A whisker-toughened dual-phase high-entropy ceramic material and its preparation method

By constructing a (TiZrHfTaV)B2-(TiZrHfTaV)C dual-phase matrix and introducing SiC-B5 whiskers in high-entropy ceramic materials, the brittle fracture problem of high-entropy ceramics was solved, and the high fracture toughness and anti-brittle fracture reliability were improved. This method is suitable for aerospace and nuclear reactor structural materials.

CN123106218APending Publication Date: 2026-11-17HELAN MOUNTAIN LABORATORY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611393821.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

High-entropy ceramic materials are prone to rapid brittle fracture under external loads. They lack effective energy dissipation paths for phase transformation toughening and crack deflection, resulting in low fracture toughness and limiting their engineering applications in aerospace, thermal protection, and nuclear reactor structural materials.

Method used

A (TiZrHfTaV)B2-(TiZrHfTaV)C dual-phase matrix was constructed, and SiC-B5 whiskers were introduced as toughening phases. By utilizing the differences in the crack propagation path of the whiskers, multi-stage energy dissipation was achieved through crack deflection, bridging and pull-out effects.

Benefits of technology

It significantly improves the fracture toughness and brittle fracture resistance of the material, with fracture toughness increased by approximately 88.3% and hardness maintained at 21.55 GPa, making it suitable for extreme service environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106218A_ABST
    Figure CN123106218A_ABST
Patent Text Reader

Abstract

This invention discloses a whisker-toughened biphase high-entropy ceramic material and its preparation method, belonging to the technical field of non-oxide ceramic matrix composite materials. The material uses a biphase high-entropy ceramic as the matrix and SiC-B5 whiskers as the toughening phase to obtain a whisker-toughened biphase high-entropy ceramic material. The obtained whisker-toughened biphase high-entropy ceramic material maintains the HEB / HEC biphase structure and the phase-selective distribution characteristics of transition metal cations. The SiC-B5 whiskers improve the material's resistance to crack propagation through synergistic energy dissipation via crack deflection, whisker bridging, and whisker pull-out. The fracture toughness of the 5wt% SiC-B5 whisker-toughened biphase ceramic reaches 5.913 MPa·m. 1 / 2 It maintains a Vickers hardness of 21.55 GPa, making it suitable for extreme service environments such as aerospace, high-speed cutting tools, wear-resistant components, and nuclear reactor structural materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of non-oxide ceramic matrix composite materials technology, specifically relating to a whisker-toughened dual-phase high-entropy ceramic material and its preparation method. Background Technology

[0002] High-entropy ceramics, due to their multi-principal-element solid solution structure, high hardness, and good high-temperature stability, are considered important candidate structural materials for extreme service environments. Compared with single-phase high-entropy ceramics, constructing two-phase high-entropy ceramics by combining high-entropy borides and high-entropy carbides, and utilizing the complementary properties of the two phases in terms of hardness, thermal stability, and crack propagation resistance, provides a new microstructure design approach for improving overall mechanical properties.

[0003] However, dual-phase high-entropy ceramics constructed from high-entropy borides and high-entropy carbides still exhibit significant brittle characteristics. Cracks tend to propagate rapidly under external loads. The multi-principal solid solution structure in dual-phase high-entropy ceramics leads to a large number of atomic size mismatches, causing local lattice distortion and inducing local stress concentration. Furthermore, the system lacks effective external energy dissipation mechanisms for phase transformation toughening or crack deflection, resulting in rapid crack propagation without resistance after initiation. This intrinsic brittle behavior is directly reflected in the fact that the fracture toughness is generally lower than the threshold for engineering applications. Under thermal shock or mechanical impact loads, it is extremely prone to sudden, unpredictable overall brittle fracture, which severely weakens the load-bearing reliability and service life of components, restricting their engineering applications in aerospace thermal protection, high-speed cutting tools, and nuclear reactor structural materials. Summary of the Invention

[0004] To address the technical problem in existing high-entropy ceramic systems that lack effective energy dissipation pathways for phase transformation toughening and crack deflection, resulting in a lack of propagation resistance after crack initiation and a high susceptibility to sudden brittle fracture, this invention provides a whisker-toughened dual-phase high-entropy ceramic material and its preparation method.

[0005] This invention constructs a (TiZrHfTaV)B2-(TiZrHfTaV)C dual-phase matrix using high-entropy borides HEB and high-entropy carbides HEC. The differences between the two phases in crystal structure, element affinity, and crack propagation path are utilized to create a high-density phase interface, providing a basis for crack deflection and bifurcation. Simultaneously, SiC-B5 whiskers are further introduced as a one-dimensional toughening phase, causing cracks to deflect, bridge, and pull out at the whiskers, thereby achieving multi-stage, multi-scale energy dissipation and ultimately effectively improving the fracture toughness and brittle fracture resistance of the material.

[0006] To achieve the above objectives, the technical solution of the present invention is as follows.

[0007] The first objective of this invention is to provide a whisker-toughened biphase high-entropy ceramic material, wherein the whisker-toughened biphase high-entropy ceramic material uses biphase high-entropy powder as a matrix and SiC-B5 whiskers as a toughening phase, wherein the toughening phase is dispersed in the matrix.

[0008] The dual-phase high-entropy powder comprises (TiZrHfTaV)B2 phase and (TiZrHfTaV)C phase.

[0009] The amount of SiC-B5 whiskers added is 5wt% to 15wt% of the mass of the dual-phase high-entropy powder.

[0010] In a preferred embodiment, the SiC-B5 whiskers have a diameter of 80nm to 150nm and a length of 0.5μm to 8μm.

[0011] In this invention, SiC-B5 whiskers with a diameter of approximately 80 nm to 150 nm and a length of approximately 0.5 μm to 8 μm are used. These whiskers have a high aspect ratio, and this one-dimensional structure is beneficial for forming crack deflection, whisker bridging, and whisker pull-out toughening units within the ceramic matrix. Both SiC-B4 and SiC-B5 whiskers can be mixed with the matrix powder, but SiC-B4 whiskers, due to their smaller diameter and tendency to entangle, exhibit slight localized agglomeration. In contrast, SiC-B5 whiskers are more uniformly distributed within the matrix, with no significant large-area agglomeration, which is beneficial for densification during subsequent SPS sintering and for achieving crack bridging and toughening effects. Therefore, SiC-B5 whiskers have better compatibility with the HEB / HEC matrix, resulting in a denser microstructure, more continuous grain bonding, and fewer pores and whisker agglomerations in the SiC-B5 whisker-toughened dual-phase high-entropy ceramic material.

[0012] In a preferred embodiment, the fracture toughness of the whisker-toughened dual-phase high-entropy ceramic material is 5.76 MPa·m. 1 / 2 ~5.913MPa·m 1 / 2 Its Vickers hardness is 21.55 GPa to 23.04 GPa, and its relative density is 97.417% to 98.934%.

[0013] In a preferred embodiment, the two-phase high-entropy powder is prepared by ball milling TiO2, ZrO2, HfO2, V2O5, Ta2O5, B4C and carbon black as raw materials to form a mixed powder, and then subjecting the mixed powder to a boron / carbothermic reduction reaction under vacuum.

[0014] In a preferred embodiment, the molar ratio of TiO2, ZrO2, HfO2, V2O5, Ta2O5, B4C and carbon black is 3:3:3:1.5:1.5:5:33.

[0015] In a preferred embodiment, the boron / carbothermic reduction reaction conditions are: temperature of 1650℃~1800℃ and time of 1h~1.5h.

[0016] In a preferred embodiment, the ball milling speed is 400 rpm to 800 rpm, preferably 600 rpm, and the ball milling time is 10 h to 24 h, preferably 12 h.

[0017] A second objective of this invention is to provide a method for preparing whisker-toughened dual-phase high-entropy ceramic materials, comprising the following steps: SiC-B5 whiskers and dual-phase high-entropy powder were wet ball-milled to obtain SiC whisker / dual-phase high-entropy composite powder.

[0018] SiC whisker / dual-phase high-entropy composite powder was subjected to spark plasma sintering to obtain SiC whisker-toughened dual-phase high-entropy ceramic material.

[0019] In a preferred embodiment, the conditions for the discharge plasma sintering are: a heating rate of 100℃ / min to 120℃ / min, a sintering temperature of 1800℃ to 2000℃, a sintering pressure of 35MPa to 45MPa, and a time of 10min to 15min.

[0020] Compared with the prior art, the present invention has the following beneficial effects: The whisker-toughened dual-phase high-entropy ceramic material provided by this invention uses dual-phase high-entropy powder as a matrix and introduces SiC-B5 whiskers as a toughening phase dispersed in the matrix. Specifically, the differences in crystal structure, element affinity, and crack propagation path between the (TiZrHfTaV)B2 and (TiZrHfTaV)C phases in the matrix are utilized to construct a high-density phase interface, providing a basis for crack deflection and bifurcation. Simultaneously, the introduction of SiC-B5 whiskers as a one-dimensional toughening phase causes cracks in propagation to deflect, bridge, and pull out at the whiskers, thereby achieving multi-stage, multi-scale energy dissipation and ultimately effectively improving the fracture toughness and brittle fracture resistance of the material.

[0021] This invention introduces SiC-B5 whiskers to form one-dimensional toughening units within the matrix. When a crack propagates to the SiC-B5 whiskers, it is deflected due to changes in the local stress field, causing the crack to advance in a zigzag pattern along the SiC-B5 whisker / matrix interface, thereby increasing the fracture surface area and consuming some energy. As the crack continues to open, the whiskers spanning the crack surface act as "bridges," applying a closing stress of SiC-B5 whisker bridging behind the crack tip through interfacial friction and their own strength, resisting crack propagation and dissipating a large amount of energy. When the stress further increases to the point where the interface can no longer be maintained, the SiC-B5 whiskers are slowly pulled out of the matrix, and the work they do to overcome interfacial frictional resistance becomes the final energy absorption channel. These three processes are triggered sequentially and cooperate with each other, transforming the brittle fracture of a single crack propagation into a toughening mode of multi-path synergistic energy consumption, thereby effectively inhibiting rapid crack penetration and significantly improving the fracture toughness of the dual-phase high-entropy ceramic material.

[0022] The dual-phase high-entropy powder of this invention comprises a high-entropy boride phase and a high-entropy carbide phase, exhibiting a stable elemental selectivity distribution. V and Ti elements are mainly enriched in the high-entropy boride phase, while Hf, Ta, and Zr elements are mainly enriched in the high-entropy carbide phase. In this invention, the fracture toughness of the SiC-B5 whisker-toughened dual-phase high-entropy ceramic can reach 5.913 MPa·m. 1 / 2 It increases hardness by about 88.3% compared to the matrix without whiskers, while maintaining a hardness of 21.55 GPa, thus combining high hardness with excellent crack propagation resistance. Attached Figure Description

[0023] Figure 1 The images shown are SEM images of the SiC-B5 whisker material at different magnifications in Example 1 of this invention, where image a is the low-magnification morphology and image b is the high-magnification morphology.

[0024] Figure 2 The image shows the XRD pattern of SiC-B5 whiskers in Example 1 of this invention.

[0025] Figure 3 The XRD pattern of the boron / carbothermic reduction synthesis of biphase high-entropy powder in Example 1 of this invention is shown.

[0026] Figure 4 The images show the SEM morphology and EDS spot scan analysis of the two-phase high-entropy powder in Example 1 of the present invention, where Figure a shows the EDS spot scan images of different regions and Figure b shows the SEM morphology of the two-phase high-entropy powder.

[0027] Figure 5 The images show the SEM morphology and EDS elemental distribution of the two-phase high-entropy powder in Example 1 of this invention, used to characterize the spatial distribution of elements such as V, Ti, B, Zr, Ta, Hf, C, and Si.

[0028] Figure 6 The image shows the XRD pattern of the two-phase high-entropy ceramic powder in Example 1 of this invention.

[0029] Figure 7 This is a SEM image of the two-phase high-entropy ceramic matrix without added whiskers, as described in this invention.

[0030] Figure 8 The images show the SEM morphology of the SiC-B4 whisker / two-phase high-entropy composite powder of Comparative Example 2 and the SiC-B5 whisker / two-phase high-entropy composite powder of Example 2 of this invention. Figure a shows the SiC-B4 whisker / two-phase high-entropy composite powder, and Figure b shows the SiC-B5 whisker / two-phase high-entropy composite powder.

[0031] Figure 9 The XRD patterns are those of the SiC-B5 whisker-toughened dual-phase high-entropy ceramic of Example 2 and the SiC-B4 whisker-toughened dual-phase high-entropy ceramic of Comparative Example 2.

[0032] Figure 10 These are SEM images of the SiC-B5 whisker-toughened dual-phase high-entropy ceramic of Example 2 and the SiC-B4 whisker / dual-phase high-entropy ceramic of Comparative Example 2. Image a shows the SiC-B4 whisker-toughened dual-phase high-entropy ceramic at 10kx magnification; image b shows the SiC-B5 whisker-toughened dual-phase high-entropy ceramic at 10kx magnification; image c shows the SiC-B4 whisker-toughened dual-phase high-entropy ceramic at 20kx magnification; and image d shows the SiC-B5 whisker-toughened dual-phase high-entropy ceramic at 20kx magnification.

[0033] Figure 11 The images show the SEM images and EDS elemental distribution diagrams of the whisker-toughened dual-phase high-entropy ceramic of this invention.

[0034] Figure 12 This is a comparison chart of the relative density, Vickers hardness, and fracture toughness of the whisker-toughened dual-phase high-entropy ceramics of Example 2 and Comparative Example 2 of the present invention.

[0035] Figure 13 The images show the indentation crack morphology of the whisker-toughened dual-phase high-entropy ceramics of Embodiment 2 and Comparative Example 2 of the present invention. Images a and b show the indentation crack morphology of the SiC-B4 whisker-toughened dual-phase high-entropy ceramics at different fields of view, while images c and d show the indentation crack morphology of the SiC-B5 whisker-toughened dual-phase high-entropy ceramics at different fields of view.

[0036] Figure 14 The images show the SEM morphology of composite powders with different SiC-B5 whisker addition amounts in Examples 1 to 3 of the present invention, where image a represents 5wt% SiC-B5 whiskers, image b represents 10wt% SiC-B5 whiskers, and image c represents 15wt% SiC-B5 whiskers.

[0037] Figure 15The XRD patterns of two-phase high-entropy ceramics with different SiC-B5 whisker addition amounts in Examples 1 to 3 of this invention are shown.

[0038] Figure 16 The images show the SEM morphology of two-phase high-entropy ceramics with different SiC-B5 whisker addition amounts in Examples 1 to 3 of this invention.

[0039] Figure 17 The graph shows the effect of different SiC-B5 whisker addition amounts on the relative density, Vickers hardness and fracture toughness of dual-phase high-entropy ceramics in Examples 1 to 3 and Comparative Example 1 of this invention.

[0040] Figure 18 The images show the indentation crack propagation morphology of biphase high-entropy ceramics with different SiC-B5 whisker addition amounts in Examples 1 to 3 of the present invention. In Figure a, the indentation crack propagation morphology is 5 wt% SiC-B5 whisker, Figure b, the indentation crack propagation morphology is 10 wt% SiC-B5 whisker, and Figure c, the indentation crack propagation morphology is 15 wt% SiC-B5 whisker.

[0041] Figure 19 This is a comparison of the mechanical properties of the unadded whisker-based dual-phase matrix in Comparative Example 1 and the 5wt% SiC-B5 whisker-toughened dual-phase high-entropy ceramic in Example 1. Detailed Implementation

[0042] To enable those skilled in the art to better understand and implement the technical solutions of this invention, the invention will be further described below with reference to specific embodiments and accompanying drawings. In the description of this invention, unless otherwise specified, all reagents used are commercially available, and all methods used are conventional techniques in the art.

[0043] High-entropy ceramics, due to their multi-principal-element solid solution structure, high hardness, and good high-temperature stability, are considered important candidate structural materials for extreme service environments. However, their intrinsic brittleness leads to low fracture toughness. To address these issues, this invention provides a whisker-toughened dual-phase high-entropy ceramic and its preparation method.

[0044] The whisker-toughened dual-phase high-entropy ceramic material provided by the present invention is obtained by introducing SiC-B5 whiskers as a toughening phase using dual-phase high-entropy powder as the matrix.

[0045] The amount of SiC whiskers added is 5wt% to 15wt% based on the mass of the dual-phase high-entropy powder.

[0046] In the above technical solution, this invention constructs a (TiZrHfTaV)B2-(TiZrHfTaV)C dual-phase matrix using high-entropy borides (HEB) and high-entropy carbides (HEC), and introduces SiC whiskers as a toughening phase. The SiC-B5 whiskers can form one-dimensional toughening units within the matrix. Through crack deflection, whisker bridging, and whisker pull-out, energy is dissipated in synergy. When the crack propagates to the SiC-B5 whiskers, crack deflection occurs due to changes in the local stress field, causing the crack to propagate along the SiC-B5 whiskers. The whisker / matrix interface advances in a tortuous manner, increasing the fracture surface area and consuming some energy. As the crack continues to open, the SiC-B5 whiskers spanning the crack surface act as "bridges," applying bridging stress behind the crack tip through interfacial friction and their own strength, resisting crack propagation and dissipating a large amount of energy. When the stress further increases to the point where the interface can no longer be maintained, the SiC-B5 whiskers are slowly pulled out of the matrix, and the work done by them to overcome interfacial friction becomes the final energy absorption channel. These three processes are triggered sequentially and cooperate with each other, transforming the brittle fracture of a single crack propagation into a toughening mode of multi-path synergistic energy consumption, thereby effectively inhibiting the rapid propagation of cracks and significantly improving the fracture toughness of the dual-phase high-entropy ceramic material. At the same time, the dual-phase high-entropy powder is composed of high-entropy boride phases and high-entropy carbide phases, and has a stable elemental selectivity distribution; V and Ti elements are mainly enriched in the boride phase, while Hf, Ta, and Zr elements are mainly enriched in the carbide phase.

[0047] The technical solution of the present invention will be further illustrated below through the following embodiments and comparative examples.

[0048] Example 1 A method for preparing a whisker-toughened dual-phase high-entropy ceramic material includes the following steps: S1, weigh 1.251g of TiO2, 1.930g of ZrO2, 3.297g of HfO2, 3.462g of Ta2O5, 1.424g of V2O5, 1.298g of B4C and 2.164g of carbon black and mix them to obtain raw material powder.

[0049] S2, weigh raw material powder with a mass ratio of 3:1 and zirconia balls with a diameter of 10 mm, and mix them by ball milling at a speed of 600 rpm for 12 h to obtain mixed powder; place the mixed powder in a graphite crucible covered with carbon paper and put it into a vacuum pressureless furnace, heat it from room temperature to 1800℃ at a rate of 5℃ / min and hold it at that temperature for 1 h; then grind it, pass it through a 200-mesh sieve, wash it with water, centrifuge it and dry it at 100℃ for 12 h to obtain a two-phase high-entropy powder with the chemical formula (TiZrHfTaV)B2-(TiZrHfTaV)C.

[0050] S3, based on the mass of the dual-phase high-entropy powder, 5wt% SiC-B5 whiskers were weighed, added to anhydrous ethanol and ultrasonically dispersed for 30 min, and then mixed with dual-phase high-entropy powder by wet ball milling for 6 h. After ball milling, the resulting slurry was dried at 100℃ for 12 h to obtain 5wt% SiC-B5 / dual-phase high-entropy composite powder.

[0051] S4. 5wt% SiC-B5 / dual-phase high-entropy composite powder was loaded into a graphite mold with an inner diameter of 25mm and densified by spark plasma (SPS) sintering. The heating rate was 10℃ / min, the sintering temperature was 2000℃, the sintering pressure was 40MPa, and the holding time was 10min. After furnace cooling, 5wt% SiC-B5 whisker-toughened dual-phase high-entropy ceramic was obtained.

[0052] Example 2 A method for preparing a whisker-toughened dual-phase high-entropy ceramic material includes the following steps: S1, weigh 1.251g of TiO2, 1.930g of ZrO2, 3.297g of HfO2, 3.462g of Ta2O5, 1.424g of V2O5, 1.298g of B4C and 2.164g of carbon black and mix them to obtain raw material powder.

[0053] S2, weigh raw material powder with a mass ratio of 3:1 and zirconia balls with a diameter of 10 mm, and mix them by ball milling at a speed of 600 rpm for 12 hours to obtain mixed powder; place the mixed powder in a graphite crucible covered with carbon paper and put it into a vacuum pressureless furnace, heat it from room temperature to 1800℃ at a rate of 5℃ / min and hold it at that temperature for 1 hour; then grind it, pass it through a 200-mesh sieve, wash it with water, centrifuge it and dry it at 100℃ for 12 hours to obtain biphase high-entropy powder.

[0054] S3, based on the mass of the dual-phase high-entropy powder, 10wt% SiC-B5 whiskers were weighed, added to anhydrous ethanol and ultrasonically dispersed for 30min, and then mixed with dual-phase high-entropy powder by wet ball milling for 6h; after ball milling, the slurry was dried at 100℃ for 12h to obtain 10wt% SiC-B5 / dual-phase high-entropy composite powder.

[0055] S4, SPS sintering was performed according to step S4 of Example 1 to obtain 10wt% SiC-B5 whisker-toughened dual-phase high-entropy ceramic.

[0056] Example 3 A method for preparing a whisker-toughened dual-phase high-entropy ceramic material includes the following steps: S1, weigh 1.251g of TiO2, 1.930g of ZrO2, 3.297g of HfO2, 3.462g of Ta2O5, 1.424g of V2O5, 1.298g of B4C and 2.164g of carbon black and mix them to obtain raw material powder.

[0057] S2, weigh raw material powder with a mass ratio of 3:1 and zirconia balls with a diameter of 10 mm, and mix them by ball milling at a speed of 600 rpm for 12 hours to obtain mixed powder; place the mixed powder in a graphite crucible covered with carbon paper and put it into a vacuum pressureless furnace, heat it from room temperature to 1800℃ at a rate of 5℃ / min and hold it at that temperature for 1 hour; then grind it, pass it through a 200-mesh sieve, wash it with water, centrifuge it and dry it at 100℃ for 12 hours to obtain biphase high-entropy powder.

[0058] S3, based on the mass of the dual-phase high-entropy powder, 15wt% SiC-B5 whiskers were weighed, added to anhydrous ethanol and ultrasonically dispersed for 30min, and then mixed with dual-phase high-entropy powder by wet ball milling for 6h; after ball milling, the slurry was dried at 100℃ for 12h to obtain 15wt% SiC-B5 / dual-phase high-entropy composite powder.

[0059] S4, SPS sintering was performed according to step S4 of Example 1 to obtain 15wt% SiC-B5 whisker-toughened dual-phase high-entropy ceramic.

[0060] To further illustrate the technical effects of the present invention, a comparative example is also provided, as follows.

[0061] Comparative Example 1 A method for preparing a whisker-free two-phase high-entropy ceramic matrix includes the following steps: (TiZrHfTaV)B2-(TiZrHfTaV)C dual-phase high-entropy powder was prepared according to the steps of Example 1; without adding SiC-B5 whiskers, the dual-phase high-entropy powder was directly loaded into a graphite mold with an inner diameter of 25 mm, and SPS sintering was performed according to step S4 of Example 1 to obtain a dual-phase high-entropy ceramic matrix without added whiskers, which is denoted as composite ceramic.

[0062] Comparative Example 2 A method for preparing SiC-B4 whisker-toughened dual-phase high-entropy ceramic includes the following steps: S1, weigh 1.251g of TiO2, 1.930g of ZrO2, 3.297g of HfO2, 3.462g of Ta2O5, 1.424g of V2O5, 1.298g of B4C and 2.164g of carbon black and mix them to obtain raw material powder.

[0063] S2, weigh raw material powder with a mass ratio of 3:1 and zirconia balls with a diameter of 10 mm, and mix them by ball milling at a speed of 600 rpm for 12 hours to obtain mixed powder; place the mixed powder in a graphite crucible covered with carbon paper and put it into a vacuum pressureless furnace, heat it from room temperature to 1800℃ at a rate of 5℃ / min and hold it at that temperature for 1 hour; then grind it, pass it through a 200-mesh sieve, wash it with water, centrifuge it and dry it at 100℃ for 12 hours to obtain biphase high-entropy powder.

[0064] S3, based on the mass of the dual-phase high-entropy powder, 10wt% SiC-B4 whiskers were weighed, added to anhydrous ethanol and ultrasonically dispersed for 30min, and then mixed with dual-phase high-entropy powder by wet ball milling for 6h; after ball milling, the slurry was dried at 100℃ for 12h to obtain 10wt% SiC-B4 / dual-phase high-entropy composite powder.

[0065] S4, SPS sintering was performed according to step S4 of Example 1 to obtain 10wt% SiC-B4 whisker-toughened dual-phase high-entropy ceramic.

[0066] Figure 1 The images show the SEM morphology of SiC-B5 whisker raw materials at different magnifications. Low-magnification images show that the SiC-B5 whiskers exhibit an aggregate morphology, while high-magnification images show that the whiskers have a one-dimensional short rod-like or fibrous structure, with a diameter of approximately 80 nm to 150 nm and a length of approximately 0.5 μm to 8 μm, exhibiting a high aspect ratio. This one-dimensional structure is beneficial for forming toughening units in the ceramic matrix, such as crack deflection, whisker bridging, and whisker pull-out.

[0067] Figure 2 The image shows the XRD pattern of SiC-B5 whiskers. The pattern exhibits characteristic SiC diffraction peaks, and no obvious impurity peaks were observed, indicating that the SiC-B5 whiskers have high crystallinity and a relatively stable phase composition, making them suitable as an effective toughening phase for subsequent multiphase ceramics.

[0068] Figure 3 The XRD patterns of the boron / carbothermic reduction synthesized biphase high-entropy powder are shown. The results indicate that the obtained powder consists of a high-entropy boride phase and a high-entropy carbide phase, which maintain hexagonal and face-centered cubic structures, respectively. No obvious complex intermetallic compounds or impurity phases are observed, proving that this process can successfully prepare (TiZrHfTaV)B2-(TiZrHfTaV)C biphase high-entropy powder.

[0069] Figure 4The images show the SEM morphology and EDS spot scan analysis of the two-phase high-entropy powder. SEM results show that the overall powder morphology is relatively uniform, but localized melt adhesion and irregular agglomeration exist. Two typical grain types are visible in the powder: fine equiaxed particles mainly correspond to the carbide phase, while larger hexagonal prism or rod-shaped particles mainly correspond to the boride phase. The difference in the distribution of B and C elements in the EDS spot scan further confirms the coexistence of the two phases. The difference in morphology between the two phases stems from the difference in crystal structure: carbides have a cubic structure and easily form equiaxed grains; borides have a hexagonal structure and tend to grow anisotropically.

[0070] Figure 5 The images show the SEM morphology and EDS elemental distribution of the two-phase high-entropy powder. The EDS distribution reveals that V and Ti are mainly enriched in the boride phase region, while Hf, Ta, and Zr tend to be enriched in the carbide phase region, indicating a significant cation-selective distribution in this two-phase system. This distribution pattern may be related to the difference in standard enthalpy of formation between different transition metal elements and B / C atoms, and is important evidence for maintaining the HEB / HEC two-phase structure and elemental selectivity distribution pattern in this invention.

[0071] Figure 6 The XRD patterns of the two-phase high-entropy ceramic after SPS sintering are shown. The results indicate that the sintered ceramic still consists of HEB and HEC phases, without significant phase transformation or decomposition. Compared to the powder before sintering, the diffraction peaks are sharper and more intense, indicating that high-temperature sintering promotes grain development and increases crystallinity. The peak positions did not shift significantly, suggesting that the two phases maintained good structural stability during sintering.

[0072] Figure 7 The image shows the SEM morphology of the two-phase high-entropy ceramic matrix without SiC-B5 whiskers. The material is relatively dense overall, with good intergranular bonding and only a small amount of porosity. Under backscattered contrast, the HEB and HEC phases are distinguishable, and the two phases are relatively uniformly distributed with clear and continuous grain boundaries. This two-phase microstructure provides a stable matrix and a foundation for fracture inhibition at the phase interface during subsequent whisker toughening.

[0073] Figure 8 The images show the SEM morphology of SiC-B4 whiskers / two-phase high-entropy powder and SiC-B5 whiskers / two-phase high-entropy powder. Both types of whiskers can be mixed with the matrix powder, but SiC-B4 whiskers, due to their smaller diameter and ease of entanglement, exhibit slight local agglomeration; SiC-B5 whiskers are more uniformly distributed in the matrix, with no obvious large-area agglomeration, which is beneficial for subsequent SPS sintering densification and crack bridging toughening.

[0074] Figure 9XRD patterns of two-phase high-entropy ceramics toughened with whiskers of different specifications are shown. At the same 10wt% addition, both SiC-B4 and SiC-B5 samples retain the characteristic peaks of the (TiZrHfTaV)B2 and (TiZrHfTaV)C two-phase high-entropy matrix, indicating that the addition of whiskers did not destroy the two-phase matrix structure; at the same time, SiC-related diffraction peaks appeared, proving that SiC whiskers were successfully introduced.

[0075] Figure 10 SEM images of the toughened dual-phase high-entropy ceramics with SiC whiskers of different specifications were provided for this invention. Compared with the SiC-B4 sample, the SiC-B5 sample has a denser microstructure, more continuous intergranular bonding, and fewer pores and whisker agglomerations, indicating that the SiC-B5 whiskers have better composite compatibility with the HEB / HEC matrix.

[0076] Figure 11 SEM images and EDS elemental distribution diagrams of whisker-toughened dual-phase high-entropy ceramics are shown. The results show that Si is effectively introduced into the multiphase ceramics, while V and Ti are still mainly associated with the boride phase, and Hf, Ta, and Zr are still mainly associated with the carbide phase. This indicates that the addition of SiC whiskers does not disrupt the dual-phase structure and elemental selectivity of the matrix, and the whiskers have good chemical compatibility with the matrix.

[0077] Figure 12 This is a comparison of the mechanical properties of multiphase ceramics with different whisker specifications. As shown in Table 1, the relative density and fracture toughness of the 10wt% SiC-B5 multiphase ceramic reach 98.934% and 5.76 MPa·m, respectively. 1 / 2 All of them are higher than 10wt% SiC-B4 multiphase ceramics; although the SiC-B4 sample has higher hardness, SiC-B5 is more suitable as a whisker phase for toughening purposes.

[0078] Figure 13 The images show the indentation crack morphology of whisker / two-phase high-entropy composite powders of different specifications. The indentation crack propagation path of the SiC-B5 sample is more tortuous, with crack deflection, crack bridging and local pull-out signs visible, indicating that whiskers participate in energy dissipation at both the crack tip and the crack tail region. The toughening effect of the SiC-B4 sample is not as stable as that of SiC-B5 due to local agglomeration and entanglement.

[0079] Figure 14 SEM images of composite powders with different SiC-B5 whisker addition amounts are shown. As the SiC-B5 whisker addition amount increases from 5 wt% to 10 wt% and 15 wt%, the number of whiskers increases, but local agglomeration and overlapping phenomena become increasingly apparent. At 5 wt%, the whiskers are more uniformly dispersed, which is beneficial for forming an effective and continuous crack-blocking network.

[0080] Figure 15The XRD patterns of dual-phase ceramics with different SiC-B5 whisker additions are shown. The 5wt%, 10wt%, and 15wt% samples all retain the characteristic peaks of the HEB / HEC dual-phase high-entropy matrix, indicating that the matrix structure is stable under different whisker addition amounts. With the increase of SiC-B5 content, the SiC-related diffraction peaks are enhanced, proving that the SiC content in the dual-phase ceramics is related to the addition amount.

[0081] Figure 16 SEM images of dual-phase ceramics with different SiC-B5 addition amounts. The 5wt% sample is generally dense with relatively uniform whisker dispersion; the 10wt% sample has a higher relative density but an increased whisker content; the 15wt% sample shows more obvious local agglomeration and porosity, indicating that excessive whiskers will affect sintering densification.

[0082] Table 1 Mechanical properties of dual-phase ceramics with different SiC whisker specifications sample Whisker addition amount Relative density / % Vickers hardness / GPa <![CDATA[Fracture toughness / MPa·m 1 / 2 > Main conclusions <![CDATA[SiC-B4 dual-phase ceramic]]> 10wt% 95.505 24.858 5.255 It has high hardness, but lower density and toughness than B5. <![CDATA[SiC-B5 dual-phase ceramic]]> 10wt% 98.934 23.04 5.76 Better density and toughness As shown in Table 1, the relative density and fracture toughness of the 10wt% SiC-B5 sample reached 98.934% and 5.76 MPa·m, respectively. 1 / 2 The hardness of the 10wt% SiC-B4 sample is higher than that of the 10wt% SiC-B5 sample. Although the hardness of the 10wt% SiC-B4 sample is 24.858 GPa, which is higher than that of the 10wt% SiC-B5 sample (23.04 GPa), from the perspective of the comprehensive goal of improving fracture toughness and density, SiC-B5 whiskers are more suitable as the whisker toughening phase of the system of this invention.

[0083] Table 2 Mechanical properties of duplex ceramics with different SiC-B5 addition amounts sample Relative density / % Vickers hardness / GPa Fracture toughness / MPa·m1 / 2 evaluate No whisker matrix added 97.6 27.0±1.3 3.14±0.35 In comparison, it has the highest hardness but the lowest toughness. <![CDATA[5wt% SiC-B5]]> 97.417 21.55 5.913 Best toughened sample <![CDATA[10wt% SiC-B5]]> 98.934 23.04 5.76 Highest density and hardness <![CDATA[15wt% SiC-B5]]> 94.189 22.92 5.901 High toughness but decreased density From Table 2 and Figure 17 It can be seen that the material prepared without the addition of whiskers has the highest hardness but lower toughness; compared with the unadded whisker-based dual-phase high-entropy ceramic, the 5wt% SiC-B5 dual-phase ceramic, under similar relative density conditions, exhibits a fracture toughness that increases from 3.14 MPa·m. 1 / 2 Increased to 5.913 MPa·m 1 / 2 The hardness increased by approximately 88.3%; meanwhile, the hardness decreased from 27.0 GPa to 21.55 GPa, a decrease of approximately 20.2%. This indicates that an appropriate amount of SiC-B5 whiskers can significantly improve the material's resistance to crack propagation, but excessive whiskers can lead to defects such as agglomeration and porosity. Therefore, 5 wt% SiC-B5 is the preferred addition amount in this invention.

[0084] Figure 18Indentation crack propagation morphology of dual-phase ceramics with different SiC-B5 whisker additions. The whiskers in the 5wt% sample are more uniformly dispersed, and deflection and bridging are more likely to occur during crack propagation. Although the 10wt% and 15wt% samples have more whisker crack-inhibiting sites, local agglomeration, interface defects and porosity will weaken the uniform stress and densification effect.

[0085] Figure 19 The figure shows a comparison of the mechanical properties of a two-phase high-entropy ceramic matrix without whiskers and a two-phase ceramic matrix toughened with 5wt% SiC-B5 whiskers. Compared with the matrix without whiskers, the fracture toughness of the 5wt% SiC-B5 sample is significantly improved, indicating that the present invention effectively improves the crack propagation resistance by combining the crack inhibition at the phase interface of the two-phase matrix with the external toughening of SiC whiskers.

[0086] From the crack propagation morphology, crack deflection, whisker bridging and whisker pull-out are visible in the 5wt% SiC-B5 sample. The crack no longer propagates rapidly along a single path, but transforms into a multi-path, multi-resistance energy-consuming propagation process under the combined action of the two-phase interface and whiskers. In the 10wt% and 15wt% samples, local whisker agglomeration and pores may become stress concentration sources, weakening the overall toughening effect.

[0087] In summary, SiC-B5 whiskers can significantly improve the fracture toughness of materials without destroying the HEB / HEC dual-phase high-entropy matrix structure. Among them, the 5wt% SiC-B5 sample has the best overall performance and is suitable as the preferred embodiment of the present invention.

[0088] It should be noted that when numerical ranges are involved in this invention, it should be understood that the two endpoints of each numerical range, as well as any value between the two endpoints, can be selected. Since the steps and methods used are the same as in the embodiments, preferred embodiments are described in this invention to avoid redundancy. Although preferred embodiments of this invention have been described, those skilled in the art, once they understand the basic inventive concept, can make other changes and modifications to these embodiments, and all such changes and modifications fall within the scope of this invention.

[0089] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. If these modifications and variations fall within the scope of equivalents of this invention, then this invention also intends to include these modifications and variations.

Claims

1. A whisker-toughened dual-phase high-entropy ceramic material, characterized in that, The whisker-toughened dual-phase high-entropy ceramic material uses dual-phase high-entropy powder as the matrix and SiC-B5 whiskers as the toughening phase, with the toughening phase dispersed in the matrix. The dual-phase high-entropy powder comprises (TiZrHfTaV)B2 phase and (TiZrHfTaV)C phase; The SiC-B5 whiskers are added at a rate of 5 wt% to 15 wt% of the mass of the dual-phase high-entropy powder.

2. The whisker-toughened dual-phase high-entropy ceramic material according to claim 1, characterized in that, The SiC-B5 whiskers have a diameter of 80nm to 150nm and a length of 0.5μm to 8μm.

3. The whisker-toughened dual-phase high-entropy ceramic material according to claim 1, characterized in that, The fracture toughness of the whisker-toughened dual-phase high-entropy ceramic material is 5.76 MPa·m. 1 / 2 ~5.913MPa·m 1 / 2 Its Vickers hardness is 21.55 GPa to 23.04 GPa, and its relative density is 97.417% to 98.934%.

4. The whisker-toughened dual-phase high-entropy ceramic material according to claim 1, characterized in that, The dual-phase high-entropy powder is prepared by ball milling TiO2, ZrO2, HfO2, V2O5, Ta2O5, B4C and carbon black as raw materials to form a mixed powder, and then subjecting the mixed powder to a boron / carbothermic reduction reaction under vacuum.

5. The whisker-toughened dual-phase high-entropy ceramic material according to claim 4, characterized in that, The molar ratio of TiO2, ZrO2, HfO2, V2O5, Ta2O5, B4C and carbon black is 3:3:3:1.5:1.5:5:

33.

6. The method for preparing whisker-toughened dual-phase high-entropy ceramic material according to claim 4, characterized in that, The boron / carbothermic reduction reaction conditions are: temperature of 1650℃~1800℃, time of 1h~1.5h.

7. The method for preparing whisker-toughened dual-phase high-entropy ceramic material according to claim 4, characterized in that, The ball milling speed is 400 rpm to 800 rpm, and the ball milling time is 10 h to 24 h.

8. A method for preparing the whisker-toughened dual-phase high-entropy ceramic material according to any one of claims 1 to 7, characterized in that, Includes the following steps: SiC-B5 whiskers and dual-phase high-entropy powder were wet ball-milled to obtain SiC whisker / dual-phase high-entropy composite powder. SiC whisker / dual-phase high-entropy composite powder was subjected to spark plasma sintering to obtain SiC whisker-toughened dual-phase high-entropy ceramic material.

9. The method for preparing the whisker-toughened dual-phase high-entropy ceramic material according to claim 8, characterized in that, The conditions for the discharge plasma sintering are as follows: heating rate of 100℃ / min to 120℃ / min, sintering temperature of 1800℃ to 2000℃, sintering pressure of 35MPa to 45MPa, and time of 10min to 15min.