A mine filling material based on molybdenum tailings-fly ash synergistic solidification and a preparation method and application thereof
By synergistically solidifying molybdenum tailings and fly ash, a composite activation system is constructed to activate their potential gelling activity and form a CASH gel network. This solves the problems of low resource utilization rate of fly ash and molybdenum tailings and high cost of traditional cement-based materials, achieving efficient heavy metal solidification and long-term material stability, and meeting the engineering requirements of mine backfilling.
Patent Information
- Application Number
- CN202611522931.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, the utilization rate of fly ash from municipal solid waste incineration and molybdenum tailings is low, traditional cement-based backfill materials are costly and have high carbon emissions, single solid waste backfill bodies have poor long-term stability in harsh environments, and the solidification effect of heavy metals is not ideal.
By scientifically proportioning molybdenum tailings and fly ash, a composite activation system is constructed to activate their potential cementing activity, forming a CASH gel network to achieve long-term stabilization of heavy metals and soluble salts. Molybdenum tailings provide a siliceous framework, fly ash introduces an aluminum phase and auxiliary cementing components, slag powder/fly ash serves as a highly active precursor, carbide slag and red mud constitute a composite alkaline activation system, gypsum provides a sulfate activation environment, and waste glass powder/aluminum ash serves as a silicon-aluminum fine-tuning component. This optimizes the material system to reduce costs and improve mechanical properties.
It achieves efficient solidification of heavy metals, reduces the preparation cost of filling materials, meets the stringent requirements of mine filling for material strength and deformation characteristics, significantly improves the long-term durability and compressive strength of materials, reduces the risk of pipe blockage, and meets the engineering requirements of mine filling.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of solid waste resource utilization and mine backfill materials, specifically relating to a fly ash co-solidification mine backfill material based on molybdenum tailings, its preparation method, and its application. Background Technology
[0002] With the acceleration of urbanization, the output of fly ash from municipal solid waste incineration has been increasing year by year. Fly ash contains high concentrations of heavy metals, chlorides, dioxins, and other pollutants, and is classified as hazardous waste. Currently, the mainstream treatment method in the industry is cement solidification and landfill, but this method suffers from problems such as large volume increase, poor long-term stability, and high carbon emissions. To overcome the drawbacks of cement solidification, the industry has explored various alternative technologies in recent years, including alkali activation, low-temperature pyrolysis, high-temperature sintering, and carbonation curing. However, alkali activation technology has stringent requirements for the silicon and aluminum composition of raw materials and often faces problems such as efflorescence and shrinkage cracking; while pyrolysis or sintering technologies can completely decompose dioxins, they consume extremely high energy and are economically unfeasible; carbonation curing is limited by the CO2 diffusion rate, making it difficult to achieve deep solidification of large-volume components. These technologies generally suffer from bottlenecks such as complex process routes, large equipment investment, high operating costs, and the curing effect being greatly affected by fluctuations in operating conditions, making it difficult to achieve large-scale, low-cost resource utilization of fly ash.
[0003] Meanwhile, molybdenum tailings, a large amount of solid waste generated by the molybdenum mining and beneficiation industry, also faces severe disposal challenges. Molybdenum tailings are typically fine-grained waste slag mainly composed of silicate minerals such as quartz, feldspar, and mica. Not only are their stockpiles enormous, occupying vast amounts of land resources, but the trace heavy metals they contain are also highly susceptible to migration under rainwater leaching and oxidation, posing a potential ecological and environmental risk to surrounding soil and groundwater. Currently, the main disposal methods for molybdenum tailings are stockpiling, landfilling, or use as aggregate for mine backfill. However, due to the extremely low cementing activity of molybdenum tailings, their use as backfill material requires a large amount of high-grade cement as an alkaline activator and cementing phase. This not only leads to high backfill costs (cementing material costs typically account for more than 60% of the total backfill cost) but also limits the overall amount of tailings that can be incorporated, making large-scale disposal difficult.
[0004] In the field of solid waste-based backfill materials, while existing technologies have made preliminary attempts to use single tailings or fly ash to prepare backfill materials, most are limited to the independent utilization of single solid wastes. This utilization method fails to fully explore the chemical synergistic effects between different solid wastes, resulting in limited material performance. Especially under harsh service environments such as high humidity, rich salt ions, or alternating wet and dry conditions, the matrix is prone to interfacial delamination and chemical erosion due to the lack of effective chemical bonding and microstructure control, leading to a decline in mechanical properties and a significant reduction in the coating and solidification effects on heavy metals. This makes it difficult to meet the stringent requirements of modern green mine backfill for both engineering mechanical strength and environmental safety.
[0005] Therefore, based on the aforementioned technical challenges, how to cleverly utilize the complementary chemical composition of molybdenum tailings and municipal solid waste incineration fly ash, and through specific process design to stimulate the synergistic cementing effect between the two, to develop a high-performance mine backfill material with simple process, high curing efficiency, excellent mechanical properties, and the ability to achieve long-term stabilization of heavy metals, has become a key technical problem that urgently needs to be solved in the current intersection of environmental protection and mining engineering. Summary of the Invention
[0006] In view of the many shortcomings of the existing technology, the present invention aims to provide a mine backfill material based on the synergistic solidification of molybdenum tailings and fly ash, so as to solve the technical problems in the existing technology, such as the low resource utilization rate of fly ash and molybdenum tailings, the high cost of traditional cement-based backfill materials, the large carbon emissions, the poor long-term stability of single solid waste backfill bodies in harsh environments, and the unsatisfactory solidification effect of heavy metals. This invention achieves efficient synergistic solidification of molybdenum tailings and fly ash through scientific formulation, enabling physical-chemical synergy at the microscopic level (such as volcanic ash reaction, ion exchange, and chemical bonding) to achieve long-term stable solidification of heavy metals and soluble salts in fly ash. By constructing a composite activation system, the potential cementitious activity of molybdenum tailings and fly ash is deeply activated, allowing industrial solid waste to completely or largely replace traditional high-energy-consuming and high-carbon-emission cement, significantly reducing the preparation cost of backfill materials. By optimizing the material system, the prepared backfill material can maintain excellent mechanical properties (such as compressive strength) and long-term durability under complex and harsh service environments such as high humidity, high salt content, and alternating wet and dry conditions, meeting the stringent requirements of modern mine backfilling mining processes for material strength and deformation characteristics.
[0007] In addition, the present invention also provides a method for preparing and applying mine backfill materials.
[0008] To solve the above-mentioned technical problems, the present invention provides the following technical solutions:
[0009] A mine backfill material based on the synergistic solidification of molybdenum tailings and fly ash comprises the following raw material components in parts by weight:
[0010] 100 portions of molybdenum tailings;
[0011] 10-30 parts fly ash;
[0012] 10-20 parts of gelling component;
[0013] The gelling components include mineral admixtures, composite alkaline activators, sulfate activators, and silica-alumina active admixtures, wherein the mass ratio of the mineral admixtures to the composite alkaline activators, sulfate activators, and silica-alumina active admixtures is 60-80:5-15:5-15:5-15.
[0014] In a preferred embodiment of the present invention, the molybdenum tailings are ball-milled and sieved after high-temperature calcination, with a sieve aperture of 60-100 mesh. Specifically, the process includes the following steps: placing the molybdenum tailings raw material in a ball mill for grinding, controlling the ball-to-material ratio at 2:1, and grinding for 40 minutes; placing the ground molybdenum tailings powder in a high-temperature furnace and calcining it at 800-850℃; after calcination, allowing it to cool naturally, and then sieving to obtain activated molybdenum tailings powder. Preferably, the calcination temperature is controlled at 850℃.
[0015] In a preferred embodiment of the present invention, the fly ash undergoes pyrolysis to remove residual organic pollutants, resulting in a particle size of less than 0.25 mm. Specifically, the process includes the following steps: the fly ash undergoes staged pyrolysis under an inert atmosphere, controlling the oxygen content to be below 1%, followed by sequential dehydration at 100-200℃ for 10-30 min, polycrystalline transformation at 480-670℃ for 1-2 h, and melting at 1101-1244℃. After these three temperature treatments, the fly ash is cooled and ground to a particle size of less than 0.25 mm to obtain pretreated fly ash micro powder.
[0016] In a preferred embodiment of the present invention, the mass ratio of the mineral admixture to the composite alkaline activator, sulfate activator, and silica-alumina active admixture is 70:10:10:10.
[0017] In a preferred embodiment of the present invention, the mineral admixture is selected from one or more of slag powder and fly ash. Preferably, the mineral admixture is composed of slag powder and fly ash, and the mass ratio of slag powder to fly ash is 50-70:5-15, more preferably 60:10.
[0018] Specifically, the slag powder is selected from S95 and S105 grade granulated blast furnace slag powder. Blast furnace slag powder has high glass content, high fineness, and high chemical stability, which can optimize particle size distribution and promote a balanced improvement in the early and later strength of the cementitious system.
[0019] Specifically, the fly ash is Class F, Grade I fly ash. The fly ash is rich in glassy aluminosilicate microspheres, possessing a triple function of pozzolanic effect, micro-aggregate effect, and morphological effect. The active Al2O3 component can chemically bond with heavy metal ions in the fly ash, assisting in the stabilization of heavy metals.
[0020] In a preferred embodiment of the present invention, the composite alkaline activator is composed of carbide slag and red mud, wherein the mass ratio of carbide slag to red mud is 5-7:3-5, preferably 5:5. Carbide slag, as a rapid alkaline activator, can quickly provide a high concentration of OH-. -Ions activate the early hydration of mineral admixtures such as slag powder; red mud, as a slow-release alkaline activator, contains alkali metal compounds that can slowly release alkalinity to maintain the mid-to-late stage hydration reaction. The two work together to achieve a combination of rapid early activation and continuous late activation, ensuring a balanced increase in the early and late strength of the filling body.
[0021] Specifically, the carbide slag is made of 200-mesh particles with a moisture content of less than 5% and an effective Ca(OH)2 content of more than 60%.
[0022] Specifically, the red mud is a highly alkaline solid waste generated during the Bayer process for alumina production. After being naturally air-dried, the red mud is milled and passed through a 0.15mm sieve (approximately 100 mesh). Its chemical composition shows that the Na2O content is ≥10%, the Al2O3 content is ≥15%, and the Fe2O3 content is ≥30%.
[0023] In a preferred embodiment of the present invention, the sulfate activator is gypsum.
[0024] Specifically, the gypsum is selected from one or more of desulfurized gypsum and fluorogypsum. The desulfurized gypsum is made of 200-mesh granules and can provide SO4. 2- The fluorinated gypsum ions react with the aluminum and calcium phases to form ettringite (AFt), which fills the pores and acts as a skeletal support, thereby enhancing early strength. It also achieves chemical stability of heavy metal ions. The fluorinated gypsum is in the form of 200-mesh particles.
[0025] In a preferred embodiment of the present invention, the silica-alumina active admixture is selected from one or more of waste glass powder and aluminum ash. Preferably, the silica-alumina active admixture is composed of waste glass powder and aluminum ash, wherein the mass ratio of waste glass powder to aluminum ash is 3-7:3-7, and more preferably 5:5. The combined use of these two materials can adjust the Si / Al ratio of the system to an optimal window of 1.5-3.0 and the Ca / Si ratio to 0.8-1.2, thereby achieving directional optimization of the gel phase composition.
[0026] Specifically, the waste glass powder is sodium-calcium-silicon waste glass powder with a fineness of less than 30 μm. Its main chemical composition is SiO2 (70%-75%), Na2O (5%-12%) and CaO (8%-12%). Its high silicon and low calcium characteristics can adjust the Ca / Si ratio of the system and guide the formation of low calcium-silicon ratio CASH gel. The resulting gel phase has higher density, which effectively improves the impermeability and long-term stability of the material.
[0027] Specifically, the aluminum ash is secondary aluminum ash, which passes through a 200-mesh sieve. Its main chemical composition is Al2O3 (40%-60%) and metallic aluminum (5%-15%). Its high aluminum properties can adjust the Si / Al ratio of the system and promote the formation of NASH and CASH gels.
[0028] A method for preparing mine backfill material includes the following steps:
[0029] Mineral admixtures, composite alkaline activators, sulfate activators, and silica-alumina active admixtures are mixed in proportion (stirred evenly for 5-10 minutes) to obtain the gelling components;
[0030] Molybdenum tailings, fly ash, and cementing components are mixed in a certain proportion (dry mixing for 3-5 minutes) to obtain mine backfill material.
[0031] In a preferred embodiment of the present invention, the molybdenum tailings are ball-milled and sieved after high-temperature calcination, with a sieve aperture of 60-100 mesh. The specific operation is the same as above.
[0032] In a preferred embodiment of the present invention, the fly ash undergoes pyrolysis to remove residual organic pollutants, resulting in a particle size of less than 0.25 mm. The specific operation is the same as described above.
[0033] Application of a mine backfill material in backfilling mine goaf areas.
[0034] As a preferred embodiment of the present invention, the application includes:
[0035] Water is added to the mine backfill material at a water-to-solid ratio of 0.3-0.5, and the mixture is stirred to produce a backfill slurry.
[0036] The filling slurry is injected into the goaf of the mine and then solidified.
[0037] The beneficial effects of this invention are:
[0038] This invention uses typical industrial solid wastes such as molybdenum tailings, municipal solid waste incineration fly ash, granulated blast furnace slag powder / fly ash, carbide slag, red mud, gypsum, and sodium-calcium-silicon waste glass powder / aluminum ash as core raw materials, with a total solid waste content exceeding 95%. The various solid waste components are chemically complementary: molybdenum tailings provide a siliceous framework, fly ash introduces the aluminum phase and auxiliary cementing components, slag powder / fly ash serves as a highly active precursor, carbide slag and red mud form a composite alkaline activation system, gypsum provides a sulfate activation environment, and waste glass powder / aluminum ash acts as a silicon-aluminum fine-tuning component. This formulation not only provides a large-scale, high-value-added disposal method for solid waste from multiple industrial chains, effectively alleviating the land occupation and environmental pollution problems caused by solid waste stockpiling, but also boasts extremely low raw material procurement costs; estimated overall raw material costs are far lower than traditional cement-based filling cementitious materials.
[0039] This invention utilizes a synergistic solidification mechanism of molybdenum tailings and fly ash. Through multiple solidification pathways—physical encapsulation by CASH gel, solid solution in the ettringite lattice, and chemical bonding of the Afm phase (single-carbon hydrated calcium sulfoaluminate) formed by active Al2O3 in fly ash and heavy metal ions—it achieves long-term stabilization of typical heavy metal ions such as Pb, Ni, As, and Cr in fly ash and molybdenum tailings. According to the "Horizontal Oscillation Method for Leaching Toxicity of Solid Waste" (HJ 557-2010), after 28 days of curing of the backfill, the leaching concentrations of the aforementioned heavy metals were all far below the Class III water limit of the "Groundwater Quality Standard" (GB / T 14848-2017), with a heavy metal chelation solidification efficiency exceeding 99.5%, fundamentally eliminating the risk of secondary pollution during the resource utilization of solid waste.
[0040] The alkaline-sulfate activated composite activation system constructed in this invention combines the rapid alkalinity supply from carbide slag with the slow-release alkali source from red mud, supplemented by sulfate ions provided by desulfurized gypsum / titanium gypsum, to achieve stepwise activation of the potential cementitious activity of active silica-alumina components such as slag powder / fly ash and waste glass powder / aluminum ash. This synergistic activation mechanism promotes the rapid formation of hydration products in the early stages, forming a dense network structure with ettringite (AFt) as the framework and CSH / CASH gel as the matrix. Example data shows that the 28-day compressive strength of this material is stable in the range of 5.5-12 MPa, fully meeting the engineering requirements for self-supporting strength and long-term stability in most mine backfilling processes. By fine-tuning the mass ratio of carbide slag and red mud in the composite alkaline activator, the initial setting time of the slurry can also be controlled within the range of 1.5-6 hours to adapt to different seasonal temperature changes and the construction window requirements of different mine backfilling processes (such as subsequent backfilling, layered backfilling, etc.). Meanwhile, thanks to the scientific particle size distribution design and the physical water retention effect of fine particles, the slurry can still maintain a high fluidity of 220-280mm under low water-to-solid ratio (0.30-0.36) conditions. In addition, the slurry has good homogeneity, anti-segregation and outstanding water retention performance, which can meet the stringent requirements of rheological properties for long-distance pipeline pumping in mine filling and greatly reduce the risk of pipe blockage.
[0041] This invention introduces sodium-calcium-silicon waste glass powder / aluminum ash as an active fine-tuning component in aluminosilicate materials. Utilizing its high-silicon, low-calcium properties, it regulates the Si / Al and Ca / Si ratios of the system, guiding the hydration products towards a low-calcium-silicon ratio, high-polymerization-degree CASH (aluminum-substituted calcium silicate hydrate) gel. This dense gel phase interweaves and interpenetrates with ettringite crystals, forming a framework-filler dual-reinforcing effect at the microscopic level. This effectively compensates for chemical shrinkage and drying shrinkage, significantly inhibiting plastic cracking and long-term shrinkage deformation during the hardening process of the filling material. Its volume stability is significantly superior to ordinary solid waste-based cementitious materials.
[0042] The preparation process of the mine backfill material provided by this invention is simple and easy to industrialize. Detailed Implementation
[0043] The technical solution of the present invention will be clearly and completely described below with reference to specific embodiments and experimental examples. However, those skilled in the art should understand that the embodiments are only used to illustrate the technical solution of the present invention and should not be regarded as limiting the scope of protection of the present invention. Based on the following embodiments, all other implementation schemes obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0044] Unless otherwise specified, the raw materials, reagents, and instruments used in the following examples and comparative examples are all commonly used items in the art and commercially available to the public. Unless otherwise specified, the experimental methods used in the experimental examples are conventional methods in the art. All terms and abbreviations used have their conventional meanings in the art. The molybdenum tailings were sourced from a molybdenum mine slag heap in Luanchuan, Luoyang. The molybdenum tailings raw material was placed in a ball mill for grinding, with a ball-to-material ratio controlled at 2:1 and a grinding time of 40 minutes. The ground molybdenum tailings powder was then placed in a high-temperature furnace and calcined at 800-850℃. After calcination, the powder was naturally cooled and sieved to obtain activated molybdenum tailings powder with a sieve aperture of 100 mesh.
[0045] The fly ash comes from the circulating fluidized bed fly ash produced by the Zhengzhou Municipal Waste Incineration Power Plant in Henan Province. The fly ash is subjected to staged thermal pyrolysis under an inert atmosphere, with the oxygen content controlled to be less than 1%. It is then subjected to dehydration at 150℃ for 20 min, polycrystalline transformation at 550℃ for 1.5 h, and melting at 1200℃. After the above three-stage temperature treatment, it is cooled and ground to a particle size of less than 0.25 mm to obtain pretreated fly ash micro powder.
[0046] The slag powder is S95 grade granulated blast furnace slag powder, purchased from Henan Jinrun New Materials Co., Ltd.
[0047] The fly ash is Class F, Grade I fly ash, purchased from Henan Jinrun New Materials Co., Ltd.
[0048] The calcium carbide slag is made of 200 mesh particles with a moisture content of less than 5% and an effective Ca(OH)2 content of more than 60%. It was purchased from Lingshou County Shiyunkai Mineral Products Processing Plant.
[0049] Red mud is a highly alkaline solid waste generated during the Bayer process for producing alumina. It is taken from an alumina plant in Lüliang, Shanxi Province. After being naturally air-dried, the red mud is ground and passed through a 0.15mm sieve (about 100 mesh). Its chemical composition contains ≥10% Na2O, ≥15% Al2O3, and ≥30% Fe2O3.
[0050] The desulfurized gypsum was in 200-mesh granules and was purchased from Lingshou County Chuangwei Mineral Products Processing Plant.
[0051] Fluorogypsum, in 200-mesh granules, was purchased from Yantai Anda Environmental Protection Technology Co., Ltd.
[0052] The waste glass powder is sodium-calcium-silicon waste glass powder, taken from Quwo Industrial Park, Linfen City, Shanxi Province. The fineness is less than 30μm, and the main chemical composition is SiO2 (70%-75%), Na2O (8%-12%) and CaO (8%-12%).
[0053] The aluminum ash is secondary aluminum ash, taken from Jinzhong Aluminum Industry in Linfen City, Shanxi Province, and passed through a 200-mesh sieve. Its main chemical composition is Al2O3 (about 50%) and metallic aluminum (about 10%).
[0054] To clarify the phase composition of waste incineration fly ash, X-ray diffraction analysis was performed on the collected primary fly ash samples. The analysis was conducted according to the standard "X-ray Diffraction Analysis Method for Clay Minerals and Common Non-Clay Minerals in Sedimentary Rocks" (SY / T 5163-2018) at room temperature. To ensure the uniformity and representativeness of the test, all samples were micro-powders with a particle size of less than 300 mesh. The test results are shown in Table 1.
[0055] Table 1. Main phase composition of fly ash
[0056]
[0057] Heavy metal leaching tests were conducted on fly ash according to the "Solid Waste Leaching Toxicity Leaching Method Acetic Acid Buffer Solution Method" (HJ / T 300-2007), and the results were compared with the pollutant concentration limits of the leachate specified in the "Pollution Control Standard for Municipal Solid Waste Landfills" (GB 16889-2024). The analysis results are shown in Table 2.
[0058] Table 2 Results of fly ash leaching toxicity
[0059]
[0060] Example 1
[0061] This embodiment provides a mine backfill material based on the synergistic solidification of molybdenum tailings and fly ash, comprising the following raw material components in parts by weight:
[0062] 100 portions of molybdenum tailings;
[0063] 10 parts fly ash;
[0064] 10 parts of gelling component;
[0065] The gelling components include mineral admixtures, composite alkaline activators, sulfate activators, and silica-alumina active admixtures, with the mass ratio of mineral admixtures to composite alkaline activators, sulfate activators, and silica-alumina active admixtures being 70:10:10:10.
[0066] The mineral admixture is composed of slag powder and fly ash, with a mass ratio of 60:10.
[0067] The composite alkaline activator is composed of carbide slag and red mud, with a mass ratio of 5:5.
[0068] The sulfate activator is desulfurized gypsum;
[0069] The silicon-aluminum active admixture is composed of waste glass powder and aluminum ash, with a mass ratio of 5:5.
[0070] This embodiment also provides a method for preparing mine backfill material, including the following steps:
[0071] Mineral admixtures, composite alkaline activators, sulfate activators, and silica-alumina active admixtures are mixed in proportion and stirred evenly for 10 minutes to obtain the gelling component.
[0072] Accurately weigh the molybdenum tailings, fly ash, and cementing components according to the above proportions, and dry mix them in a mixer at low speed for 5 minutes to ensure uniform mixing (mixing speed is 90 r / min) to obtain the mine backfill material.
[0073] This embodiment also provides an application of mine backfill material in backfilling mine goaf areas, including:
[0074] Add clean water to the mine backfill material at a water-to-solid ratio of 0.30, and stir at high speed for 150 r / min to obtain the backfill slurry.
[0075] The filling slurry is injected into the goaf of the mine and then solidified.
[0076] This embodiment also provides a sample for performance testing. The filling slurry is prepared in the same way as above. The freshly mixed slurry is injected into the mold in two batches. Each layer is vibrated on a vibrating table for 30 seconds to remove air bubbles. After the surface is smoothed, it is covered with plastic wrap to prevent moisture evaporation. After standing in a standard curing room for 24 hours, it is demolded. The demolded sample is then placed under the same conditions (temperature 20℃, humidity ≥90%) for curing until the specified age (i.e., curing for 28 days).
[0077] Example 2
[0078] This embodiment provides a mine backfill material based on the synergistic solidification of molybdenum tailings and fly ash. The only difference from Embodiment 1 is that the fly ash content is changed to 20 parts.
[0079] The preparation of the test specimens for performance testing in this embodiment is the same as in Example 1.
[0080] Example 3
[0081] This embodiment provides a mine backfill material based on the synergistic solidification of molybdenum tailings and fly ash. The only difference from Embodiment 1 is that the fly ash content is changed to 30 parts.
[0082] The preparation of the test specimens for performance testing in this embodiment is the same as in Example 1.
[0083] Example 4
[0084] This embodiment provides a mine backfill material based on the synergistic solidification of molybdenum tailings and fly ash. The only difference from Embodiment 1 is that the amount of cementitious component is changed to 15 parts and the water-to-solid ratio is changed to 0.33.
[0085] The preparation of the test specimens for performance testing in this embodiment is the same as in Example 1.
[0086] Example 5
[0087] This embodiment provides a mine backfill material based on the synergistic solidification of molybdenum tailings and fly ash. The only difference from Embodiment 4 is that the fly ash content is changed to 20 parts.
[0088] The preparation of the test specimens for performance testing in this embodiment is the same as in Example 4.
[0089] Example 6
[0090] This embodiment provides a mine backfill material based on the synergistic solidification of molybdenum tailings and fly ash. The only difference from Embodiment 4 is that the fly ash content is changed to 30 parts.
[0091] The preparation of the test specimens for performance testing in this embodiment is the same as in Example 4.
[0092] Example 7
[0093] This embodiment provides a mine backfill material based on the synergistic solidification of molybdenum tailings and fly ash. The only difference from Embodiment 1 is that the amount of cementitious component is changed to 20 parts and the water-to-solid ratio is changed to 0.36.
[0094] The preparation of the test specimens for performance testing in this embodiment is the same as in Example 1.
[0095] Example 8
[0096] This embodiment provides a mine backfill material based on the synergistic solidification of molybdenum tailings and fly ash. The only difference from Embodiment 7 is that the fly ash content is changed to 20 parts.
[0097] The preparation of the test specimens for performance testing in this embodiment is the same as in Example 7.
[0098] Example 9
[0099] This embodiment provides a mine backfill material based on the synergistic solidification of molybdenum tailings and fly ash. The only difference from Embodiment 7 is that the fly ash content is changed to 30 parts.
[0100] The preparation of the test specimens for performance testing in this embodiment is the same as in Example 7.
[0101] Example 10
[0102] This embodiment provides a mine backfill material based on the synergistic solidification of molybdenum tailings and fly ash. The only difference from Embodiment 2 is that the water-to-solid ratio is changed to 0.36.
[0103] The preparation of the test specimens for performance testing in this embodiment is the same as in Example 2.
[0104] Example 11
[0105] This embodiment provides a mine backfill material based on the synergistic solidification of molybdenum tailings and fly ash. The only difference from Embodiment 6 is that the water-to-solid ratio is changed to 0.30.
[0106] The preparation of the test specimens for performance testing in this embodiment is the same as in Example 6.
[0107] Example 12
[0108] This embodiment provides a mine backfill material based on the synergistic solidification of molybdenum tailings and fly ash. The only difference from Embodiment 5 is that the water-to-solid ratio is changed to 0.36.
[0109] The preparation of the test specimens for performance testing in this embodiment is the same as in Example 5.
[0110] Example 13
[0111] This embodiment provides a mine backfill material based on the synergistic solidification of molybdenum tailings and fly ash. The only difference from Embodiment 8 is that the water-to-solid ratio is changed to 0.30.
[0112] The preparation of the test specimens for performance testing in this embodiment is the same as in Example 8.
[0113] Example 14
[0114] This embodiment provides a mine backfill material based on the synergistic solidification of molybdenum tailings and fly ash. The only difference from Embodiment 9 is that the water-to-solid ratio is changed to 0.33.
[0115] The preparation of the test specimens for performance testing in this embodiment is the same as in Example 9.
[0116] Comparative Example 1
[0117] This embodiment provides a mine backfill material, which differs from Embodiment 2 only in that the cementitious component is replaced in equal amounts with P·O 42.5 ordinary Portland cement.
[0118] The preparation of the test specimens used for performance testing in this comparative example is the same as in Example 2.
[0119] Comparative Example 2
[0120] This embodiment provides a mine backfill material, which differs from Embodiment 13 only in that the cementitious component is replaced in equal amounts with P·O 42.5 ordinary Portland cement.
[0121] The preparation of the test specimens used for performance testing in this comparative example is the same as in Example 13.
[0122] Experimental Example
[0123] I. Experimental Methods
[0124] 1. Compressive strength test
[0125] Three parallel samples from the specimens prepared in the examples and comparative examples were selected for compressive strength testing, and their average values were calculated. The test results are shown in Table 3. After the test, the specimens were crushed and soaked in anhydrous ethanol for 5 days to avoid interference from the subsequent hydration process on the microstructure and composition analysis of the material, and were kept for later use.
[0126] Table 3 Compressive strength test results
[0127]
[0128] 2. Heavy metal leaching toxicity test
[0129] After drying the above-mentioned accurate samples, they were placed in beakers, and deionized water was added at a solid-liquid ratio of 1:10 (w / v) for a 24-hour leaching experiment. During the leaching process, the mouth of the beaker was sealed with plastic wrap to inhibit water evaporation. After leaching, the supernatant was taken to quantitatively assess the heavy metal leaching toxicity of fly ash under acidic leaching conditions, according to the standard method of "Leaching Toxicity of Solid Waste - Acetic Acid Buffer Solution Method" (HJ / T 300-2007). The test results are shown in Table 4.
[0130] Table 4 Results of Heavy Metal Leaching Toxicity Tests
[0131]
[0132] II. Experimental Results and Analysis
[0133] As shown in Tables 3 and 4, the mechanical strength and heavy metal solidification effect of the samples in the examples were significantly better than those in the comparative examples. In the ternary system of molybdenum tailings / fly ash / cementing components, the matching relationship between fly ash and cementing components plays a decisive role in the material properties, while the water-to-solid ratio further affects the density of the solidified body by regulating the hydration environment. In the compressive strength test results, Examples 1-3 show that insufficient cementing components make it difficult for fly ash to effectively participate in the cementation reaction, and it only plays a dilution role in the molybdenum tailings matrix; while in Examples 4-6, the activity of molybdenum tailings is fully activated, and the entire composite system forms a synergistic enhancement effect. The strength of Example 6 can reach 10.38 MPa, the highest strength of Example 13 reaches 11.26 MPa, and the strength of Example 14 reaches 11.13 MPa, indicating that the combination of medium-high cementing component content and moderate fly ash content is the key to constructing a dense cementitious network.
[0134] The heavy metal leaching data showed a strong negative correlation with the compressive strength. In Examples 13 and 14, which had the highest strength, the Pb leaching concentration was only 0.03-0.04 mg / L, far below the limit of 0.25 mg / L. Elements such as Ni, As, and Cr were also effectively stabilized. In contrast, the comparative examples had a strength of less than 6 MPa due to insufficient solidification, with Pb leaching reaching 0.32 and 0.24 mg / L, respectively. This further verifies that in the presence of the molybdenum tailings matrix, the synergistic ratio of fly ash and cementitious components and the appropriate water-to-solid ratio (0.30-0.33) are the core guarantees for achieving high strength and excellent environmental safety.
[0135] Although the technical solution of the present invention has been described in detail above with general descriptions, specific embodiments, and experimental examples, it should be noted that the embodiments and experimental examples are only used to illustrate the technical solution and technical effects of the present invention, and should not be regarded as limiting the scope of protection of the present invention. The scope of protection of the present invention is determined by the appended claims. Any modifications, equivalent substitutions, or improvements made based on the technical concept of the present invention that do not depart from the essence of the technical solution of the present invention shall fall within the scope of protection of the present invention.
Claims
1. A mine filling material based on molybdenum tailings-fly ash synergistic stabilization, characterized by: The mine backfill material comprises the following raw material components in parts by weight: 100 portions of molybdenum tailings; 10-30 parts fly ash; 10-20 parts of gelling component; The gelling components include mineral admixtures, composite alkaline activators, sulfate activators, and silica-alumina active admixtures, wherein the mass ratio of the mineral admixtures to the composite alkaline activators, sulfate activators, and silica-alumina active admixtures is 60-80:5-15:5-15:5-15.
2. A minefill material according to claim 1 characterised in that: The mass ratio of the mineral admixture to the composite alkaline activator, sulfate activator, and silica-alumina active admixture is 70:10:10:
10.
3. A minefill material according to claim 1 or 2, characterised in that: The mineral admixture is selected from one or more of slag powder and fly ash.
4. A minefill material according to claim 3, characterised in that: The slag powder is selected from S95 grade and S105 grade granulated blast furnace slag powder; And / or, the fly ash is Class F, Grade I fly ash.
5. A minefill material according to claim 1 or 2, characterised in that: The composite alkaline activator is composed of carbide slag and red mud, and the mass ratio of carbide slag to red mud is 5-7:3-5.
6. A minefill material according to claim 1 or 2, characterised in that: The sulfate activator is gypsum.
7. A minefill material according to claim 6, characterised in that: The gypsum is selected from one or more of desulfurized gypsum and fluorogypsum.
8. A minefill material according to claim 1 or 2, characterised in that: The silicon-aluminum active admixture is selected from one or more of waste glass powder and aluminum ash.
9. A method of producing a minefill material as claimed in any one of claims 1 to 8, characterised by: Includes the following steps: Mineral admixtures, composite alkaline activators, sulfate activators, and silica-alumina active admixtures are mixed in proportion to obtain a gelling component; Molybdenum tailings, fly ash, and cementing components are mixed in a certain proportion to obtain mine backfill material.
10. The application of a mine backfill material as described in any one of claims 1-8 in backfilling mine goaf areas.