Preparation method of high-purity yttrium oxide ceramic

Through high-purity Y2O3 and YF3 at high temperature sintering and HIP treatment, high-density and low-impact yttrium oxide ceramics are prepared, which solves the problem of particle and metal pollution in semiconductor manufacturing of traditional ceramic materials, improves plasma resistance and meets the satisfaction of Higher semiconductor manufacturing standards.

CN118955136APending Publication Date: 2024-11-15SHANGHAI SILICON PRECISION CERAMICS TECH (SUZHOU) CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310497728.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In semiconductor manufacturing, the particle and metal contamination generated by traditional ceramic materials in plasma etching and cleaning processes is difficult to meet high requirements, especially in device manufacturing with sizes of 20nm or less, resulting in device defects and sintering of yttrium oxide ceramics There are challenges in densification.

Method used

The yttrium oxide ceramic material is prepared using high-purity Y2O3 powder and YF3 as additives sintered in a high-temperature vacuum or hydrogen atmosphere, combined with HIP treatment and air annealing to achieve high relative density and low cationic impurities.

Benefits of technology

Achieve higher purity and density yttrium oxide ceramics, significantly improve plasma resistance, meet higher semiconductor manufacturing needs, and reduce particle defects and metal pollution levels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004212851840000051
    Figure BDA0004212851840000051
  • Figure BDA0004212851840000061
    Figure BDA0004212851840000061
Patent Text Reader

Abstract

According to the preparation method of the high-purity yttrium oxide ceramic, YF3 is used as a sintering aid, densification of the yttrium oxide ceramic is promoted in a vacuum atmosphere, meanwhile, the removal effect on impurities such as Na, Si and Fe is achieved, and the high-purity yttrium oxide ceramic is obtained. The yttrium oxide ceramic is suitable for a plasma environment in semiconductor equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to rare earth oxide ceramic materials. Background Art

[0002] In the field of semiconductor manufacturing, plasma etching and plasma cleaning processes are important means of processing substrates. Plasma can be highly corrosive and can corrode the processing chamber and other surfaces exposed to the plasma. This corrosion can produce particles that often contaminate the substrate being processed, resulting in device defects. In addition, corrosion can cause metal atoms from chamber components to contaminate the processed wafers. For example, plasma-resistant ceramic covers and nozzles made using traditional ceramics may produce unacceptable levels of particle defects when used in plasma etching processes for semiconductor devices with critical dimensions of 20nm or less.

[0003] As the level and requirements of semiconductor manufacturing continue to improve, it is more sensitive to particle contaminants and metal atom contamination. Therefore, the allowable level of particle defects and metal contamination may continue to decrease. In order to solve the particle defects and metal contamination introduced by plasma etching or plasma cleaning processes, it is urgent to develop plasma-resistant chamber materials. Compared with traditional materials such as quartz, alumina, and aluminum nitride, yttrium oxide ceramics (Y2O3) exhibit excellent plasma resistance. However, the sintering temperature of yttrium oxide ceramics is higher, and its sintering densification is a key technical challenge. The conventional method is to add ZrO2, TiO2 or other oxides to promote its densification, but these added additives will introduce new metal ions, which may cause pollution to processes such as etching.

[0004] Therefore, the development of yttrium oxide ceramic materials with higher purity, higher density, and better plasma resistance has become an important issue in the field of semiconductor manufacturing. Summary of the invention

[0005] The invention discloses a preparation method of high-purity yttrium oxide ceramics. High-purity Y2O3 powder is used as a raw material, YF3 is used as an auxiliary agent, and high-temperature sintering is performed at 1600-1850° C. in a vacuum or hydrogen atmosphere to achieve Y2O3 ceramics with a relative density of not less than 98%, and the content of cationic impurities in the yttrium oxide ceramics is significantly reduced.

[0006] The preferred embodiment of the present invention also discloses that the sintered Y2O3 ceramic is subjected to HIP treatment at a pressure of 150-200 MPa and a high temperature of 1500-1700° C. to obtain a Y2O3 ceramic having a relative density of not less than 99.5%.

[0007] In order to eliminate the defects of the reducing atmosphere, preferably, the ceramics after vacuum sintering and HIP treatment need to be annealed in air.

[0008] Beneficial Effects

[0009] The rare earth yttrium oxide ceramic of the present invention has better purity and density than the existing alumina ceramics and yttrium oxide ceramics, thereby obtaining better plasma resistance and meeting higher requirements of plasma etching and plasma cleaning processes. DETAILED DESCRIPTION

[0010] The present invention will be further described in detail below with reference to the embodiments.

[0011] It is necessary to point out here that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the content of the present invention belong to the scope of protection of the present invention.

[0012] The melting point of yttrium fluoride is lower than that of yttrium oxide, so it can be used as a candidate material for the sintering aid of yttrium oxide ceramics. In addition, the effect of a small amount of residual fluorine on the plasma erosion resistance of yttrium oxide can be ignored, because both yttrium fluoride and yttrium oxyfluoride have good resistance to plasma, especially fluorine-containing plasma.

[0013] More importantly, yttrium fluoride can form volatile substances with sodium, silicon, iron, aluminum and other ions in yttrium oxide, and be removed from the yttrium oxide ceramic material during vacuum sintering.

[0014] Examples 1-5 provide the specific implementation process of the present invention for preparing yttrium oxide ceramics. Yttrium oxide powder and yttrium fluoride powder with a purity of 99.9% are used as raw materials, and the particle size of the raw materials is not greater than 10 μm. The raw materials are mixed evenly by ball milling, and the average particle size is less than 1 μm, so as to facilitate the subsequent sintering densification.

[0015] After sintering, the obtained ceramics were analyzed for main impurity content by glow discharge mass spectrometry (GM-MS), and the ceramic density was measured by Archimedes drainage method. The results are shown in Table 1.

[0016] Example 1

[0017] According to the ratio of YF3 content of 0.4wt%, two powders of yttrium oxide and yttrium fluoride were weighed, and anhydrous ethanol was used as the medium. The mixed powder with an average particle size of about 500nm was obtained by wet ball milling. After the obtained powder was sieved through a 200-mesh sieve, it was treated at a high temperature of 1200℃ to remove the hydroxyl and carbonate adsorbed on the surface. The impurity content test results of the obtained powder are shown in Table 1. The calcined powder was pressed into a blank by cold isostatic pressing technology at 200MPa. The blank was placed in a vacuum better than 5*10 -3Pa vacuum tungsten wire furnace sintering, heating at a rate of 5 ° C / min to 1600 ° C and keeping the temperature for 3 hours. The relative density and impurity content of the obtained yttrium oxide ceramics are shown in Table 1.

[0018] Example 2

[0019] According to the ratio of YF3 content of 0.4wt%, the two powders of yttrium oxide and yttrium fluoride were mixed and milled in the same manner as in Example 1. The obtained powder was calcined at 1000°C and isostatically pressed at a pressure of 200MPa. -3 Pa vacuum tungsten furnace, heated to 1600℃ at a rate of 5℃ / min for 3h, and then heated to 1800℃ for 10h to improve the purity of yttrium oxide. The obtained ceramic was treated in an air atmosphere at 1000℃ for 10h to eliminate the oxygen defects caused by vacuum. The measured density and impurity content are shown in Table 1.

[0020] Example 3

[0021] According to the ratio of YF3 content of 0.2wt%, the two powders of yttrium oxide and yttrium fluoride were mixed and ball-milled, and the mixing method was the same as in Example 1. After the obtained powder was passed through a 200-mesh sieve, it was pressed into a blank by cold isostatic pressing technology at 200MPa. The blank was heated to 1700℃ in a vacuum furnace at a rate of 2℃ / min and kept warm for 4h to obtain a yttrium oxide ceramic pre-sintered body. The pre-sintered body was treated in a hot isostatic pressing furnace at 1600℃ for 8h, and the pressure medium was high-purity Ar gas. The obtained ceramic was treated in an air atmosphere at 1000℃ for 10h to eliminate oxygen defects caused by vacuum. The measured density and impurity content are shown in Table 1.

[0022] Example 4

[0023] According to the ratio of YF3 content of 0.3wt%, the two powders of yttrium oxide and yttrium fluoride were mixed and milled in the same manner as in Example 1. The obtained powder was calcined at 1100°C, passed through a 200 mesh sieve, and then pressed into a green blank by cold isostatic pressing technology at 200MPa. The green blank was placed in a vacuum of better than 5*10 -3 Pa in a vacuum hydrogen furnace and keep the hydrogen flowing. The temperature was raised at a rate of 5°C / min to 1800°C and kept at that temperature for 20h to obtain yttrium oxide ceramics. The obtained yttrium oxide ceramics were treated in an air atmosphere at 1000°C for 10h to eliminate the oxygen defects caused by vacuum. The measured density and impurity content are shown in Table 1.

[0024] Example 5

[0025] According to the ratio of YF3 content of 0.1wt%, the two powders of yttrium oxide and yttrium fluoride are mixed and milled, and the mixing method is the same as that in Example 1.

[0026] The obtained powder was calcined at 1200℃ for solid phase reaction, then passed through a 200 mesh sieve, and then pressed into a green billet using cold isostatic pressing technology at 200MPa. -3 Pa vacuum tungsten furnace, and heated at a rate of 8 ° C / min to 1850 ° C for 25 hours to obtain a yttrium oxide ceramic pre-sintered body. The pre-sintered body was treated in a hot isostatic pressing furnace at 1700 ° C for 8 hours, and the pressure medium was high-purity Ar gas. The obtained ceramic was treated in an air atmosphere at 1000 ° C for 10 hours to eliminate the oxygen defects caused by vacuum. The measured density and impurity content are shown in Table 1.

[0027] Table 1 Density and impurity content of yttrium oxide ceramics

[0028]

[0029]

Claims

1. A method for preparing high-purity yttrium oxide ceramics, characterized in that High-purity Y2O3 powder is used as raw material, high-purity YF3 is used as auxiliary agent, and sintering is carried out at high temperature of 1600-1850℃ in vacuum or hydrogen atmosphere.

2. The method according to claim 1, characterized in that The purity of the high-purity Y2O3 powder and high-purity YF3 is above 99.9%.

3. The method according to claim 1, characterized in that The high-purity yttrium oxide ceramic is also subjected to hot isostatic pressing treatment at 1600-1700°C.

4. The method according to any one of claims 1 to 3, characterized in that The obtained yttria ceramics also need to be annealed in air at 1000°C.

Citation Information

Cited By

  • Preparation method of high-purity yttrium oxide target material based on Joule hot pressed sintering

    CN121377768A

  • A method for preparing high-purity yttrium oxide targets based on Joule hot pressing sintering

    CN121377768B