A silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials and its preparation method

A silica fume composite polydimethylsiloxane emulsion was prepared by combining silane-modified silica fume with wet ball milling and ultrasonic dispersion. This solved the problem of poor dispersibility of PDMS in cement-based materials and improved the hydrophobic and impermeable properties and maintained the strength of cement-based materials.

CN123106044APending Publication Date: 2026-11-17WUHAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611281800.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the prior art, polydimethylsiloxane (PDMS) has poor dispersibility in cement-based materials, which leads to the aggregation, floating and uneven dispersion of hydrophobic components, affecting the uniformity and long-term stability of the hydrophobic properties of cement-based materials, and may also cause strength loss.

Method used

A silica fume composite polydimethylsiloxane emulsion was prepared by wet ball milling of silane-modified silica fume with water and ultrasonic dispersion with polydimethylsiloxane. The silane-modified silica fume was depolymerized and dispersed by wet ball milling to form a dense particle layer for stable dispersion, avoiding oil droplet agglomeration and local enrichment.

Benefits of technology

Stable dispersion of silica fume composite polydimethylsiloxane emulsion was achieved in a high alkalinity and high ion concentration environment, which improved the hydrophobic and impermeable properties of cement-based materials and avoided strength loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106044A_ABST
    Figure CN123106044A_ABST
Patent Text Reader

Abstract

This invention discloses a silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials and its preparation method. The emulsion is obtained by further ultrasonically dispersing a silica fume slurry obtained by wet ball milling of silane-modified silica fume with water with polydimethylsiloxane. The silane-modified silica fume is silica fume modified with triethoxyoctylsilane and γ-aminopropyltriethoxysilane. The silica fume composite polydimethylsiloxane emulsion provided by this invention can be stably dispersed in cement pastes with high alkalinity, high ion concentration, and continuous hydration. After the cement paste hardens, it can improve the hydrophobic and impermeable properties of cement-based materials and avoid strength loss.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of using organic materials as effective components of mortar, concrete or artificial stone, and specifically relates to a silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials and its preparation method. Background Technology

[0002] Cement-based materials are widely used in building construction, transportation infrastructure, and underground engineering. However, the cement stone formed after cement paste hardens contains capillary pores, gel pores, and microcracks. Furthermore, the surface of hydration products is usually highly hydrophilic, allowing water and corrosive media such as chloride and sulfate ions to easily penetrate the material through the pores, causing freeze-thaw damage, steel corrosion, salt crystallization damage, and chemical corrosion, thereby reducing structural durability.

[0003] To improve the water resistance, impermeability, and durability of cement-based materials, existing methods mainly involve surface coating or internal admixture to modify the materials for hydrophobicity. Surface coating typically uses silanes, siloxanes, or organic resins to form a hydrophobic film on the material surface. However, this method has limited protective depth, the coating is prone to failure due to wear, UV aging, cracking, and environmental factors, and it is difficult to achieve overall hydrophobicity within the material.

[0004] Internal admixture involves directly adding hydrophobic agents to cement-based materials, distributing the hydrophobic components within the slurry. Polydimethylsiloxane (PDMS) possesses characteristics such as low surface energy, good chemical stability, and significant hydrophobic effects, making it a potential candidate for hydrophobic modification of cement-based materials. However, PDMS exhibits poor compatibility with cement-based systems, and direct incorporation can easily lead to agglomeration, floating, and uneven dispersion. Furthermore, PDMS may form a hydrophobic coating on the surface of cement particles or hydration products, hindering hydration reactions and interfacial bonding, resulting in deterioration of the pore structure and a decrease in compressive strength.

[0005] To improve the dispersibility of PDMS, existing technologies often use organic surfactants to prepare emulsions. However, cement paste is characterized by high alkalinity, high ion concentration, and continuous hydration. Conventional emulsions are prone to demulsification, flocculation, or oil droplet aggregation in this environment, resulting in local enrichment of hydrophobic components and affecting the uniformity and long-term stability of the hydrophobic properties of cementitious materials. In addition, some organic surfactants may also entrain air, retard setting, or interfere with cement hydration, adversely affecting the mechanical properties of the material.

[0006] Therefore, there is an urgent need to develop a composite emulsion that can maintain stable dispersion in a cement-based strong alkaline environment, achieve overall hydrophobic modification of the material, and reduce or suppress the strength loss caused by hydrophobic components. Summary of the Invention

[0007] The technical problem to be solved by the present invention is to address the above-mentioned deficiencies in the prior art by providing a silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials and its preparation method. The silica fume composite polydimethylsiloxane emulsion can be stably dispersed in cement paste with high alkalinity, high ion concentration and continuous hydration. After the cement paste hardens, it can improve the hydrophobic and impermeable properties of cement-based materials and avoid the loss of strength of cement-based materials.

[0008] The first aspect of this invention is to provide a silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials, which is obtained by further ultrasonically dispersing silica fume slurry obtained by wet ball milling of silane-modified silica fume with water with polydimethylsiloxane (PDMS). The silane-modified silica fume is obtained by modifying triethoxyoctylsilane (JH-N308) and γ-aminopropyltriethoxysilane (KH-550). JH-N308 contains long-chain alkyl groups, which can impart hydrophobicity to the silica fume, but it has large steric hindrance and low grafting efficiency. KH-550 has low steric hindrance, promotes grafting, and the amino groups are negatively charged, which improves the dispersion effect of encapsulating the weakly positively charged PDMS.

[0009] The second aspect of this invention includes the preparation method of the above-mentioned silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials, the specific steps of which are as follows: 1) Preparation of silane-modified silica fume: Triethoxyoctylsilane, γ-aminopropyltriethoxysilane, water and anhydrous ethanol are mixed, the pH value is adjusted to 4.0-5.5, and the mixture is stirred to hydrolyze the silane to obtain a bissilane hydrolysate. Then, the obtained bissilane hydrolysate is slowly added to the silica fume ethanol dispersion at 60-70℃ to carry out a dehydration condensation reaction. After post-treatment, silane-modified silica fume is obtained. 2) Preparation of silica fume slurry: The silane-modified silica fume obtained in step 1) is mixed with water and wet ball milled to obtain silica fume slurry; 3) Preparation of silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials: Polydimethylsiloxane is added to the silica fume slurry obtained in step 2), and ultrasonic emulsification is performed to obtain silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials.

[0010] According to the above scheme, the mass ratio of triethoxyoctylsilane, γ-aminopropyltriethoxysilane, water and anhydrous ethanol in step 1) is 0.60-0.72:0.20-0.24:0.25:2.

[0011] According to the above scheme, the silica fume ethanol dispersion in step 1) is obtained by mixing silica fume and anhydrous ethanol at a mass ratio of 12.5-15:100 and then ultrasonically dispersing them.

[0012] According to the above scheme, the average particle size of the silica fume in step 1) is 0.1-0.3μm.

[0013] According to the above scheme, the bissilane hydrolysate and silica fume ethanol dispersion in step 1) are mixed at a mass ratio of 3.05-3.2:100.

[0014] According to the above scheme, the dehydration condensation reaction temperature in step 1) is room temperature (15-35℃), and the reaction time is 3-5h.

[0015] According to the above scheme, in step 2), the mass ratio of silane-modified silica fume to water is 1:3-8.

[0016] According to the above scheme, the wet ball milling process conditions in step 2) are: a ball milling media to material mass ratio of 3-8:1, a ball milling speed of 300-800 rpm, and a ball milling time of 0.5-3 h. In this invention, wet ball milling is a key step in achieving stable emulsion dispersion. On the one hand, the bissilane modification changes the silica fume surface from hydrophilic to hydrophobic, making it difficult to wet directly with water, causing it to float and agglomerate, and failing to form a uniform dispersion system. During subsequent emulsification, the particles cannot effectively migrate to the oil-water interface, leading to the failure of particle-stabilized emulsion construction. On the other hand, after drying, the silane-modified silica fume produces obvious hard agglomerates with particle sizes much larger than the original size, significantly reducing interfacial activity and making it impossible to form a dense coating layer on the PDMS oil droplet surface, thus making it difficult to inhibit oil droplet aggregation. Therefore, wet ball milling is used to deagglomerate and disperse the silane-modified silica fume, restoring it to a suitable fineness and uniformly dispersing it in the aqueous phase, ensuring that it can be rapidly and directionally adsorbed at the oil-water interface and form a stable particle layer during ultrasonic emulsification.

[0017] According to the above scheme, the polydimethylsiloxane in step 3) is a hydroxyl-terminated polydimethylsiloxane with a kinematic viscosity of 10-100 cSt.

[0018] According to the above scheme, the mass ratio of silica ash slurry to polydimethylsiloxane in step 3) is 1.5-4:1.

[0019] According to the above scheme, the ultrasonic emulsification process conditions for step 3) are as follows: ultrasonic emulsification temperature is 0-5℃, ultrasonic frequency is 20-40kHz, ultrasonic power is 300-800W, and ultrasonic time is 5-30min.

[0020] The third aspect of the present invention includes the application of the above-mentioned silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials in mortar, concrete or artificial stone.

[0021] According to the above scheme, the specific usage method is as follows: after mixing the silica fume composite polydimethylsiloxane emulsion used for hydrophobic modification of cement-based materials with mixing water, it is added to the cement paste. The dosage of polydimethylsiloxane is 1.0-3.0% of the mass of cementitious material.

[0022] Silica fume is an ultrafine mineral admixture with amorphous silica as its main component. It has a high specific surface area and pozzolanic activity. However, unmodified silica fume has a strong hydrophilic surface, making it difficult to stably adsorb between PDMS oil droplets and the aqueous phase. Therefore, it cannot be directly used as an effective particle emulsion stabilizer. This invention is based on the particle-stabilized emulsion mechanism. First, two silanes are selected to modify silica fume, changing it from hydrophilic to hydrophobic. Then, wet ball milling is performed to deagglomerate the dried and agglomerated modified silica fume, refine the particle size, and uniformly disperse it in the aqueous phase. The resulting silica fume slurry is ultrasonically emulsified with PDMS. The modified silica fume particles rapidly migrate to the water-PDMS oil droplet interface and form a dense particle layer, which can inhibit oil droplet aggregation, flotation, and local enrichment, and improve the stability of the emulsion in the strong alkaline and high ion concentration environment of cement paste.

[0023] The beneficial effects of this invention are as follows: 1. The silica fume composite polydimethylsiloxane emulsion provided by this invention can be stably dispersed in cement paste with high alkalinity, high ion concentration, and continuous hydration. After the cement paste hardens, it can improve the hydrophobic and impermeable properties of cement-based materials and avoid strength loss. 2. The preparation method of this invention is simple, the raw materials are widely available, and it adopts conventional processes such as hydrolysis modification, wet ball milling, and ultrasonic emulsification. The parameters are clear and highly controllable, making it suitable for cement-based engineering materials with high requirements for waterproofing, impermeability, corrosion resistance, and durability. Attached Figure Description

[0024] Figure 1 This is a schematic diagram of the microstructure of the silica fume composite polydimethylsiloxane emulsion used for hydrophobic modification of cement-based materials in Example 1 of the present invention. Detailed Implementation

[0025] To enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings.

[0026] Example 1 A silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials (microstructure schematic diagram shown) Figure 1 As shown in the figure, the specific steps of its preparation method are as follows: 1) Preparation of silane-modified silica fume: Triethoxyoctylsilane, γ-aminopropyltriethoxysilane, water and anhydrous ethanol were mixed in a mass ratio of 0.60:0.20:0.25:2. The pH was adjusted to 4.5 with dilute acid and stirred for 30 min to hydrolyze the silane to obtain a bissilane hydrolysate. Silica fume (average particle size 0.1-0.3 μm) and anhydrous ethanol were mixed in a mass ratio of 15:100 and ultrasonically dispersed to obtain a silica fume-ethanol dispersion. At 60℃, the bissilane hydrolysate was added dropwise to the silica fume-ethanol dispersion (the mass ratio of the bissilane hydrolysate to the silica fume-ethanol dispersion was 3.1:100). The total mass of triethoxyoctylsilane and γ-aminopropyltriethoxysilane was controlled to be 5.3% of the silica fume mass. After the addition was complete, the reaction was continued at room temperature (25℃) for 3 h. After the reaction was completed, the silica fume was washed with anhydrous ethanol, filtered, and dried at 60℃ to constant weight to obtain silane-modified silica fume. 2) Preparation of silica fume slurry: The silane-modified silica fume obtained in step 1) is mixed with water at a mass ratio of 1:5. Corundum balls are used as the ball milling medium, and the mass ratio of the ball milling medium to the material is 5:1. The mixture is wet-milled at 500 rpm for 1 hour to obtain silica fume slurry. 3) Ultrasonic emulsification: Hydroxyl-terminated polydimethylsiloxane (kinematic viscosity of 25 cSt) is added to the silica fume slurry obtained in step 2), and the mass ratio of silica fume slurry to polydimethylsiloxane is controlled at 2.0:1. Ultrasonic emulsification is carried out for 10 minutes at a frequency of 25 kHz and a power of 500 W under ice bath conditions to obtain silica fume composite polydimethylsiloxane emulsion.

[0027] The emulsion prepared in this embodiment has a uniform milky white appearance and shows no stratification or floating oil after standing for 24 hours. 1 mL of the emulsion was diluted in 10 mL of saturated Ca(OH)₂ solution (pH ≈ 12.5), and after standing for 30 min, it remained uniformly milky white, with no obvious demulsification, flocculation, or oil droplet floating, indicating that the particulate stabilizing layer imparts excellent alkali and salt resistance to the emulsion.

[0028] The emulsion of this embodiment was incorporated into ordinary Portland cement (P·O42.5) at a PDMS content of 1.0% of the cementitious material mass, and mixing water was added (water-cement ratio controlled at 0.4). After standard curing for 28 days, performance tests were conducted: the surface water contact angle was 122°, the 24-hour water absorption rate was 6.2%, which was 59.5% lower than the blank group without emulsion (15.3%); the 28-day compressive strength was 41.8 MPa, which was 10.5% lower than the strength loss rate of the blank group (46.7 MPa).

[0029] Example 2 A silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials, the specific steps of its preparation are as follows: 1) Preparation of silane-modified silica fume: Triethoxyoctylsilane, γ-aminopropyltriethoxysilane, water and anhydrous ethanol were mixed in a mass ratio of 0.72:0.24:0.25:2. The pH was adjusted to 5.5 with dilute acid and stirred for 40 min to hydrolyze the silane to obtain a bissilane hydrolysate. Silica fume (average particle size 0.1-0.3 μm) and anhydrous ethanol were mixed in a mass ratio of 15:100 and ultrasonically dispersed to obtain a silica fume-ethanol dispersion. At 70℃, the bissilane hydrolysate was added dropwise to the silica fume-ethanol dispersion (the mass ratio of the bissilane hydrolysate to the silica fume-ethanol dispersion was 3.2:100). The total mass of triethoxyoctylsilane and γ-aminopropyltriethoxysilane was controlled to be 6.4% of the silica fume mass. After the addition was complete, the reaction was continued at room temperature (25℃) for 4 h. After the reaction was completed, the silica fume was washed with anhydrous ethanol, filtered, and dried at 60℃ to constant weight to obtain silane-modified silica fume. 2) Preparation of silica fume slurry: The silane-modified silica fume obtained in step 1) is mixed with water at a mass ratio of 1:6. Corundum balls are used as the ball milling medium, and the mass ratio of the ball milling medium to the material is 5:1. The mixture is wet-milled at 500 rpm for 1 hour to obtain silica fume slurry. 3) Ultrasonic emulsification: Hydroxyl-terminated polydimethylsiloxane (kinematic viscosity of 25 cSt) is added to the silica fume slurry obtained in step 2), and the mass ratio of silica fume slurry to polydimethylsiloxane is controlled at 2.5:1. Ultrasonic emulsification is carried out for 10 minutes at a frequency of 25 kHz and a power of 500 W under ice bath conditions to obtain silica fume composite polydimethylsiloxane emulsion.

[0030] The emulsion prepared in this embodiment has a uniform milky white appearance and shows no stratification or floating oil after standing for 24 hours. It remains stable after being diluted in a saturated Ca(OH)₂ solution and standing for 30 minutes, without any demulsification or flocculation.

[0031] The emulsion of this embodiment was added to ordinary Portland cement (P·O42.5) at a PDMS content of 3.0% of the cementitious material mass, and mixing water was added (water-cement ratio controlled at 0.4). After standard curing for 28 days, performance tests were conducted: the surface water contact angle was 130°, the 24-hour water absorption rate was 4.3%, which was 71.9% lower than the control group (15.3%); the 28-day compressive strength was 38.8 MPa, which was 16.9% lower than the strength loss rate of the control group (46.7 MPa).

[0032] Example 3 A silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials, the specific steps of its preparation are as follows: 1) Preparation of silane-modified silica fume: Triethoxyoctylsilane, γ-aminopropyltriethoxysilane, water, and anhydrous ethanol were mixed in a mass ratio of 0.66:0.22:0.25:2. The pH was adjusted to 4.8 with dilute acid, and the mixture was stirred for 30 minutes. Silane was hydrolyzed to obtain a bissilane hydrolysate. Silica fume (average particle size 0.1-0.3 μm) and anhydrous ethanol were mixed at a mass ratio of 13.6:100 and ultrasonically dispersed to obtain a silica fume-ethanol dispersion. The bissilane hydrolysate was added dropwise to the silica fume-ethanol dispersion at 65°C (mass ratio of bissilane hydrolysate to silica fume-ethanol dispersion was 3.15:100). The total mass of triethoxyoctylsilane and γ-aminopropyltriethoxysilane was controlled to be 10.0% of the silica fume mass. After the addition was complete, the reaction was continued at room temperature (25°C) for 4 hours. After the reaction was completed, the silica fume was washed with anhydrous ethanol, filtered, and dried at 60°C to constant weight to obtain silane-modified silica fume. 2) Preparation of silica fume slurry: The silane-modified silica fume obtained in step 1) is mixed with water at a mass ratio of 1:5. Corundum balls are used as the ball milling medium, and the mass ratio of the ball milling medium to the material is 5:1. The mixture is wet-milled at 500 rpm for 1.5 h to obtain silica fume slurry. 3) Ultrasonic emulsification: Hydroxyl-terminated polydimethylsiloxane (kinematic viscosity of 50 cSt) is added to the silica fume slurry obtained in step 2), and the mass ratio of silica fume slurry to polydimethylsiloxane is controlled at 2.5:1. Ultrasonic emulsification is carried out for 15 minutes at a frequency of 30 kHz and a power of 600 W under ice bath conditions to obtain silica fume composite polydimethylsiloxane emulsion.

[0033] The emulsion prepared in this embodiment has a uniform milky white appearance and shows no stratification or floating oil after standing for 24 hours. It remains stable after being diluted in a saturated Ca(OH)₂ solution and standing for 30 minutes, without any demulsification or flocculation.

[0034] The emulsion of this embodiment was added to ordinary Portland cement (P·O42.5) at a PDMS content of 2.0% of the cementitious material mass, and mixing water was added (water-cement ratio controlled at 0.4). After standard curing for 28 days, performance tests were conducted: the surface water contact angle was 132°, the 24-hour water absorption rate was 4.6%, which was 69.9% lower than the control group (15.3%); the 28-day compressive strength was 40.8 MPa, which was 12.6% lower than the strength loss rate of the control group (46.7 MPa).

[0035] Comparative Example 1 This comparative example directly incorporates hydroxyl-terminated polydimethylsiloxane without any particle stabilization treatment into cement-based materials. The specific steps are as follows: Take the same hydroxyl-terminated polydimethylsiloxane (kinematic viscosity of 25 cSt) as in Example 2, without any silica fume particle stabilization treatment, add PDMS to ordinary Portland cement (P·O42.5) at a mass of 3.0% of the cementitious material, add mixing water (water-cement ratio controlled at 0.4), mix and mold, and then cure for 28 days under standard conditions.

[0036] In this comparative example, PDMS was observed to float on the slurry surface as oily droplets during the mixing process, failing to disperse evenly. After 28 days of standard curing, the surface water contact angle was only 107°, and the 24-hour water absorption rate was 9.1%, only 40.5% lower than the control group. The 28-day compressive strength was 35.2 MPa, a 24.6% decrease compared to the control group (46.7 MPa). This indicates that the direct incorporation of unstabilized PDMS not only results in poor hydrophobicity but also significantly damages mechanical properties.

[0037] Comparative Example 2 A silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials, compared with Example 1, involves directly emulsifying silane-modified silica fume that has not undergone wet ball milling with PDMS. The specific steps of its preparation method are as follows: 1) Preparation of silane-modified silica fume: exactly the same as step 1) in Example 1; 2) Emulsification without ball milling: The silane-modified silica fume obtained in step 1) is mixed with water at a mass ratio of 1:5. Hydroxyl-terminated polydimethylsiloxane (kinematic viscosity of 25 cSt) is added directly without wet ball milling. The mass ratio of the silica fume and water mixture to PDMS is controlled at 2.0:1. The mixture is ultrasonically emulsified for 10 min at a frequency of 25 kHz and a power of 500 W under ice bath conditions.

[0038] In this comparative example, during the ultrasonic emulsification process in step 2), a large amount of silane-modified silica fume powder floated on the liquid surface and could not effectively penetrate into the aqueous phase. The resulting mixture exhibited a clear stratification state, with the upper layer consisting of floating hydrophobic silica fume aggregates and the lower layer being the aqueous phase, failing to form a homogeneous emulsion. Upon dilution in a saturated Ca(OH)₂ solution, it rapidly stratified, lacking emulsion stability.

[0039] The emulsion prepared in this comparative example (only the upper floating oil portion was used) was added to ordinary Portland cement (P·O42.5) at a PDMS content of 1.0% of the cementitious material mass, and mixing water was added (the water-cement ratio was controlled at 0.4). After standard curing for 28 days, the test results are as follows: the surface water contact angle was 112°, the 24-hour water absorption rate was 8.9%, which was only 41.8% lower than the control group; the 28-day compressive strength was 36.8 MPa, which was 21.2% lower than the strength loss rate of the control group (46.7 MPa).

[0040] It should be understood that those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.

Claims

1. A silica-fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials, characterized in that, It is obtained by further ultrasonically dispersing the silica slurry obtained by wet ball milling of silane-modified silica ash and water with polydimethylsiloxane; The silane-modified silica fume is silica fume obtained by modifying triethoxyoctylsilane and γ-aminopropyltriethoxysilane.

2. A process for the preparation of a silica-fume composite polydimethylsiloxane emulsion for hydrophobic modification of cementitious materials as claimed in claim 1, characterized in that, The specific steps are as follows: 1) Preparation of silane-modified silica fume: Triethoxyoctylsilane, γ-aminopropyltriethoxysilane, water and anhydrous ethanol are mixed, the pH value is adjusted to 4.0-5.5, and the mixture is stirred to hydrolyze the silane to obtain a bissilane hydrolysate. Then, the obtained bissilane hydrolysate is slowly added to the silica fume ethanol dispersion at 60-70℃ to carry out a dehydration condensation reaction. After post-treatment, silane-modified silica fume is obtained. 2) Preparation of silica fume slurry: The silane-modified silica fume obtained in step 1) is mixed with water and wet ball milled to obtain silica fume slurry; 3) Preparation of silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials: Polydimethylsiloxane is added to the silica fume slurry obtained in step 2), and ultrasonic emulsification is performed to obtain silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials.

3. The method for preparing a silica ash composite polydimethylsiloxane emulsion for hydrophobic modification of cementitious materials according to claim 2, characterized in that, The mass ratio of triethoxyoctylsilane, γ-aminopropyltriethoxysilane, water and anhydrous ethanol in step 1) is 0.60-0.72:0.20-0.24:0.25:2; the silica fume ethanol dispersion in step 1) is obtained by mixing silica fume and anhydrous ethanol at a mass ratio of 12.5-15:100 and then ultrasonically dispersing them.

4. The method for preparing the silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials according to claim 2, characterized in that, The average particle size of the silica fume in step 1) is 0.1-0.3 μm; the bissilane hydrolysate and the silica fume ethanol dispersion in step 1) are mixed at a mass ratio of 3.05-3.2:

100.

5. The method for preparing the silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials according to claim 2, characterized in that, Step 1) The dehydration condensation reaction is carried out at room temperature for 3-5 hours.

6. The method for preparing the silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials according to claim 2, characterized in that, Step 2) The mass ratio of silane-modified silica fume to water is 1:3-8; Step 2) The wet ball milling process conditions are: the mass ratio of ball milling media to material is 3-8:1, the ball milling speed is 300-800 rpm, and the ball milling time is 0.5-3h.

7. The method for preparing the silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials according to claim 2, characterized in that, Step 3) The polydimethylsiloxane is hydroxyl-terminated polydimethylsiloxane with a kinematic viscosity of 10-100 cSt; Step 3) The mass ratio of silica slurry to polydimethylsiloxane is 1.5-4:

1.

8. The method for preparing the silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials according to claim 2, characterized in that, Step 3) The ultrasonic emulsification process conditions are as follows: ultrasonic emulsification temperature is 0-5℃, ultrasonic frequency is 20-40kHz, ultrasonic power is 300-800W, and ultrasonic time is 5-30min.

9. The application of the silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials according to claim 1 in mortar, concrete or artificial stone.

10. The application of the silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials according to claim 9 in mortar, concrete, or artificial stone, characterized in that, The specific method of use is as follows: after mixing the silica fume composite polydimethylsiloxane emulsion for hydrophobic modification of cement-based materials with mixing water, it is added to the cement paste. The dosage of polydimethylsiloxane is 1.0-3.0% of the mass of cementitious material.