-value coal gangue is crushed to a particle size of less than or equal to 5 mm to obtain coarse coal gangue powder; calcium carbide slag is dried to a moisture content of less than or equal to 2.0% to obtain dry calcium carbide slag powder; microsilica powder is selected; slag is crushed to a particle size of less than or equal to 3 mm to obtain coarse slag powder. Accurate weighing and batching: Weigh the four materials in the raw material pretreatment step according to the dry basis mass ratio, the ratio is: 55-65 parts of low calorific value coal gangue coarse powder, 20-30 parts of dry powdered carbide slag, 3-8 parts of microsilica powder, and 5-12 parts of slag coarse powder. Mixing and homogenization: The four weighed materials are fed into a forced mixing mixer. During the mixing process, atomized water is sprayed to control the total moisture content of the mixture to 12%-15%. The mixture is stirred for 180-300 seconds to obtain homogenized wet material. Extrusion granulation: The homogenized wet material is fed into a double-roller extrusion granulator and extruded under a pressure of 15-25 MPa to obtain shaped granules with a diameter of 8-15 mm and a length of 10-25 mm. Drying and cooling: The shaped pellets are fed into a dryer and dried with hot air at 250-350℃ until the moisture content is less than or equal to 5%, and then cooled to less than or equal to 60℃ to obtain the finished alternative fuel pellets; Pneumatic conveying and kiln feeding: The finished alternative fuel pellets are fed into the central area of the cement kiln decomposition furnace through a pneumatic conveying system for injection and combustion. The feed amount of alternative fuel is controlled to account for 15%-25% of the total calorific value of the kiln system fuel. System monitoring and dynamic adjustment: The temperature of the feed pipe of the lowest cyclone is monitored in real time. When the temperature of the feed pipe continues to be higher than 845℃, the feed amount of alternative fuel is automatically reduced, and the proportion of microsilica powder is increased by 0.5-1.0 percentage points until the temperature returns to normal.
[0009] Furthermore, the low-calorific-value coal gangue mentioned in the raw material pretreatment step has a lower heating value of 1500-2200 kcal / kg and a loss on ignition of 3%-6%. Its chemical composition, by mass percentage, includes: SiO2 20%-30%, Al2O3 15%-25%, Fe2O3 1%-3%, and CaO 3%-8%.
[0010] Furthermore, the dry basis chemical composition of the carbide slag mentioned in the raw material pretreatment step, by mass percentage, includes: loss on ignition 28%-32%, CaO≥60%, SiO2 3%-8%, Al2O3 1%-3%, Fe2O3 0.5%-1.5%, MgO≤0.5%.
[0011] Furthermore, the SiO2 content of the microsilica powder in the raw material pretreatment step is ≥80%, the specific surface area is ≥15000 m² / kg, and the loss on ignition is ≤5%.
[0012] Furthermore, the chemical composition of the slag in the raw material pretreatment step, by mass percentage, includes: loss on ignition 3%-7%, SiO2 40%-45%, Al2O3 30%-35%, Fe2O3 2%-4%, CaO 8%-12%, and MgO 0.5%-1.5%.
[0013] Furthermore, the precise weighing and proportioning of the dry basis mass of the ingredients are as follows: 60 parts of low-calorific-value coal gangue coarse powder, 25 parts of dry carbide slag powder, 5 parts of microsilica powder, and 10 parts of slag coarse powder.
[0014] Furthermore, in the mixing and homogenization process, the stirring spindle speed of the forced stirring mixer is 200-300 rpm, the mixing time is 240 seconds, and the amount of atomized water added is controlled to be 13%-14% of the total mass of the mixture.
[0015] Furthermore, the dryer described in the drying and cooling process is a mesh belt through-flow dryer, with the heat source being waste hot air at 250-350℃ extracted from the middle section of the grate cooler at the kiln head of the cement kiln. The dried shaped particles are cooled to ≤60℃ by a fluidized bed cooler.
[0016] Furthermore, the solid-to-gas ratio of the pneumatic conveying to the gas in the kiln is 3-5 kg / kg, the conveying wind speed is 18-25 m / s, and the injection into the central region of the decomposition furnace adopts a multi-head swirl spray gun to ensure that the alternative fuel particles are evenly dispersed within the cross-section of the decomposition furnace.
[0017] Furthermore, the high-limit alarm value for the temperature of the lowest-level cyclone feed pipe in the system monitoring and dynamic adjustment is 845℃, and the high-high-limit alarm value is 860℃. When the temperature continues to be higher than 845℃, the feed rate of alternative fuel is reduced in increments of 0.5 tons / hour, and the proportion of microsilica powder is increased by 0.5-1.0 percentage points within 30 seconds, while the proportion of slag is reduced by the same percentage point to maintain the total feed rate unchanged. After the feed pipe temperature drops back to below 835℃ and remains there for 300 seconds, it automatically returns to the initial proportion and feed rate. When the temperature reaches 860℃, the system automatically interlocks and cuts off the supply of alternative fuel, switching to 100% pulverized coal operation.
[0018] The present invention has the following beneficial effects: This invention utilizes silica fume and slag as regulators, synergistically compounded with low-calorific-value coal gangue and carbide slag, to prepare an alternative fuel with combustion characteristics similar to pulverized coal used in cement kilns. This helps reduce the adverse effects of directly feeding low-calorific-value coal gangue into the kiln on the stability of the kiln system. Silica fume and slag are both industrial waste residues from around cement plants, widely available and inexpensive to obtain. As regulators, they require no complex pretreatment, reducing the cost of alternative fuel preparation and expanding its resource utilization pathways. Silica fume coats the surface of coal gangue particles, providing more active interfaces for carbon oxidation, improving mass and heat transfer conditions, and promoting fuel burnout. The aluminum component in the slag corrects the silica-alumina ratio of the mixed ash, facilitating the transformation of ash into high-melting-point mineral phases at high temperatures and reducing the tendency for ash to soften and melt. The highly active calcium-based components generated from the decomposition of carbide slag react with sulfur-containing oxides released during combustion to form stable sulfates, achieving in-situ sulfur fixation and reducing sulfur emissions. Furthermore, the process flow of this invention is highly compatible with existing cement production lines, making it easy to promote and apply on existing industrial foundations.
[0019] Of course, any product implementing this invention does not necessarily need to achieve all of the advantages described above at the same time. Attached Figure Description
[0020] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0021] Figure 1 This is a schematic flowchart of a method for preparing alternative fuel for cement kilns using industrial waste residue according to the present invention. Detailed Implementation
[0022] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] Please see Figure 1 As shown, this invention discloses a method for preparing alternative fuel for cement kilns using industrial waste residue, comprising the following steps: Raw material pretreatment: Low-calorific-value coal gangue is crushed to a particle size of less than or equal to 5 mm to obtain coarse coal gangue powder; calcium carbide slag is dried to a moisture content of less than or equal to 2.0% to obtain dry calcium carbide slag powder; microsilica powder is selected; slag is crushed to a particle size of less than or equal to 3 mm to obtain coarse slag powder. Accurate weighing and batching: Weigh the four materials in the raw material pretreatment step according to the dry basis mass ratio, and the ratio is as follows: 55-65 parts of low calorific value coal gangue coarse powder, 20-30 parts of dry powdered carbide slag, 3-8 parts of microsilica powder, and 5-12 parts of slag coarse powder. Mixing and homogenization: The four weighed materials are fed into a forced mixing mixer. During the mixing process, atomized water is sprayed to control the total moisture content of the mixture to 12%-15%. The mixture is stirred for 180-300 seconds to obtain homogenized wet material. Extrusion granulation: The homogenized wet material is fed into a double-roller extrusion granulator and extruded under a pressure of 15-25 MPa to obtain shaped granules with a diameter of 8-15 mm and a length of 10-25 mm. Drying and cooling: The shaped pellets are fed into a dryer and dried with hot air at 250-350℃ until the moisture content is less than or equal to 5%, and then cooled to less than or equal to 60℃ to obtain the finished alternative fuel pellets; Pneumatic conveying and kiln feeding: The finished alternative fuel pellets are fed into the central area of the cement kiln decomposition furnace through a pneumatic conveying system for injection and combustion. The feed amount of alternative fuel is controlled to account for 15%-25% of the total calorific value of the kiln system fuel. System monitoring and dynamic adjustment: The temperature of the feed pipe of the lowest cyclone is monitored in real time. When the temperature of the feed pipe continues to be higher than 845℃, the feed amount of alternative fuel is automatically reduced, and the proportion of microsilica powder is increased by 0.5-1.0 percentage points until the temperature returns to normal.
[0024] The lower heating value of the low-calorific-value coal gangue in the raw material pretreatment step is 1500-2200 kcal / kg, and the loss on ignition is 3%-6%. Its chemical composition, by mass percentage, includes: SiO2 20%-30%, Al2O3 15%-25%, Fe2O3 1%-3%, and CaO 3%-8%.
[0025] The dry basis chemical composition of the carbide slag in the raw material pretreatment step, by mass percentage, includes: loss on ignition 28%-32%, CaO≥60%, SiO2 3%-8%, Al2O3 1%-3%, Fe2O3 0.5%-1.5%, MgO≤0.5%.
[0026] In the raw material pretreatment step, the SiO2 content of the microsilica powder is ≥80%, the specific surface area is ≥15000 m² / kg, and the loss on ignition is ≤5%.
[0027] The chemical composition of the slag in the raw material pretreatment step, by mass percentage, includes: loss on ignition 3%-7%, SiO2 40%-45%, Al2O3 30%-35%, Fe2O3 2%-4%, CaO 8%-12%, and MgO 0.5%-1.5%.
[0028] The precise weighing and batching of dry basis mass ratios are as follows: 60 parts of low-calorific-value coal gangue coarse powder, 25 parts of dry carbide slag powder, 5 parts of microsilica powder, and 10 parts of slag coarse powder.
[0029] The mixing spindle speed of the forced mixing mixer during mixing and homogenization is 200-300 rpm, the mixing time is 240 seconds, and the amount of atomized water added is controlled to be 13%-14% of the total mass of the mixture.
[0030] The drying and cooling process uses a mesh belt through-flow dryer. The heat source is 250-350℃ waste heat air extracted from the middle section of the grate cooler at the kiln head of the cement kiln. The dried shaped particles are cooled to ≤60℃ by a fluidized bed cooler.
[0031] The solid-to-gas ratio of pneumatic conveying to pneumatic conveying in the kiln is 3-5 kg / kg, and the conveying wind speed is 18-25 m / s. The injection in the middle area of the decomposition furnace adopts a multi-head swirl spray gun to make the alternative fuel particles evenly dispersed in the cross section of the decomposition furnace.
[0032] The highest alarm value for the temperature of the lowest-level cyclone feed pipe in the system monitoring and dynamic adjustment is 845℃, and the highest-highest alarm value is 860℃. When the temperature continues to be higher than 845℃, the feed rate of alternative fuel is reduced in increments of 0.5 tons / hour, and the proportion of microsilica powder is increased by 0.5-1.0 percentage points within 30 seconds, while the proportion of slag is reduced by the same percentage point to maintain the total feed rate unchanged. When the feed pipe temperature drops back to below 835℃ and is maintained for 300 seconds, it automatically restores to the initial proportion and feed rate. When the temperature reaches 860℃, the system automatically interlocks and cuts off the supply of alternative fuel, switching to 100% pulverized coal operation.
[0033] The specific application of this embodiment is as follows: Step S1: Raw material selection and pretreatment Step S11: Selection and Crushing of Low-Calorific-Value Coal Gangue: Select low-calorific-value coal gangue from coal washing plants surrounding cement plants, homogenized in the stockpile. The requirements for this coal gangue are: net calorific value between 1500 kcal / kg and 2200 kcal / kg, preferably 1500-1700 kcal / kg; loss on ignition (Loss) of 3%-6%; and SiO2 content of 20%-30% and Al2O3 content of [missing information]. The coal gangue contains 15%-25% Fe2O3, 1%-3% CaO, and 3%-8% CaO. The incoming lumpy coal gangue is fed into a jaw crusher for coarse crushing, followed by a hammer crusher for fine crushing until all particles pass through a 5mm square-hole sieve, yielding coarse coal gangue powder. During the crushing process, a dust removal system is activated to control the dust concentration in the crushing workshop to below 10mg / m³. The crushed coarse coal gangue powder is then sent to an intermediate buffer silo for later use. Step S12, Selection and Drying of Calcium Carbide Slag: Select dry-discharged calcium carbide slag or wet-discharged calcium carbide slag after pressure filtration from a nearby calcium carbide-based PVC production plant. The dry basis chemical composition requirements for this calcium carbide slag are: Loss on ignition 28%-32%, CaO content ≥60%, SiO2 content 3%-8%, Al2O3 content 1%-3%, Fe2O3 content 0.5%-1.5%, MgO content ≤0.5%. If wet-discharged calcium carbide slag is selected, its initial moisture content is 25%-40%, and it needs to be pre-dried in a calcium carbide slag drying system. The drying heat source is the exhaust gas from the cement kiln head cooler (temperature approximately 300-400℃). The moisture content of the calcium carbide slag is dried to ≤2.0% in the drying rotary drum to obtain dry powder calcium carbide slag. If dry-discharged calcium carbide slag is selected, it is directly sent to the dry powder silo for storage. The dried powder calcium carbide slag is then sent to the calcium carbide slag batching silo via a bucket elevator for later use. Step S13, Selection of Microsilica Powder: Select microsilica powder (also known as silica fume) collected by bag filter during the production process of a nearby ferrosilicon alloy plant or industrial silicon plant; the requirements for this microsilica powder are: SiO2 content ≥80%, preferably ≥85%; specific surface area ≥15000 m² / kg (BET method); Loss (loss on ignition) ≤5%; bulk density 150-300 kg / m³; as an ultrafine powder material, the microsilica powder is directly sent to a closed microsilica powder batching silo for storage via a pneumatic conveying system after entering the plant, and a pulse bag filter is installed on the top of the silo to prevent dust from overflowing; this microsilica powder does not require any pretreatment operations such as grinding or sieving; Step S14, Selection and Crushing of Slag: Select circulating fluidized bed boiler slag discharged from a nearby thermal power plant or a self-owned power station of a chemical plant; the chemical composition requirements for this slag are: Loss (loss on ignition) 3%-7%, SiO2 content 40%-45%, Al2O3 content 30%-35%, Fe2O3 content 2%-4%, CaO content 8%-12%, MgO content 0.5%-1.5%; after the slag enters the plant, it is sent to a jaw crusher for crushing until all particles pass through a 3mm square hole sieve to obtain coarse slag powder, which is then sent to the slag batching silo for storage.
[0034] Step S2, Accurate Weighing and Ingredient Dispensing Based on the calculated dry basis mass ratio, the proportions of each component are set. The core proportion range of this invention is: 55-65 parts of low-calorific-value coal gangue coarse powder, 20-30 parts of dry carbide slag powder, 3-8 parts of microsilica powder, and 5-12 parts of slag coarse powder. The preferred proportion is: 60 parts of low-calorific-value coal gangue coarse powder, 25 parts of dry carbide slag powder, 5 parts of microsilica powder, and 10 parts of slag coarse powder. This proportion is determined based on the following considerations: coal gangue provides the main heat source as the basic calorific value component; the high-calcium component in carbide slag provides the calcium-based active sites required for sulfur fixation; microsilica powder provides combustion catalytic active centers and adjusts the ash composition with its ultra-large specific surface area; and slag supplements aluminous and siliceous components to regulate the melting temperature of the ash. Start the computer-controlled loss-in-weight automatic batching system and set the flow rate of the coal gangue coarse powder batching scale to [value missing]. The flow rate of the dry carbide slag batching scale is tons / hour. The flow rate of the silica powder batching scale is tons / hour. The flow rate of the slag coarse powder batching scale is tons / hour. tons / hour; the flow rate setpoints of each scale meet the requirements. : : : The overall ratio is 60:25:5:10, and the total feed amount is... The production capacity of subsequent molding and drying processes and the demand for alternative fuels in the kiln system are pre-set; the metering accuracy of each batching scale is controlled within ±1%; after the four materials are accurately weighed by their respective batching scales, they are simultaneously unloaded onto the converging belt conveyor through a fully enclosed screw feeder.
[0035] Step S3, Mixing and Homogenizing The belt conveyor feeds the four weighed materials from step S2 into a twin-shaft paddle-type forced mixing mixer. The mixer has a U-shaped cylinder with two opposing rotating mixing shafts inside, each equipped with a specially angled paddle. During mixing, atomized water is precisely sprayed using a metering pump through multiple atomizing nozzles installed at the top of the mixer cylinder. The amount of atomized water added is controlled to 12%-15% of the total mass of the mixed materials, preferably 13%-14%. The principle for controlling the amount of water is: the mixture should be able to clump together when grasped by hand, and disperse easily when lightly touched after being released. This ensures that the silica powder can fully adhere to the surface of other particles, while avoiding excessive moisture that could lead to difficulties in subsequent molding. The mixer is then turned on, with the two main shafts rotating in opposite directions at 200-300 rpm for 180-300 seconds, preferably 240 seconds. During mixing, the coarse particles of coal gangue and slag act as a carrier and framework, while the dry carbide slag acts as a calcareous matrix filling the space. The ultrafine silica powder, under the combined action of water molecules and mechanical stirring, evenly coats the surface of the coal gangue and slag particles, forming a homogenized wet material that is microscopically dispersed and macroscopically uniform. After mixing, the pneumatic gate at the bottom of the mixer is opened, unloading the homogenized wet material into the buffer hopper below.
[0036] Step S4: Extrusion granulation molding The homogenized wet material in the buffer hopper is evenly fed into the double-roller extrusion granulator via a variable frequency screw feeder. This granulator mainly consists of a pair of counter-rotating pressure rollers with hemispherical or oblong grooves on their surfaces. The extrusion pressure of the pressure rollers is set to 15-25 MPa, preferably 20 MPa. MPa; Under high pressure, the homogenized wet material is forced into the grooves on the surface of the pressure roller, and as the pressure roller rotates, it falls off in the release zone by its own gravity or with the assistance of a scraper, forming regularly shaped cylindrical or flattened spherical particles; the diameter of these particles is 8-15mm and the length is 10-25mm; the purpose of extrusion molding is to increase the bulk density and particle strength of the material through mechanical external force, improve its flowability, and facilitate subsequent drying and long-distance pneumatic conveying; at the same time, the formed particles have high compressive strength (≥50N / particle), and are not easily broken or pulverized during conveying and injection into the decomposition furnace, reducing dust generation; the formed particles are screened by a screening machine to remove powder with a particle size <5mm and oversized particles >30mm. The undersized powder and oversized large particles are crushed and returned to the extrusion granulator for re-forming, and the qualified particles enter the next process.
[0037] Step S5, Drying and Cooling The qualified shaped pellets obtained in step S4 are evenly fed into a mesh belt through-flow dryer via a plate feeder. The dryer has three or five mesh belt layers and adopts a stepped material distribution method. The drying heat source is taken from the waste heat air extracted from the middle section of the grate cooler at the kiln head of the cement kiln. The temperature range of this waste heat air is 250-350℃. It is introduced into the dryer through a hot air duct and passes through the mesh belt and material layer from bottom to top, directly contacting the shaped pellets for heat exchange. By adjusting the mesh belt speed and hot air volume, the moisture content of the shaped pellets at the dryer outlet is controlled to be ≤5%, preferably 3%-5%. The dried shaped pellets are discharged from the dryer outlet and sent to a fluidized bed cooler via a bucket elevator. The cooler is circulated with ambient temperature air to rapidly cool the dried hot pellets to ≤60℃ to prevent moisture re-entry and pellet softening due to residual heat. The cooled pellets are the finished alternative fuel and are sent to the finished product silo for storage and later use via a closed belt conveyor.
[0038] Step S6, pneumatic conveying and injection into the decomposition furnace The finished alternative fuel obtained in step S5 is discharged from the bottom of the finished product silo and fed into the pneumatic conveying pipeline through a rotary feed valve and a Venturi injector. The conveying medium of the pneumatic conveying system is compressed air or low-pressure air provided by a Roots blower, with a solid-to-gas ratio of 3-5 kg / kg and a conveying velocity of 18-25 km / h. m / s; the pipeline is laid along the preheater tower to the platform where the pulverized coal burner of the decomposition furnace is located; in the middle area of the decomposition furnace, there is an independent alternative fuel injection point; the alternative fuel is injected into the rising airflow inside the decomposition furnace in a dispersed state through a special spray gun; the spray gun has a multi-head swirl structure, which can evenly disperse the particle flow in the horizontal cross section and increase the contact area between the particles and the high-temperature tertiary air; according to the total heat consumption of the kiln system and the low heating value of the alternative fuel, the rotation speed of the rotary feed valve is adjusted through the central control system to control the feed rate of alternative fuel to 15%-25% of the total calorific value of the kiln system fuel, and the amount of alternative pulverized coal is 15%-25% of the total amount of pulverized coal; the alternative fuel ignites and burns out rapidly in the decomposition furnace environment of 900-1100℃, and the released heat is used for carbonate decomposition.
[0039] Step S7: System monitoring and dynamic adjustment to prevent blockage Thermocouple temperature sensors and pressure transmitters are installed in the flue gas chamber at the decomposition furnace outlet, the cone of the lowest cyclone (C5), and the feed pipe to monitor the temperatures t1 and t2 and the negative pressure P of the feed pipe in real time. The high limit alarm value of the C5 feed pipe temperature t2 is set to 845℃ and the high-high limit alarm value is set to 860℃ in the human-machine interface of the central control room. When the monitoring shows that t2 is continuously higher than 845℃ and shows an upward trend, the central control system automatically triggers the adjustment program: first, the rotation speed of the rotary feed valve of the alternative fuel is gradually reduced in increments of 0.5 tons / hour to reduce the feed rate. Simultaneously, through the frequency conversion adjustment of the silica fume scale in the batching system, the proportion of silica fume in the total ratio is increased by 0.5-1.0 percentage points (absolute content) within 30 seconds, while the slag ratio is simultaneously reduced by the same percentage point to maintain the total feed amount unchanged. This dynamic adjustment utilizes the ultra-high melting point (approximately 1610℃) of silica fume to rapidly increase the actual sintering temperature of the mixed ash entering the C5 system, causing the softened or semi-molten ash to re-solidify and inhibit further growth of the crust. When t2 drops back to below 835℃ and is maintained for 300 seconds, the system automatically restores to the initial ratio and feed amount. If t2 continues to rise to the high limit of 860℃, the system issues an audible and visual alarm and automatically interlocks to cut off the supply of alternative fuel, switching to 100% pulverized coal operation. After the temperature returns to normal and manual inspection and confirmation are completed, the feeding of alternative fuel is gradually restored.
[0040] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0041] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing alternative fuel for cement kilns using industrial waste residue, characterized in that, The method includes the following steps: Raw material pretreatment: Low-calorific-value coal gangue is crushed to a particle size of less than or equal to 5 mm to obtain coarse coal gangue powder; calcium carbide slag is dried to a moisture content of less than or equal to 2.0% to obtain dry calcium carbide slag powder; microsilica powder is selected; slag is crushed to a particle size of less than or equal to 3 mm to obtain coarse slag powder. Accurate weighing and batching: Weigh the four materials in the raw material pretreatment step according to the dry basis mass ratio, the ratio is: 55-65 parts of low calorific value coal gangue coarse powder, 20-30 parts of dry powdered carbide slag, 3-8 parts of microsilica powder, and 5-12 parts of slag coarse powder. Mixing and homogenization: The four weighed materials are fed into a forced mixing mixer. During the mixing process, atomized water is sprayed to control the total moisture content of the mixture to 12%-15%. The mixture is stirred for 180-300 seconds to obtain homogenized wet material. Extrusion granulation: The homogenized wet material is fed into a double-roller extrusion granulator and extruded under a pressure of 15-25 MPa to obtain shaped granules with a diameter of 8-15 mm and a length of 10-25 mm. Drying and cooling: The shaped pellets are fed into a dryer and dried with hot air at 250-350℃ until the moisture content is less than or equal to 5%, and then cooled to less than or equal to 60℃ to obtain the finished alternative fuel pellets; Pneumatic conveying and kiln feeding: The finished alternative fuel pellets are fed into the central area of the cement kiln decomposition furnace through a pneumatic conveying system for injection and combustion. The feed amount of alternative fuel is controlled to account for 15%-25% of the total calorific value of the kiln system fuel. System monitoring and dynamic adjustment: The temperature of the feed pipe of the lowest cyclone is monitored in real time. When the temperature of the feed pipe continues to be higher than 845℃, the feed amount of alternative fuel is automatically reduced, and the proportion of microsilica powder is increased by 0.5-1.0 percentage points until the temperature returns to normal.
2. The method for preparing alternative fuel for cement kilns using industrial waste residue according to claim 1, characterized in that, The low-calorific-value coal gangue mentioned in the raw material pretreatment step has a lower heating value of 1500-2200 kcal / kg and a loss on ignition of 3%-6%. Its chemical composition, by mass percentage, includes: SiO2 20%-30%, Al2O3 15%-25%, Fe2O3 1%-3%, and CaO 3%-8%.
3. The method for preparing alternative fuel for cement kilns using industrial waste residue according to claim 1, characterized in that, The dry basis chemical composition of the carbide slag mentioned in the raw material pretreatment step, by mass percentage, includes: loss on ignition 28%-32%, CaO≥60%, SiO2 3%-8%, Al2O3 1%-3%, Fe2O3 0.5%-1.5%, MgO≤0.5%.
4. The method for preparing alternative fuel for cement kilns using industrial waste residue according to claim 1, characterized in that, The microsilica powder in the raw material pretreatment step has a SiO2 content of ≥80%, a specific surface area of ≥15000 m² / kg, and a loss on ignition of ≤5%.
5. The method for preparing alternative fuel for cement kilns using industrial waste residue according to claim 1, characterized in that, The chemical composition of the slag mentioned in the raw material pretreatment step, by mass percentage, includes: loss on ignition 3%-7%, SiO2 40%-45%, Al2O3 30%-35%, Fe2O3 2%-4%, CaO 8%-12%, and MgO 0.5%-1.5%.
6. The method for preparing alternative fuel for cement kilns using industrial waste residue according to claim 1, characterized in that, The precise weighing and batching ratio of dry basis mass is as follows: 60 parts of low-calorific-value coal gangue coarse powder, 25 parts of dry carbide slag powder, 5 parts of microsilica powder, and 10 parts of slag coarse powder.
7. The method for preparing alternative fuel for cement kilns using industrial waste residue according to claim 1, characterized in that, The mixing spindle speed of the forced mixing machine in the mixing and homogenization process is 200-300 rpm, the mixing time is 240 seconds, and the amount of atomized water added is controlled to be 13%-14% of the total mass of the mixture.
8. A method for preparing alternative fuel for cement kilns using industrial waste residue according to claim 1, characterized in that, The dryer described in the drying and cooling section is a mesh belt through-flow dryer. The heat source is taken from the waste hot air of 250-350℃ extracted from the middle section of the grate cooler at the kiln head of the cement kiln. The dried shaped particles are cooled to ≤60℃ by a fluidized bed cooler.
9. A method for preparing alternative fuel for cement kilns using industrial waste residue according to claim 1, characterized in that, The solid-to-gas ratio of the pneumatic conveying to the kiln is 3-5 kg / kg, and the conveying wind speed is 18-25 m / s. The injection into the central area of the decomposition furnace adopts a multi-head swirl spray gun to make the alternative fuel particles uniformly dispersed in the cross section of the decomposition furnace.
10. A method for preparing alternative fuel for cement kilns using industrial waste residue according to claim 1, characterized in that, The highest alarm value for the temperature of the lowest-level cyclone feed pipe in the system monitoring and dynamic adjustment is 845℃, and the highest-highest alarm value is 860℃. When the temperature continues to be higher than 845℃, the feed rate of alternative fuel is reduced in increments of 0.5 tons / hour, and the proportion of microsilica powder is increased by 0.5-1.0 percentage points within 30 seconds, while the proportion of slag is reduced by the same percentage point to maintain the total feed rate unchanged. When the feed pipe temperature drops back to below 835℃ and is maintained for 300 seconds, it automatically returns to the initial proportion and feed rate. When the temperature reaches 860℃, the system automatically interlocks and cuts off the supply of alternative fuel, switching to 100% pulverized coal operation.