A refractory and thermal insulation mortar synergistically constructed from multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles, and its preparation method thereof.
By synergistically constructing multi-size vitrified microspheres and large-size modified aerogels, and combining prefabricated closed microbubbles and silane coupling agents to improve interfacial compatibility, a multi-scale thermal insulation system is formed, which solves the shortcomings of existing thermal insulation mortars in terms of thermal conductivity, strength and crack resistance, and achieves high-efficiency fire-resistant thermal insulation performance and construction performance.
Patent Information
- Application Number
- CN202611100388.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-23
- Publication Date
- 2026-11-17
AI Technical Summary
When using single-size vitrified microspheres in existing thermal insulation mortars, the lightweight aggregate is loosely packed, making it difficult to simultaneously optimize thermal conductivity, strength, and volume stability. The aerogel and cement matrix interface is not compatible enough, affecting strength and workability. Simply relying on aerogel or lightweight aggregate to reduce thermal conductivity results in insufficient material strength, crack resistance, and decreased high-temperature stability.
The refractory and thermal insulation mortar is constructed by combining multi-size vitrified microspheres and large-size modified aerogel. The continuous graded skeleton is formed by four-stage vitrified microspheres, and a multi-scale thermal insulation system is constructed by combining pre-made closed microbubbles. Silane coupling agents are used to improve interfacial compatibility, and basalt fibers are used to enhance crack resistance.
It achieves low thermal conductivity, low density, good compressive strength and crack resistance, improves the fire resistance and thermal insulation stability and construction performance of the material, and meets the needs of building walls and fireproofing and thermal insulation projects.
Smart Images

Figure CN123106098A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of building insulation materials technology, and in particular to a fire-resistant and thermal insulation mortar composed of multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles, and its preparation method. Background Technology
[0002] With increasingly stringent building energy efficiency standards and fire safety requirements, inorganic thermal insulation mortars, which combine thermal insulation, fire resistance, and ease of construction, have gained widespread attention. Vitrified microspheres, characterized by their lightweight, closed-cell structure, high-temperature resistance, and non-combustibility, are commonly used as lightweight aggregates in inorganic thermal insulation mortars. SiO2 aerogels, with their nanoporous structure and low thermal conductivity, are also frequently used to improve the thermal insulation performance of insulation materials.
[0003] However, existing thermal insulation mortars typically have the following problems: First, when using single-size or low-grade vitrified microspheres, the lightweight aggregates are loosely packed, easily resulting in interconnected pores, localized slurry enrichment, or concentrated aggregate voids, making it difficult to simultaneously optimize thermal conductivity, strength, and volume stability. Second, when aerogel particles are directly incorporated, the aerogel has insufficient compatibility with the hydrophilic cement matrix interface, causing particles to easily agglomerate, float, or form weak bonding zones at the interface, thus affecting strength and workability. Third, when relying solely on aerogel or single lightweight aggregates to reduce thermal conductivity, the material often exhibits insufficient strength, insufficient crack resistance, or decreased structural stability after high temperatures.
[0004] Existing technologies involve grinding aerogel particles into micron-sized aerogel powder and using a dispersant system to combine the aerogel powder with finely ground cement to form a modified cement slurry. This approach focuses on the interfacial modification of cement particles and the nucleation of hydration products by the aerogel powder. However, it requires grinding the aerogel, compounding the dispersant, and grinding the cement; the core technology lies in the interfacial modification of the "aerogel powder-cement slurry" interface. In contrast, the approach of this invention differs from those that use large-diameter aerogel particles as independent insulating aggregates, multi-level vitrified microspheres as a load-bearing gradation framework, and pre-fabricated closed microbubbles as mesoscopic insulating pores.
[0005] Therefore, a new type of refractory and thermal insulation mortar is still needed. It should not be a simple superposition of vitrified microspheres, aerogels and additives, but rather a multi-scale thermal insulation structure that can be explained, controlled and replicated through a combination of aggregate gradation, wettability of aerogel particle interfaces and pre-fabricated foam pore structure. This structure should achieve a better balance between low thermal conductivity, low density, compressive strength, crack resistance and refractory thermal insulation stability. Summary of the Invention
[0006] To address the above technical problems, this invention provides a fire-resistant and thermally insulating mortar synergistically constructed from multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles, along with its preparation method. This process optimizes the gradation design of the multi-size vitrified microspheres, synergistically combines them with modified large-particle aerogel materials, and utilizes the synergistic effect of closed microbubbles to produce a fire-resistant and thermally insulating mortar that possesses excellent thermal insulation, fire resistance, and workability. Simultaneously, it effectively improves upon the problems of insufficient strength, easy cracking, and poor durability of traditional thermally insulating mortars, thereby enhancing the overall performance and application value of the material.
[0007] This invention utilizes a four-stage vitrified microsphere-filling-sealing continuous gradation structure, retains nano-insulating pores and fills the gaps in the framework using large-particle-size modified aerogel particles, and further constructs meso-scale insulating pores through pre-fabricated closed microbubbles. This results in a multi-scale insulation system synergistically combining macroscopic closed-cell aggregate, meso-scale closed microbubbles, and nano-aerogel pores. This mortar exhibits low thermal conductivity, low density, good compressive strength, crack resistance, and fire-resistant insulation stability, making it suitable for building walls, roofs, and fireproofing and insulation projects.
[0008] The first objective of this invention is to provide a refractory and thermal insulation mortar synergistically constructed from multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles, comprising the following raw materials: 50-70 parts of large-size SiO2 aerogel particles, 25-45 parts of four-size vitrified microspheres, 80-120 parts of cement, 1-3 parts of hydrophilic nano-SiO2, 0.8-1.2 parts of foaming agent, 0.1-0.2 parts of foam stabilizer, 1-3 parts of basalt fiber, 1-3 parts of methyl cellulose ether, 3-7 parts of redispersible latex powder, and 1-3 parts of water-reducing agent.
[0009] In this invention, basalt fiber is an inorganic refractory reinforcing fiber made from natural basalt. Its primary function is not thermal insulation, but rather to improve the crack resistance, toughness, and high-temperature structural stability of the mortar. Because the matrix contains lightweight porous components, the mortar is prone to shrinkage cracks or interfacial microcracks. Basalt fiber can form a bridging reinforcement effect within the cement matrix, inhibiting crack propagation. Basalt fiber possesses good refractory properties and high-temperature dimensional stability, and it does not easily melt and drip under fire or high-temperature conditions, thus helping to maintain the internal structural integrity of the mortar and improving its refractory and thermal insulation stability. It is irreplaceable by other fibers.
[0010] In this invention, methylcellulose ether primarily functions to retain water, thicken, improve workability and extensibility, enhance slurry cohesiveness, and stabilize the distribution of lightweight aggregates and precast foam. Because this invention utilizes lightweight porous components such as vitrified microspheres, aerogel particles, and precast closed microbubbles, insufficient slurry cohesiveness and water retention can easily lead to problems such as lightweight aggregate floating, uneven aerogel particle dispersion, and foam breakage or segregation. The addition of methylcellulose ether improves the water retention and cohesiveness of the mortar system, allowing the cement slurry to better encapsulate the vitrified microspheres and modified aerogel particles, and promoting the stable existence of closed microbubbles, thereby improving the mortar's workability, internal structural uniformity, and molding stability.
[0011] In some embodiments of the present invention, the particle size of the four-level vitrified microspheres is 30-50 mesh, 50-70 mesh, 70-90 mesh and 90-120 mesh.
[0012] In some embodiments of the present invention, the mass ratio of the 30-50 mesh, 50-70 mesh, 70-90 mesh and 90-120 mesh vitrified microspheres is (9-21):(15-30):(15-30):(9-21).
[0013] In some embodiments of the present invention, the cement is ordinary Portland cement, P·O42.5 grade cement;
[0014] The foaming agent is selected from one or more of the following: plant-based high-efficiency cement foaming agents, animal protein foaming agents, plant-based composite foaming agents, and synthetic surfactant foaming agents;
[0015] The foam stabilizer is selected from one or more of the following: hydroxypropyl methyl cellulose ether foam stabilizers, polymer foam stabilizers, cellulose ether composite foam stabilizers, or cement foaming-specific composite foam stabilizers.
[0016] The water-reducing agent is selected from one or more of polycarboxylate ether water-reducing agent (PCE), polycarboxylate-based high-performance water-reducing agent, naphthalene-based water-reducing agent, or aliphatic water-reducing agent;
[0017] The redispersible latex powder is selected from one or more of the following: ethylene-vinyl acetate copolymer redispersible latex powder, vinyl acetate-vinyl tert-carbonate copolymer redispersible latex powder, and acrylate redispersible latex powder. Redispersible latex powder is a type of polymer-modified powder that can redisperse upon contact with water to form a polymer emulsion and forms a polymer film during cement hydration and hardening. In this invention, the redispersible latex powder is mainly used to improve the bonding strength, flexibility, crack resistance, and workability of mortar, and to enhance the encapsulation and interfacial bonding effect of the cement matrix on vitrified microspheres and modified aerogel particles, thereby reducing the problems of interface debonding and drying shrinkage cracking of lightweight aggregates.
[0018] Large-diameter SiO2 aerogel particles have a particle size of 2.36-5.00 mm.
[0019] The second objective of this invention is to provide a method for preparing the refractory and thermal insulation mortar synergistically constructed from multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles, comprising the following steps:
[0020] Large-diameter SiO2 aerogel particles were surface-wetted with a silane coupling agent to obtain modified aerogel particles.
[0021] Add the foaming agent to water and stir at 300–600 rpm for 3–5 minutes to fully dissolve the foaming agent, obtaining an aqueous solution of the foaming agent. Then, use mechanical foaming to foam the foam at a speed of 1000–3000 rpm for 2–5 minutes to form fine and uniform foam. Next, add the foam stabilizer and stir at a low speed of 60–120 rpm for 1–3 minutes to evenly disperse the foam stabilizer and stabilize the cell structure, obtaining pre-prepared stable foam.
[0022] Cement, vitrified microspheres of four particle sizes, hydrophilic nano-SiO2 powder, basalt fiber, methyl cellulose ether and redispersible latex powder are dry-mixed, and then the modified aerogel particles are added and mixed at a low speed of 80-150 r / min to obtain a mixed dry material.
[0023] Add the water-reducing agent to water and stir until homogeneous to obtain a liquid additive mixture;
[0024] The liquid additive mixture is slowly added to the dry mixture while continuously stirring to form a uniform mortar matrix;
[0025] The pre-prepared stable foam is added to the mortar matrix under stirring conditions of 100-300 r / min. After stirring until the foam is evenly distributed, it is molded and cured to obtain the refractory and heat-insulating mortar.
[0026] In some embodiments of the present invention, the silane coupling agent is selected from aminosilane coupling agents.
[0027] In this invention, low-speed stirring is used when adding modified aerogel to avoid high-speed shearing causing aerogel particles to break or the pore structure to collapse, thereby affecting the thermal insulation performance of the material. At the same time, low-speed stirring is beneficial for the modified aerogel to be gradually wetted and encapsulated by the slurry, reducing the problems of particle floating, agglomeration and uneven dispersion, so that it is evenly distributed in the mortar system.
[0028] In this invention, the preferred mixing speed for mixing the pre-stabilized foam and the mortar matrix is 150–250 r / min. The reason for using low-speed mixing is that the pre-stabilized foam needs to maintain its structural integrity as much as possible after being added to the mortar matrix. Low-speed mixing can reduce shear forces, prevent excessive foam breakage, and ensure that the foam is evenly dispersed in the mortar.
[0029] If the stirring speed exceeds the above range, the stirring shear force will be too large, which can easily lead to foam rupture, bubble co-occurrence, or uneven pore size distribution, causing instability in the internal pore structure of the mortar. This will result in increased material density, decreased thermal insulation performance, poorer fire resistance and heat insulation effect, and may even affect the mechanical properties and volume stability of the mortar after molding.
[0030] In some embodiments of the present invention, the aminosilane coupling agent is selected from one or more of γ-aminopropyltriethoxysilane (KH550), γ-aminopropyltrimethoxysilane (KH540), N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane (KH792), and N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane (KH602).
[0031] In some embodiments of the present invention, the amount of the silane coupling agent is 0.5wt%-10wt%.
[0032] In some embodiments of the present invention, the wetting treatment conditions are as follows: a silane coupling agent is added to an alcohol-water mixture and stirred evenly to prepare a silane coupling agent treatment solution; the silane coupling agent treatment solution is uniformly sprayed onto the surface of large-diameter SiO2 aerogel particles, and the aerogel particles are continuously turned over during the spraying process to ensure that their surfaces are uniformly wetted; after spraying, the particles are allowed to stand for 20 to 40 minutes, and then dried at 40 to 60°C for 2 to 6 hours to obtain modified SiO2 aerogel particles.
[0033] The formation mechanism of the continuous gradation structure in this invention lies in the fact that the four-level vitrified microspheres are not randomly mixed, but rather form a stacked structure of "coarse skeleton - medium particle size filling - fine particle size sealing" through the stepwise intercalation between particles of different sizes. Among them, 30-50 mesh vitrified microspheres, as larger-sized lightweight aggregates, mainly form the supporting skeleton inside the mortar; 50-70 mesh and 70-90 mesh vitrified microspheres further fill the larger pores and transition pores between coarse particles; and 90-120 mesh vitrified microspheres enter the finer interfacial gaps, playing a role in sealing micropores and locally interconnected pores.
[0034] Through the aforementioned multi-level particle size embedding, the continuous channels that would normally easily form within the mortar are divided into dispersed closed or semi-closed pores, reducing gas convection heat transfer and solid-phase continuous thermal bridges. Simultaneously, large-particle-size modified SiO2 aerogel particles are embedded in the gaps between the vitrified microspheres, retaining their nanoporous thermal insulation function; pre-fabricated closed microbubbles further form a mesoscopic closed-pore structure within the cement matrix. This constitutes a multi-scale thermal insulation system with the synergistic effect of vitrified microsphere closed pores, pre-fabricated closed microbubbles, and aerogel nanopores.
[0035] The effects of this structure are: on the one hand, it reduces the number of interconnecting holes and heat conduction channels, thereby lowering the thermal conductivity of the mortar; on the other hand, it improves the uniformity of lightweight aggregate packing and the slurry coating state, thereby enhancing molding stability, compressive strength, and crack resistance; at the same time, inorganic components such as vitrified microspheres and basalt fibers have good high-temperature resistance, which is beneficial to improving the fire resistance and heat insulation stability of the material.
[0036] The technical solution of the present invention has the following advantages over the prior art:
[0037] 1. This invention uses four-level vitrified microspheres to form a continuous graded skeleton, rather than simply using lightweight aggregate of a single particle size. The vitrified microspheres include four particle size specifications: 30-50 mesh, 50-70 mesh, 70-90 mesh, and 90-120 mesh. Under the optimal compound ratio of the four, each particle size plays a unique role in the system: coarse particles provide skeleton support, medium particles fill the skeleton voids, and fine particles block micropores and interfacial gaps, thereby reducing the proportion of interconnected pores and improving the uniformity and volume stability of the mortar structure. Through the scientific gradation and compounding of the above four particle sizes, a multi-level dense packing structure of "skeleton-filling-sealing" is formed, which effectively improves the dispersion and packing state of lightweight aggregate in the mortar system, and significantly improves the uniformity, density and volume stability of the internal structure of the mortar. At the same time, SiO2 aerogel particles fill the gaps between the stacked vitrified microspheres with ultra-low thermal conductivity, blocking the heat conduction path. The vitrified microspheres, on the other hand, rely on their lightweight properties and high temperature resistance to build a fireproof support system. The two form a functional synergy of "microscopic thermal insulation and macroscopic fire resistance", which can significantly improve the thermal insulation performance and fire resistance limit of the mortar, and overcome the technical defects of the imbalance between the thermal insulation and fire resistance performance of single lightweight aggregate.
[0038] 2. This invention uses large-particle-size SiO2 aerogel particles as an independent insulating phase, preserving their nanoporous structure, and avoids the technical route of ball milling aerogel powder to modify cement particles. This design allows the low thermal conductivity of the aerogel to be used more for insulation between the skeletal gaps, rather than as a surface-modifying powder for cement particles.
[0039] 3. This invention uses a silane coupling agent to wettable the outer surface of large-diameter aerogel particles, thereby improving the interfacial compatibility between aerogel and cement paste, vitrified microspheres and nano-SiO2, and reducing the risk of agglomeration, floating and interfacial debonding.
[0040] 4. This invention pre-forms foaming agents and foam stabilizers into stable foam and adds them in the later stage of wet mixing, which differs from simply adding air-entraining components to dry materials. The pre-formed closed microbubbles, together with the closed pores of vitrified microspheres and aerogel nanopores, form a multi-scale porous structure, which is beneficial for reducing thermal conductivity and minimizing thermal bridging.
[0041] 5. This invention uses hydrophilic nano-SiO2 powder for micro-filling and interface densification, and uses basalt fibers of about 6mm to form a fire-resistant and crack-resistant reinforcing network, which can improve compressive strength, toughness and structural stability under high temperature while maintaining lightweight and low thermal conductivity.
[0042] 6. The core of this invention lies in the combination of "multi-size aggregate gradation - large-size aerogel interface control - pre-made closed microbubbles followed by admixture", which is not simply a mechanical superposition of aerogel, vitrified microspheres, cement and conventional admixtures. Attached Figure Description
[0043] To make the content of this invention easier to understand, the invention will be further described in detail below with reference to specific embodiments and accompanying drawings, wherein...
[0044] Figure 1 This invention relates to the preparation process of lightweight thermal insulation mortar. Detailed Implementation
[0045] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, so that those skilled in the art can better understand and implement the present invention. However, the embodiments described are not intended to limit the present invention.
[0046] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of this application. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains.
[0047] It should be noted that the terminology used herein is for the purpose of describing particular implementations only and is not intended to limit the exemplary implementations according to this application. As used herein, the singular form includes the plural form unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this description, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.
[0048] Example 1
[0049] This embodiment provides a refractory and thermal insulation mortar synergistically constructed from multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles, and its preparation method. The raw material amounts are shown in Table 1, and the specific steps include the following:
[0050] Step A: Weigh 1.0 kg of plant-based high-efficiency cement foaming agent (purchased from Zhengzhou Jinyuan Chemical Building Materials Co., Ltd.), add it to 50 mL of deionized water and dissolve it completely. Use a high-speed dispersing mixer at 2500 r / min and mechanically stir for 5 min to dissolve it completely. Prepare fine and uniform foam by mechanical foaming to form a foaming liquid; then add 0.1 kg of molecular adhesive foam stabilizer (high molecular adhesive foam stabilizer purchased from Zhengzhou Jinyuan Chemical Building Materials Co., Ltd.) and stir at 100 r / min for 2 min to obtain pre-stabilized foam;
[0051] Step B: Weigh 60.29 kg of SiO2 aerogel particles with a particle size of 2.36-5.00 mm, and sieve out the fine aerogel powder smaller than 2.36 mm. Then, perform surface modification treatment with a silane coupling agent on the sieved SiO2 aerogel particles. Weigh 3.01 kg of KH550 silane coupling agent and add it to an alcohol-water mixture composed of anhydrous ethanol and deionized water. Add the above KH550 silane coupling agent alcohol-water treatment solution to a stirring container and stir using a magnetic stirrer at a speed of 400 r / min for 10 min to ensure that the KH550 silane coupling agent is fully dispersed in the alcohol-water system, obtaining a uniform and stable modified treatment solution. After uniform mixing, a KH550 silane coupling agent alcohol-water treatment solution with a mass concentration of 5 wt% is obtained. The sieved SiO2 aerogel particles were evenly spread on a stainless steel tray, and the KH550 silane coupling agent alcohol-water treatment solution was sprayed evenly onto the surface of the SiO2 aerogel particles using a spray method. During the spraying process, the SiO2 aerogel particles were continuously turned over to ensure that the modified treatment solution fully wetted the outer surface of the aerogel particles, improving the uniformity of the silane coupling agent distribution on the aerogel particle surface. After spraying, the wetted SiO2 aerogel particles were allowed to stand for 30 minutes to allow the KH550 silane coupling agent to fully react with the hydroxyl groups on the surface of the aerogel particles. Subsequently, the treated SiO2 aerogel particles were placed in a forced-air drying oven for drying at a temperature controlled at 50°C to obtain modified aerogel particles.
[0052] Step C: Weigh 116 kg of P·O42.5 grade cement, 32 kg of vitrified microspheres (30-50 mesh vitrified microspheres, 50-70 mesh vitrified microspheres, 70-90 mesh vitrified microspheres, and 90-120 mesh vitrified microspheres in a ratio of 9:16:16:9), 0.464 kg of 6 mm high-strength basalt fiber (purchased from Senxiang Building Materials Store, Langli Street, Changsha County), 0.580 kg of methyl cellulose ether (purchased from Shandong Heda Group Co., Ltd., model HPMC-E50), and 1.700 kg of redispersible latex powder (using VAE type redispersible latex powder produced by Shandong Yiteng New Materials Co., Ltd., model ET-3060).
[0053] Step D: First, add cement, nano-SiO2 powder, basalt fiber, methyl cellulose ether, and redispersible latex powder to a mortar mixer for premixing at a speed of 60 r / min for 5 min. Then, add vitrified microspheres of four particle sizes and continue mixing at low speed for 5 min. Finally, add the modified SiO2 aerogel particles obtained in step B and mix at low speed of 40 r / min for 5 min to obtain a dry mixture.
[0054] Step E: Add the water-reducing agent (polycarboxylate ether water-reducing agent (PCE) purchased from Guangzhou Dingzun Trading Co., Ltd.) to the remaining mixing water and stir evenly. The amount of water-reducing agent is 5.8 kg of cement mass. Then, slowly add the obtained water-reducing agent aqueous solution to the dry mixture obtained in Step D and stir for 5 minutes using a mortar mixer to obtain the refractory and thermal insulation mortar matrix. Then add the pre-made stable foam obtained in Step A and stir at low speed for 3 minutes at 250 r / min to obtain the refractory and thermal insulation mortar slurry. Pour the obtained slurry into a mold to form it. After compaction, place it under constant temperature and humidity conditions of 20±2℃ and relative humidity ≥90% for 28 days to obtain the refractory and thermal insulation mortar specimen.
[0055] Example 2
[0056] This comparative example provides a method for preparing mortar, which is similar to that in Example 1, except that the aerogel is modified with 1 wt% silane coupling agent.
[0057] Example 3
[0058] This comparative example provides a method for preparing mortar, which is similar to that in Example 1, except that the aerogel is modified with 10wt% silane coupling agent.
[0059] Example 4
[0060] The refractory and thermal insulation mortar constructed by multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles provided in this embodiment and its preparation method are similar to those in Embodiment 1. The difference is that the mass ratio of the four-stage vitrified microspheres is 7:5:5:3.
[0061] Example 5
[0062] The refractory and thermal insulation mortar constructed by multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles provided in this embodiment and its preparation method are similar to those in Embodiment 1. The difference is that the mass ratio of the four-stage vitrified microspheres is 3:5:5:7.
[0063] Example 6
[0064] The refractory and thermal insulation mortar constructed by multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles in this embodiment and its preparation method are similar to those in Embodiment 1. The difference is that the mass ratio of the four-stage vitrified microspheres is 1:1:1:1.
[0065] Example 7
[0066] The refractory and thermal insulation mortar constructed by multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles provided in this embodiment and its preparation method are similar to those in Example 1. The difference is that 0.116 kg of nano SiO2 powder (purchased from Xuancheng Jingna Environmental Protection Technology Co., Ltd., model VK-SP30S hydrophilic type) is added to the mortar based on Example 1.
[0067] Comparative Example 1
[0068] This comparative example provides a method for preparing mortar, which is similar to that in Example 1, except that vitrified microspheres, aerogel, foaming agent and foam stabilizer are not added.
[0069] Comparative Example 2
[0070] This comparative example provides a method for preparing mortar, similar to that in Example 1, except that vitrified microspheres and aerogel are not added. Instead, a foaming agent and a foam stabilizer are added, and stable foam is pre-formed.
[0071] Comparative Example 3
[0072] This comparative example provides a method for preparing mortar, which is similar to that of Example 1. The difference is that vitrified microspheres and aerogel are not added, but foaming agent and foam stabilizer are added. Instead of pre-forming stable foam, the foaming agent and foam stabilizer are directly added to the mixing water and mixed with the water-reducing agent before being added to the mortar system at one time. Foam is formed by mechanical stirring to induce air.
[0073] Comparative Example 4
[0074] This comparative example provides a method for preparing mortar, which is similar to that in Example 1, except that aerogel is not added, but the four-level vitrified microspheres are replaced with single 70-90 mesh vitrified microspheres.
[0075] Comparative Example 5
[0076] This comparative example provides a method for preparing mortar, which is similar to that in Example 1, except that aerogel is not added, but the quaternary vitrified microspheres are replaced with secondary vitrified microspheres.
[0077] Comparative Example 6
[0078] This comparative example provides a method for preparing mortar, which is similar to that in Example 1, except that aerogel is not added, but the quaternary vitrified microspheres are replaced with tertiary vitrified microspheres.
[0079] To verify the synergistic effect of multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles, the following comparative examples and embodiments were set up. In Table 1, Comparative Example 1 is the baseline group without vitrified microspheres, aerogel, foaming agent, or foam stabilizer; Comparative Example 2 is the foaming baseline group with foaming agent and foam stabilizer added and a pre-formulated stable foam process; Comparative Example 3 is the control group where foaming agent and foam stabilizer are directly added to the mixing water to induce air foaming without pre-formulated stable foam, used to verify the technical effect of the pre-formulated stable foam process; Comparative Example 4 is a single vitrified microsphere thermal insulation mortar; Comparative Example 5 is a two-component vitrified microsphere thermal insulation mortar; Comparative Example 6 is a three-component vitrified microsphere thermal insulation mortar; Examples 1-7 are groups with different four-stage vitrified microsphere gradations and aerogel compounding; Examples 2-3 are implementation groups with different silane coupling agent dosages based on the preferred gradation of Example 1; Example 7 is an implementation group with nano-SiO2 powder added based on the preferred gradation of Example 1. For details on the raw material usage of Examples 1 to 7 and Comparative Examples 1 to 6, please refer to Table 1.
[0080] Table 1. Raw material consumption of comparative examples and embodiments.
[0081] Serial Number cement / kg Vitrified microspheres / kg aerogel / kg Water / kg admixtures Example 1 116.8 9:16:16:9 (Total mass 32) 60.29 116.8 - Example 2 116.8 9:16:16:9 (Total mass 32) 60.29 116.8 Same as Example 1, but the aerogel was modified with 1 wt% silane coupling agent. Example 3 116.8 9:16:16:9 (Total mass 32) 60.29 116.8 Same as in Example 1, the aerogel was modified with 10 wt% silane coupling agent. Example 4 116.8 7:5:5:3 (Total mass 32) 60.29 116.8 Same as Example 1 Example 5 116.8 3:5:5:7 (Total mass 32) 60.29 116.8 Same as Example 1 Example 6 116.8 1:1:1:1 (Total mass 32) 60.29 116.8 Same as Example 1 Example 7 116.8 9:16:16:9 (Total mass 32) 60.29 116.8 <![CDATA[Hydrophilic nano-SiO₂ is added on the basis of Example 1]]> Comparative Example 1 116.8 0 0 116.8 Similar to Example 1, except that vitrified microspheres, aerogel, foaming agent and foam stabilizer were not added. Comparative Example 2 116.8 0 0 116.8 Similar to Example 1, the difference is that vitrified microspheres and aerogel were not added. A foaming agent and a foam stabilizer were added, and a stable foam was pre-formed. Comparative Example 3 116.8 0 0 116.8 The difference from Example 1 is that vitrified microspheres and aerogel are not added. Instead of pre-forming a stable foam, the foaming agent and foam stabilizer are added directly to the mixing water and then mixed with the water-reducing agent before being added to the mortar system all at once. Comparative Example 4 116.8 Single 70-90 mesh (total mass 70) 0 116.8 Similar to Example 1, the difference is that no aerogel was added, but the four-level vitrified microspheres were replaced with single 70-90 mesh vitrified microspheres. Comparative Example 5 116.8 Second-grade 30-50 mesh: 90-120 mesh = 1:1 (total mass 70) 0 116.8 Similar to Example 1, the difference is that no aerogel was added, but the quaternary vitrified microspheres were replaced with tertiary vitrified microspheres. Comparative Example 6 116.8 Grade 3 30-50 mesh : 70-90 mesh : 90-120 mesh = 9 : 16 : 9 (total mass 70) 0 116.8 Similar to Example 1, the difference is that no aerogel was added, but the quaternary vitrified microspheres were replaced with tertiary vitrified microspheres.
[0082] Table 2 Performance tests of Examples 1-5 and Comparative Examples 1-6
[0083]
[0084] As shown in Table 2, the performance test results indicate that Comparative Example 1, without the addition of foaming agent and foam stabilizer, yielded a mortar with a dry density as high as 611 kg / m³. 3 The thermal conductivity was 0.135 W / (m·K), which does not meet the requirements of GB / T20473-2021 "Building Thermal Insulation Mortar" standard, indicating that it is difficult to obtain good lightweight thermal insulation performance by relying solely on cement-based systems. In Comparative Example 2, after adding foaming agents and foam stabilizers and pre-forming stable foam, the dry density decreased to 320 kg / m³, and the thermal conductivity decreased to 0.060 W / (m·K). In Comparative Example 3, using foaming agents and foam stabilizers for direct air-entrained foaming, the dry density was further reduced to 288 kg / m³. 3 The thermal conductivity is 0.055 W / (m·K). This indicates that introducing foam can significantly increase the porosity of the material, reduce the dry density and thermal conductivity, and provide a foundation for the subsequent construction of a lightweight insulation system.
[0085] The dosage of silane coupling agent has a significant impact on the dispersion stability and thermal insulation performance of large-particle-size SiO2 aerogel particles in cement-based systems. Examples 1 to 3 were used to verify the effect of different silane coupling agent dosages on the aerogel modification effect. When the silane coupling agent dosage is insufficient, the surface modification of the aerogel particles is inadequate, and problems such as hydrophobic agglomeration, floating, and insufficient slurry encapsulation still easily occur, leading to an uneven pore structure within the insulation system and a relatively increased thermal conductivity. When the silane coupling agent dosage is 5 wt%, the dry density of the sample is 260 kg / m³. 3 The thermal conductivity was 0.043 W / (m·K), the lowest among Examples 1 to 3, and met the Class I standard of GB / T20473-2021 building thermal insulation mortar. This indicates that the addition of 5 wt% silane coupling agent can form a relatively complete and moderate interface modification layer on the aerogel surface, improving the wetting and dispersion state of aerogel particles in the cement-based system, and allowing its low thermal conductivity properties to be fully utilized. When the dosage of silane coupling agent continues to increase, excessive coupling agent is prone to local self-condensation or the formation of an excessively thick organic layer, which in turn affects particle dispersion and foam stability, resulting in no further reduction in thermal conductivity. Therefore, 5 wt% silane coupling agent is the preferred dosage in this system that balances aerogel dispersion stability, interface compatibility, and low thermal conductivity.
[0086] The comparative results of Comparative Examples 4 to 6 show that the particle size gradient number of vitrified microspheres has a significant impact on the lightweighting and thermal conductivity of mortar. Comparative Example 4 used single 70-90 mesh vitrified microspheres with a dry density of 403 kg / m³. 3 The thermal conductivity is 0.071 W / (m·K), which only meets the Class II standard of GB / T20473-2021 building thermal insulation mortar, indicating that concentrated pores and local heat conduction channels are easily formed between single-size vitrified microspheres. Comparative Example 5, after using a two-stage blend of 30-50 mesh and 90-120 mesh particles, showed a dry density reduction to 390 kg / m³. 3 The thermal conductivity decreased to 0.066 W / (m·K), meeting the Class I standard, indicating that the blending of coarse and fine particles can improve the particle packing state. In Comparative Example 6, after a three-stage blending process, the dry density was further reduced to 374 kg / m³. 3 The thermal conductivity decreased to 0.063 W / (m·K), indicating that increasing the particle size gradient is beneficial to improving the filling continuity and pore structure distribution of the vitrified microspheres.
[0087] However, the three-stage compound still struggles to simultaneously achieve the four functions of coarse skeleton support, intermediate transition filling, fine filling, and micropore sealing. Therefore, this invention further employs a four-stage continuous particle size compound of vitrified microspheres: 30-50 mesh, 50-70 mesh, 70-90 mesh, and 90-120 mesh. Specifically, 30-50 mesh vitrified microspheres are used to construct a lightweight support skeleton; 50-70 mesh and 70-90 mesh vitrified microspheres are used to progressively fill the gaps in the skeleton; and 90-120 mesh vitrified microspheres are used to seal micropores and improve the interface transition zone. This four-stage continuous particle size structure forms a continuous interlocking system of "coarse skeleton—primary filling—secondary filling—micropore sealing," transforming the internal pores of the mortar from a concentrated, interconnected state to a dispersed, closed state, thereby reducing heat conduction channels and providing a more stable embedding space for large-particle-size modified SiO2 aerogel particles.
[0088] Examples 1-3 were used to verify the effect of different silane coupling agent dosages on the aerogel modification effect. The silane coupling agent dosage has a significant impact on the dispersion stability and thermal insulation performance of large-particle-size SiO2 aerogel particles in cement-based systems. Specifically, when the silane coupling agent dosage is insufficient, the surface modification of the aerogel particles is inadequate, and problems such as hydrophobic agglomeration, floating, and insufficient slurry encapsulation still easily occur, leading to an uneven internal pore structure and a relatively increased thermal conductivity in the insulation system. When the silane coupling agent dosage is 5 wt%, the dry density of the sample is 260 kg / m³. 3 The thermal conductivity was 0.043 W / (m·K), the lowest among Examples 1 to 3, and met the Class I standard of GB / T20473-2021 for building thermal insulation mortar. This indicates that the addition of 5 wt% silane coupling agent can form a relatively complete and moderate interface modification layer on the aerogel surface, improving the wetting and dispersion state of aerogel particles in the cement-based system, and allowing its low thermal conductivity properties to be fully utilized. When the dosage of silane coupling agent continues to increase, excessive coupling agent is prone to local self-condensation or the formation of an excessively thick organic layer, which in turn affects particle dispersion and foam stability, resulting in no further reduction in thermal conductivity. Therefore, 5 wt% silane coupling agent is the preferred dosage in this system that balances aerogel dispersion stability, interface compatibility, and low thermal conductivity.
[0089] The comparative results of Examples 1 and 4-6 show that in the four-stage particle size blending system, different gradation ratios have a significant impact on the dry density and thermal conductivity of the mortar. Example 1 uses a four-stage continuous gradation of 30-50 mesh: 50-70 mesh: 70-90 mesh: 90-120 mesh = 9:16:16:9, with a dry density of 260 kg / m³. 3The thermal conductivity is 0.043 W / (m·K), the lowest among the examples, and meets the Class I standard of GB / T20473-2021 "Building Thermal Insulation Mortar", indicating that this gradation can form a superior continuous interlocking structure and effectively reduce heat conduction channels. Example 4 uses a 7:5:5:3 coarser gradation, reducing the dry density to 250 kg / m³. 3 However, the thermal conductivity was 0.044 W / (m·K), slightly higher than that of Example 1, indicating that increasing the proportion of coarse particles is beneficial for reducing the system density. However, due to insufficient filling of medium and fine particles, the continuity of the skeletal gaps is enhanced, which is not conducive to further reducing the thermal conductivity. Example 5 used a 3:5:5:7 finer gradation, and the dry density increased to 278 kg / m³. 3 The thermal conductivity increased to 0.052 W / (m·K), indicating that an excessively high proportion of fine particles would increase the system's density and the continuity of solid-phase heat conduction, which is detrimental to lightweight insulation. Example 6 used a 1:1:1:1 homogeneous mixture with a dry density of 265 kg / m³. 3 The thermal conductivity is 0.049 W / (m·K), indicating that simple uniform distribution cannot form the optimal pore structure and packing state.
[0090] Therefore, the 9:16:16:9 four-stage continuous gradation is not an arbitrary ratio, but a gradation scheme that achieves a better balance between coarse skeleton support, intermediate particle size transition filling, and fine particle size micropore sealing. This ratio avoids the pore connectivity problem caused by insufficient filling of medium and fine particles in a coarse gradation, and also avoids the problem of increased thermal conductivity caused by increased solid-phase contact in a fine gradation. Thus, it achieves the lowest thermal conductivity while maintaining a low dry density, making it a suitable preferred gradation for the multi-size vitrified microsphere-modified aerogel-closed microbubble system of this invention.
[0091] Therefore, considering lightweight and low thermal conductivity, the four-stage continuous particle size blend is significantly superior to the single-size, two-stage, and three-stage blends. Among them, the 9:16:16:9 gradation can form a relatively stable continuous interlocking structure, taking into account the functions of skeletal support, transition filling, and micropore sealing, making it suitable as the basic preferred gradation of this invention. If further pursuit of lower dry density and lower thermal conductivity is desired, a coarser 7:5:5:3 gradation can be used; if structural stability and subsequent nano-SiO2 enhancement are considered comprehensively, then 9:16:16:9 is more suitable as the preferred reference ratio.
[0092] Furthermore, in Example 7, hydrophilic nano-SiO2 was added to the 9:16:16:9 four-level optimized gradation of Example 1, resulting in a dry density of 255 kg / m³. 3The thermal conductivity is 0.045 W / (m·K), still meeting the Class I standard of GB / T20473-2021 "Building Thermal Insulation Mortar"; at the same time, its compressive strength increased from 0.80 MPa in Example 1 to 0.90 MPa, an increase of about 12.5%. This indicates that the addition of hydrophilic nano-SiO2 did not significantly damage the multi-scale thermal insulation structure composed of aerogel, vitrified microspheres and closed microbubbles, and can still maintain a low thermal conductivity; at the same time, nano-SiO2 can improve the transition zone between cement paste and lightweight aggregate interface through micro-filling effect and pozzolanic activity, improve matrix density and interfacial bonding strength, thereby further improving the mechanical stability of mortar while basically maintaining thermal insulation performance.
[0093] In summary, 5wt% KH550 modification enables large-particle-size SiO2 aerogel particles to achieve a better wetting and dispersion state, fully leveraging their low thermal conductivity advantage. The four-stage continuous particle size vitrified microsphere blend forms a continuous interlocking and filling structure, which is more beneficial for reducing dry density and thermal conductivity compared to single-particle-size, two-stage, and three-stage blends. The 9:16:16:9 gradation can serve as a basic preferred ratio that balances structural stability and thermal insulation performance. The addition of hydrophilic nano-SiO2 further improves the interface structure while maintaining Class I thermal insulation performance. These results demonstrate that this invention achieves comprehensive optimization of lightweight, low thermal conductivity, and standard compliance in thermal insulation mortar through the synergistic effects of KH550 aerogel interface modification, four-stage continuous vitrified microsphere gradation, closed microbubble insulation, and nano-SiO2 interface enhancement.
[0094] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A refractory and thermal insulation mortar synergistically constructed from multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles, characterized in that, The raw materials include: 50-70 parts of large-particle-size SiO2 aerogel particles, 25-45 parts of four-stage vitrified microspheres, 80-120 parts of cement, 1-3 parts of hydrophilic nano-SiO2, 0.8-1.2 parts of foaming agent, 0.1-0.2 parts of foam stabilizer, 1-3 parts of basalt fiber, 1-3 parts of methyl cellulose ether, 3-7 parts of redispersible latex powder, and 1-3 parts of water-reducing agent.
2. The refractory and thermal insulation mortar synergistically constructed from multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles according to claim 1, is characterized in that... The four-level vitrified microspheres have particle sizes of 30-50 mesh, 50-70 mesh, 70-90 mesh, and 90-120 mesh.
3. The refractory and thermal insulation mortar synergistically constructed from multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles according to claim 2, is characterized in that... The mass ratio of the 30-50 mesh, 50-70 mesh, 70-90 mesh and 90-120 mesh vitrified microspheres is (9-21):(15-30):(15-30):(9-21).
4. The refractory and thermal insulation mortar synergistically constructed from multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles according to claim 1, characterized in that, The cement is ordinary Portland cement, grade P·O42.
5. The foaming agent is selected from one or more of the following: plant-based high-efficiency cement foaming agents, animal protein foaming agents, plant-based composite foaming agents, and synthetic surfactant foaming agents; The foam stabilizer is selected from one or more of the following: hydroxypropyl methyl cellulose ether foam stabilizers, polymer foam stabilizers, cellulose ether composite foam stabilizers, or cement foaming-specific composite foam stabilizers. The water-reducing agent is selected from one or more of polycarboxylate ether water-reducing agent (PCE), polycarboxylate-based high-performance water-reducing agent, naphthalene-based water-reducing agent, or aliphatic water-reducing agent; The redispersible latex powder is selected from one or more of the following: ethylene-vinyl acetate copolymer redispersible latex powder, vinyl acetate-vinyl tert-carbonate copolymer redispersible latex powder, and acrylate redispersible latex powder.
5. The refractory and thermal insulation mortar synergistically constructed from multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles according to claim 1, characterized in that, Large-diameter SiO2 aerogel particles have a particle size of 2.36-5.00 mm.
6. A method for preparing a refractory and thermal insulation mortar synergistically constructed from multi-size vitrified microspheres, large-size modified aerogel, and closed microbubbles as described in any one of claims 1 to 5, characterized in that, Includes the following steps: Large-diameter SiO2 aerogel particles were surface-wetted with a silane coupling agent to obtain modified aerogel particles. Add the foaming agent to water and stir at 300-600 rpm for 3-5 minutes to fully dissolve the foaming agent and obtain an aqueous solution of the foaming agent; then use mechanical foaming to foam the foam at a speed of 1000-3000 rpm for 2-5 minutes to form fine and uniform foam. Add the foam stabilizer and stir at 60-120 r / min for 1-3 min to evenly disperse the foam stabilizer and stabilize the cell structure, thus obtaining pre-made stable foam; Cement, vitrified microspheres with four particle sizes, hydrophilic nano-SiO2 powder, basalt fiber, methyl cellulose ether and redispersible latex powder are dry-mixed, and then the modified aerogel particles are added and mixed at a speed of 80-150 r / min to obtain a mixed dry material. Add the water-reducing agent to water and stir until homogeneous to obtain a liquid additive mixture; The liquid additive mixture is added to the dry mixture and stirred continuously to form a uniform mortar matrix; The pre-prepared stable foam is added to the mortar matrix under stirring conditions of 100-300 r / min. After stirring until the foam is evenly distributed, it is molded and cured to obtain the refractory and heat-insulating mortar.
7. The preparation method according to claim 6, characterized in that, The silane coupling agent is selected from aminosilane coupling agents.
8. The preparation method according to claim 7, characterized in that, The aminosilane coupling agent is selected from γ-aminosilane coupling agents, including one or more of γ-aminopropyltriethoxysilane KH550, γ-aminopropyltrimethoxysilane KH540, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane KH792, and N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane KH602.
9. The preparation method according to claim 6, characterized in that, The amount of the silane coupling agent used is 0.5wt%-10wt%.
10. The preparation method according to claim 6, characterized in that, Conditions for wetting treatment: Add silane coupling agent to alcohol-water mixture, stir evenly to prepare silane coupling agent treatment solution; spray the silane coupling agent treatment solution evenly on the surface of large-diameter SiO2 aerogel particles, and continuously turn the aerogel particles during the spraying process to make their surface evenly wetted. After spraying, let stand for 20-40 minutes, then dry at 40-60℃ for 2-6 hours to obtain modified SiO2 aerogel particles.