Bionic structure microwave absorbing coating and its preparation method

By constructing a biomimetic structure microwave absorbing coating through alternating layers of rare earth niobate and sheet-like SiC, the problems of high brittleness and low fracture toughness of SiC-based coatings at high temperatures are solved, achieving excellent microwave absorption performance and toughness in aerospace hot-end components.

CN123106221APending Publication Date: 2026-11-17NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611455233.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing SiC-based microwave absorbing coatings are brittle at high temperatures, have low fracture toughness, and poor microwave absorption performance, making them difficult to apply in aerospace hot-end components.

Method used

Rare earth niobate is used as a biomimetic "mud" phase material, and it is stacked alternately with sheet-like SiC to construct a biomimetic structure microwave absorbing coating. It is prepared by tape casting and hot pressing sintering to form a brick-mud alternating structure, which enhances the toughness and microwave absorption performance of the coating.

Benefits of technology

It achieves excellent radar wave absorption performance and good fracture toughness over a wide frequency range. The coating has good stability at high temperatures and is suitable for aerospace hot-end components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106221A_ABST
    Figure CN123106221A_ABST
Patent Text Reader

Abstract

This invention discloses a biomimetic structure absorbing coating and its preparation method. The biomimetic structure absorbing coating consists of a brick phase with a volume percentage of 50%-80% oriented lamellar SiC powder and a binder mud phase with a volume percentage of 20%-50%. Both the brick phase and the binder mud are layered structures, and the two phases are alternately stacked to form the coating. Referring to the multi-level microstructure of natural seashell nacre, lamellar silicon carbide is used as the main load-bearing brick phase, which is constructed by alternating layers of the brick phase and the mud phase. This structure causes frequent deflection, bridging, and bifurcation of cracks during propagation, efficiently dissipating impact energy, thereby endowing the coating with good fracture toughness. The interfacial polarization loss generated by the heterogeneous interface between the brick phase and the mud phase works synergistically to achieve excellent radar wave absorption performance over a wide frequency range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of functional ceramic coating technology, specifically to a biomimetic structure microwave absorbing coating and its preparation method. Background Technology

[0002] Silicon carbide (SiC) ceramics are considered ideal high-temperature microwave absorbing materials due to their excellent high-temperature stability, moderate dielectric constant, and good microwave absorption properties. However, the inherent high brittleness and low fracture toughness of intrinsic SiC ceramics are their fatal weaknesses. When subjected to mechanical impacts such as bird strikes, hail impacts, or high-speed particle erosion, traditional SiC-based microwave absorbing coatings are prone to microcracks or even catastrophic fragmentation, causing their protective and microwave absorption functions to fail instantly.

[0003] In nature, nacre is composed of over 95% brittle aragonite flakes as "bricks" and a small amount of soft organic matter as "mud," layered alternately at the micro- and nano-scale, yet exhibiting extremely high toughness and strength. Current technologies have attempted to incorporate this structure into ceramic materials, such as using alumina sheets and polymers to prepare biomimetic ceramics. However, the polymer "mud" phase in these materials cannot withstand high temperatures, limiting their application in aerospace hot-end components. Other studies have used metals as the "mud" phase, but the plastic deformation of metals intensifies at high temperatures, and their high conductivity often disrupts the impedance matching of the coating, severely impairing its microwave absorption performance.

[0004] Although rare earth niobates have been studied as high-temperature dielectric materials, there are no reports in the current technology of using them as the "mud" phase in a biomimetic "brick-mud" structure to alternately laminate with sheet-like SiC to construct microwave absorbing coatings. This is mainly because: 1) the sintering activity, interfacial compatibility with SiC, and thermal expansion matching of rare earth niobates have not been systematically studied; 2) the evolution law of their complex permittivity at high temperatures and their synergistic microwave absorption mechanism with SiC are still unclear. This application addresses these technological gaps by proposing for the first time a systematic solution using rare earth niobates as a high-temperature biomimetic "mud" phase material.

[0005] Therefore, there is an urgent need in this field to develop a novel microwave absorbing coating that can achieve a toughening mechanism similar to nacre in its microstructure, while also being able to withstand high temperatures and maintain good electromagnetic properties. Finding a high-temperature "mud" phase material that can simultaneously meet both mechanical and electromagnetic requirements is key to solving this technical challenge. It must simultaneously satisfy the following stringent requirements: 1) a melting point above 1200℃ and structural stability; 2) a thermal expansion coefficient matching that of SiC; 3) appropriate mechanical properties to transfer loads and dissipate energy; and 4) a suitable dielectric constant to maintain impedance matching. Existing material systems cannot simultaneously meet these conditions. Summary of the Invention

[0006] This invention provides a biomimetic structure microwave absorbing coating and its preparation method. By constructing a high-temperature resistant biomimetic structure microwave absorbing coating, it solves the technical bottlenecks of high brittleness, low fracture toughness and poor microwave absorption performance of existing traditional SiC high-temperature coatings.

[0007] The present invention provides the following technical solution: a biomimetic structure absorbing coating, which is composed of a brick phase of 50%-80% oriented sheet-like SiC powder and a binder mud phase of 20%-50% by volume. Both the brick phase and the binder mud phase are layered structures, and the two phases are alternately stacked to form a coating.

[0008] As an alternative to the biomimetic structure microwave absorbing coating described in this invention, the binder mud phase consists of 80%-90% RE n It consists of NbO4 powder, 5%-10% mechanically reinforcing phase, and 5%-10% microwave absorbing reinforcing phase. RE n NbO4 powder, n is an integer from 1 to 5, RE n Representing n different rare earth elements, each rare earth element is in an equimolar or near-equimolar ratio, where the mole fraction deviation of each rare earth element does not exceed 5%. Rare earth niobates were innovatively selected as the mud phase, thus successfully constructing a high-temperature resistant biomimetic microwave absorbing coating. RE is selected from Y, Gd, Tb, Dy, Ho, Er, Tm, Yb, or Lu. The aspect ratio of the flake-shaped SiC powder is 10:1 to 100:1, and the characteristic length is 5-100 μm. The average particle size of the mechanically reinforcing phase and the microwave absorbing phase is 20-100 nm.

[0009] It should be noted that in this application, the value of n ranges from 1 to 5, representing different choices of the amount of rare earth elements, but its core functional unit is always RE. n The NbO4 niobate system. Experimental results in this application show that, regardless of whether n=1 or 2≤n≤5, this mud-phase material can construct a biomimetic coating with a similar "brick-mud" structure with plate-like SiC, and achieves equally excellent performance levels in terms of absorption bandwidth and fracture toughness. This indicates that the change in the value of n does not affect the overall technical effect of this application and belongs to a general inventive concept.

[0010] A method for preparing a biomimetic structure microwave absorbing coating, comprising: Step 1: Prepare the powder for the binding mud phase, then mix it evenly with the solvent to obtain the mud phase slurry; Step 2: Mix the flake SiC powder with the solvent evenly to obtain the brick phase slurry; Step 3: The brick phase slurry and the clay phase slurry are cast into brick phase green body strips and clay phase green body strips respectively using the casting method; the brick phase green body strips and clay phase green body strips are alternately layered in a manner of one layer of brick phase strip and one layer of clay phase strip, so that the volume ratio of brick phase to clay phase is 50%-80%:20%-50%, to obtain a laminated green body; after the laminated green body is debonded, it is hot-pressed and sintered to form a ceramic coating. Step 4: Heat treat the coating at 650-850℃ for 1-2 hours to obtain a coating with a thickness of 1.5-2mm.

[0011] As an optional solution to the biomimetic structure absorbing coating preparation method of the present invention, wherein: Step 1 includes: weighing n rare earth oxides and niobium pentoxide powder in equimolar or near-equimolar ratios, mixing and ball milling them, drying the slurry, sieving it, and pressing it into a green body; heating the green body to 1400-1600℃ at a rate of 3-5℃ / min and holding it at that temperature for 4-10 hours to form a pre-sintered ceramic block, which is then crushed and ball-milled to obtain RE with an average particle size of 0.5-2μm. n NbO4 powder, RE n NbO4 powder, mechanically reinforcing phase powder, and microwave-absorbing reinforcing phase powder are mixed with solvent, and 2-5 wt% PVB as a binder, 1-3 wt% dioctyl phthalate (DOP) as a plasticizer, and 0.5-1.5 wt% triethanolamine as a dispersant are added and stirred evenly to obtain mud phase slurry.

[0012] Step 2 includes: mixing the flake SiC powder with a solvent, adding 1-3 wt% PVB as a binder and 0.5-1.5 wt% triethanolamine as a dispersant, stirring evenly to obtain a brick phase slurry.

[0013] Step 3 includes: using a casting method, casting brick phase slurry and clay phase slurry separately to obtain a brick phase green body with a thickness of 0.05-0.15mm and a clay phase green body with a thickness of 0.02-0.08mm; cutting the brick phase green body and clay phase green body, and stacking them alternately in layers of brick phase and clay phase to achieve a total thickness of 1.5-2mm; placing the stacked green bodies in a muffle furnace and heating them from room temperature to 600℃ at a rate of 1℃ / min and holding them for 1-3 hours to completely remove organic additives; placing the debonded green bodies in a graphite mold coated with a release agent and placing them in a vacuum hot pressing sintering furnace; the sintering procedure is: vacuum degree ≤10 -2 Pa, heating to 1550-1950℃ at 10℃ / min, applying axial pressure of 25-35MPa, holding at the temperature and pressure for 1-2 hours, and then cooling to room temperature with the furnace to obtain a ceramic coating with an alternating brick-mud layered microstructure.

[0014] The present invention has the following beneficial effects: 1. This biomimetic radar-absorbing coating mimics the multi-level microstructure of the nacreous layer of natural seashells. It utilizes sheet-like silicon carbide as the primary load-bearing "brick" phase and rare-earth niobate as the primary bonding "mud" phase, constructed through alternating layers. This structure causes frequent deflection, bridging, and bifurcation of cracks during propagation, efficiently dissipating impact energy and thus endowing the coating with good fracture toughness. The dielectric loss of silicon carbide and rare-earth niobate, combined with the interfacial polarization loss generated by the numerous "brick-mud" heterogeneous interfaces, achieves excellent radar wave absorption performance over a wide frequency range.

[0015] 2. The advantage of the brick-phase SiC in this biomimetic microwave absorbing coating structure lies in its ability to synergistically toughen the structure through multiple mechanisms when external impact loads induce cracks. When the crack extends to the hard brick-phase SiC, it cannot pass through in a straight line and is forced to deflect along the weaker "brick-mud" interface, lengthening the crack path, increasing the fracture surface area, and thus consuming more energy. When the crack opens, the brick-phase SiC at its tail acts like a bridge across the crack, generating a closing stress that directly resists further crack propagation. The brick-phase SiC transforms from the mud phase RE... n Pulling out of the NbO4 matrix requires overcoming enormous frictional forces, and this process is also a highly efficient energy dissipation process.

[0016] 3. The mud phase RE in this biomimetic microwave absorbing coating structure n The advantage of NbO4 lies in the fact that RE elements with different ionic radii are dissolved together in a single niobate lattice, forming a high-entropy rare-earth niobate solid solution. This solution is stable in a monoclinic zircon structure over a wide temperature range, has a high melting point (typically >1800℃), and can operate stably for extended periods above 1200℃. Furthermore, its coefficient of thermal expansion is more compatible with SiC, which helps reduce internal stress caused by thermal mismatch during preparation and service, improving the coating's bonding strength and thermal shock resistance. n NbO4 has a hardness and toughness between that of plate-like SiC and pure metals. It can effectively transfer and disperse stress, and can also undergo micro-plastic deformation or micro-cracking when subjected to stress, thereby dissipating energy.

[0017] 4. The sheet-like SiC and RE in this biomimetic microwave absorbing coating n During the heat treatment process following hot pressing sintering, micro-oxidation may occur on the surface of the lamellar SiC in NbO4 ceramic phases. The resulting SiO2 reacts with adjacent REs. n The NbO4 reaction has the potential to generate a thin layer of rare earth silicate (RE2Si2O7) in situ at the interface, which is expected to improve the interfacial bonding strength and high-temperature stability.

[0018] 5. This biomimetic absorbing coating exhibits excellent absorption performance. The periodically arranged "brick-and-mortar" interfaces form a massive array of microscopic capacitors. Under the influence of alternating electromagnetic fields, charges accumulate in large quantities at these heterogeneous interfaces, generating extremely strong interfacial polarization relaxation losses, which is the core mechanism for achieving broadband absorption. SiC provides the basic dielectric constant and conductivity loss, RE n NbO4 provides dielectric loss, and together the two optimize the overall complex dielectric constant of the coating, achieving good impedance matching from free space to the coating body and reducing electromagnetic wave reflection.

[0019] 6. The mud phase RE of this biomimetic structure microwave absorbing coating n The advantages of adding a dispersed nanoscale reinforcing phase to NbO4 are that the mechanical reinforcing phase improves the fracture toughness of the mud phase through the toughening mechanism of nanoparticles, crack deflection, and bridging; the microwave absorbing reinforcing phase has a high dielectric constant, which, as an additional electromagnetic wave loss supplement, enhances the overall microwave absorption capability of the coating.

[0020] 7. The preparation method of this biomimetic structure absorbing coating is to make the sheet SiC highly oriented in the green strip through the tape casting process, and then densify it by hot pressing and sintering after stacking. This method can obtain a coating with regular structure and excellent performance. Attached Figure Description

[0021] Figure 1 This is a schematic diagram of the internal structure of the coating protected in this application.

[0022] Figure 2 The image shows the reflection loss curve of the coating in Example 1. Detailed Implementation

[0023] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0024] The performance testing method in this application employs a vector network analyzer combined with a high-temperature waveguide testing system. Within the temperature range of room temperature to 1200°C, the reflection loss of the coating in the 2-18 GHz frequency band is tested using the bow-shaped method. The fracture toughness of the coating at room temperature is tested using the single-sided notched beam method on a universal testing machine. The absorption bandwidth is defined as the continuous frequency range with a reflection loss ≤ -5 dB. This threshold is suitable for evaluating the temperature-adaptive absorption characteristics of the coating over an extremely wide frequency range, meeting the basic requirement for wideband coverage in engineering applications.

[0025] The present application will be further described in detail below through five specific embodiments, but the scope of protection of the present application is not limited thereto. These embodiments demonstrate different rare earth element selections, preparation methods, and structural designs to verify the universality and excellent effects of the present application.

[0026] Example 1

[0027] The brick phase uses SiC with an aspect ratio of approximately 30:1 and an average length of 40 μm, with a volume ratio of 80%. The mud phase uses YbNbO4, with a volume ratio of 20%. The mechanical reinforcement phase is n-SiC, and the microwave absorption reinforcement phase is n-TiO2, with a total content of 10% of the mud phase and a volume ratio of 3:1. YbNbO4 powder, n-SiC, and n-TiO2 are mixed with a mixed solvent of anhydrous ethanol and butanone in a volume ratio of 1:1. 3 wt% PVB is added as a binder, 2 wt% DOP as a plasticizer, and 1 wt% triethanolamine as a dispersant, and the mixture is stirred evenly to obtain a mud phase slurry. Flake SiC powder is mixed with a mixed solvent of anhydrous ethanol and butanone, and 2 wt% PVB is added as a binder, 2 wt% DOP as a plasticizer, and 1 wt% triethanolamine as a dispersant, with a volume ratio of 2 wt% PVB as a binder, and 1 wt% triethanolamine as a dispersant. PVB (1% PVB) was used as a binder, and triethanolamine (1 wt%) was used as a dispersant. The mixture was stirred evenly to obtain a brick-phase slurry. Using a casting process, the brick-phase slurry and clay-phase slurry were cast separately to obtain a brick-phase green body with a thickness of approximately 0.10 mm and a clay-phase green body with a thickness of approximately 0.03 mm. The brick-phase and clay-phase green bodies were cut and then layered alternately with four layers of brick-phase and one layer of clay-phase, with a brick:clay volume ratio of approximately 80%:20%, to achieve a total thickness of 1.8 mm. The layered green bodies were placed in a muffle furnace and heated from room temperature to 600℃ at a rate of 1℃ / min for 2 hours to completely remove organic additives. The unbound green body was placed in a graphite mold coated with a release agent and then placed in a vacuum hot-pressing sintering furnace with a vacuum degree ≤10. -2 The temperature was increased to 1850℃ at 10℃ / min, and an axial pressure of 30MPa was applied. The temperature and pressure were maintained for 1 hour, and then the coating was cooled to room temperature in the furnace. The coating was then heat-treated at 800℃ for 1 hour to obtain a SiC / YbNbO4 biomimetic structure microwave absorbing coating.

[0028] Example 2

[0029] The brick phase uses SiC with an aspect ratio of approximately 10:1 and an average length of 15 μm, with a volume ratio of 65%; the clay phase uses [Y,Dy]NbO4, with a volume ratio of 35%; the mechanical reinforcement phase is n-Al2O3, and the microwave absorption reinforcement phase is n-CeO2, with a total content of 5% of the clay phase and a volume ratio of 4:1; Y2O3, Dy2O3, and Nb2O5 powders are accurately weighed in equimolar ratio; the weighed raw materials are then mixed with anhydrous ethanol. The alcohol mixture was ball-milled, the slurry was dried, sieved, and pressed into a green body. The green body was heated to 1400℃ at a rate of 3℃ / min and held for 10h to form a pre-sintered ceramic block, which was then crushed and ball-milled to obtain [Y,Dy]NbO4 with an average particle size of 0.5-2μm. The [Y,Dy]NbO4 powder, n-Al2O3, and n-CeO2 were mixed with a mixed solvent of anhydrous ethanol and butanone, and then a powder was added. A mud-phase slurry was prepared by mixing 3 wt% PVB, 2 wt% DOP, and 1 wt% triethanolamine by weight of the total material. Flake SiC powder was then mixed with a mixture of anhydrous ethanol and methyl ethyl ketone (MEK), and 2 wt% PVB and 1 wt% triethanolamine by weight of the powder were added and mixed thoroughly to obtain a brick-phase slurry. The brick-phase slurry and mud-phase slurry were cast separately to obtain a brick-phase green body with a thickness of approximately 0.15 mm and a mud-phase green body with a thickness of approximately 0.08 mm. Approximately two layers of brick-phase green body and one layer of mud-phase green body were alternately layered, with a brick:mud volume ratio of approximately 65%:35%, to achieve a total thickness of 2.0 mm. The layered green bodies were placed in a muffle furnace and heated from room temperature to 600℃ at a rate of 1℃ / min for 2 hours to completely remove organic additives. The debinded green body was placed in a graphite mold coated with a release agent and then placed in a vacuum hot-pressing sintering furnace with a vacuum degree ≤10. -2 Pa, heated to 1550℃ at 10℃ / min, applied axial pressure of 25MPa, held at the temperature and pressure for 1.5h, and then cooled to room temperature in the furnace; the coating was then heat-treated at 800℃ for 1h to obtain a SiC / [Y,Dy]NbO4 biomimetic structure microwave absorbing coating.

[0030] Example 3

[0031] The brick phase uses SiC with an aspect ratio of approximately 100:1 and an average length of 100 μm, with a volume ratio of 55%; the clay phase uses [Y,Dy,Yb]NbO4, with a volume ratio of 35%; the mechanical reinforcement phase is n-YSZ, and the microwave absorption reinforcement phase is n-Ga2O3, with a total content of 5% of the clay phase and a volume ratio of 5:1; Y2O3, Dy2O3, Yb2O3, and Nb2O5 powders are accurately weighed in equimolar ratio; the weighed raw materials are mixed with anhydrous ethanol and ball-milled; the slurry is dried, sieved, and pressed into a green body; the green body is then heated at a rate of 5℃ / min. The temperature was raised to 1550℃ and held for 6 hours to form a pre-sintered ceramic block. After crushing and ball milling, [Y,Dy,Yb]NbO4 powder with an average particle size of 0.5-2μm was obtained. The mud phase slurry consisted of [Y,Dy,Yb]NbO4 powder, n-YSZ, n-Ga2O3 and solvent, 3wt% PVB, 2wt% DOP and 1wt% triethanolamine. The brick phase slurry consisted of flake SiC and solvent, 2wt% PVB and 1wt% triethanolamine. The bricks were cast separately, with a brick strip thickness of about 0.12mm and a mud strip thickness of about 0.08mm. The brick and mortar strips are alternately layered, with a brick:mortar volume ratio of approximately 55%:35%, and a total thickness of 1.5 mm. The laminated body is placed in a muffle furnace and heated from room temperature to 600°C at a rate of 1°C / min, and held for 1.5 hours. The unglazed blank after debinding is placed in a graphite mold coated with a release agent and then placed in a vacuum hot-pressing sintering furnace with a vacuum degree ≤10. -2 The temperature was increased to 1750℃ at 10℃ / min, and an axial pressure of 30MPa was applied. The temperature and pressure were maintained for 1 hour, and then the coating was cooled to room temperature in the furnace. Finally, the coating was heat-treated at 750℃ for 1 hour to obtain the SiC / [Y,Dy,Yb]NbO4 microwave absorbing coating.

[0032] Example 4

[0033] The brick phase uses SiC with an aspect ratio of approximately 80:1 and an average length of 90 μm, with a volume ratio of 80%. The clay phase uses [Y,Dy,Yb,Gd]NbO4, with a volume ratio of 20%. The mechanical reinforcement phase is n-SiC, and the microwave absorption reinforcement phase is n-TiO2, with a total content of 10% of the clay phase and a volume ratio of 3:1. Y2O3, Dy2O3, Yb2O3, Gd2O3, and Nb2O5 powders are accurately weighed in equimolar or near-equimolar ratios. The weighed raw materials are then mixed with anhydrous acetylene... The alcohol mixture was ball-milled, the slurry was dried, sieved, and pressed into a green body. The green body was heated to 1500℃ at a rate of 5℃ / min and held for 5h to form a pre-sintered ceramic block. This block was then crushed and ball-milled to obtain [Y,Dy,Yb,Gd]NbO4 powder with an average particle size of 0.5-2μm. The [Y,Dy,Yb,Gd]NbO4 powder, n-SiC, and n-TiO2 were mixed with a 1:1 volume ratio of anhydrous ethanol and butanone as a mixed solvent. The mixture was added to the total mass of the powder. 3 wt% PVB was used as a binder, 2 wt% DOP as a plasticizer, and 1 wt% triethanolamine as a dispersant. The mixture was stirred until homogeneous to obtain a mud-phase slurry. Flake-shaped SiC powder was mixed with a mixture of anhydrous ethanol and methyl ethyl ketone (MEK), and 2 wt% PVB (as a binder) and 1 wt% triethanolamine (as a dispersant) were added. The mixture was stirred until homogeneous to obtain a brick-phase slurry. The brick-phase slurry and mud-phase slurry were cast separately using a casting method to obtain bricks with a thickness of approximately 0.12 mm. The process involves preparing a brick-phase green body and a clay-phase green body with a thickness of approximately 0.03 mm. After cutting the brick-phase and clay-phase green bodies, they are layered alternately with four layers of brick-phase green body and one layer of clay-phase green body, with a brick:clay volume ratio of approximately 80%:20%, resulting in a total thickness of 2.0 mm. The laminated body is placed in a muffle furnace and heated from room temperature to 600℃ at a rate of 1℃ / min, holding for 2 hours to completely remove organic additives. The unbleached green body is then placed in a graphite mold coated with a release agent and placed in a vacuum hot-pressing sintering furnace with a vacuum degree ≤10. -2 The temperature was increased to 1850℃ at 10℃ / min, and an axial pressure of 30MPa was applied. The temperature and pressure were maintained for 1.5h, and then the coating was cooled to room temperature in the furnace. Finally, the coating was heat-treated at 700℃ for 1h to obtain the SiC / [Y,Dy,Yb,Gd]NbO4 microwave absorbing coating.

[0034] Example 5

[0035] The brick phase uses SiC with an aspect ratio of approximately 50:1 and an average length of 60 μm, with a volume ratio of 70%; the clay phase uses [Y,Dy,Yb,Gd,Tb]NbO4, with a volume ratio of 30%; the mechanical reinforcement phase is n-SiC, and the microwave absorption reinforcement phase is n-Ga2O3, with a total content of 13% of the clay phase and a volume ratio of 5:1; Y2O3, Dy2O3, Yb2O3, Gd2O3, Tb2O3, and Nb2O5 powders are accurately weighed in equimolar or near-equimolar ratios; the weighed raw materials are then... The material was mixed with anhydrous ethanol and ball-milled. The slurry was dried, sieved, and pressed into a green body. The green body was heated to 1600℃ at a rate of 5℃ / min and held for 8 hours to form a pre-sintered ceramic block. After crushing and ball milling, [Y,Dy,Yb,Gd,Tb]NbO4 powder with an average particle size of 0.5-2μm was obtained. The [Y,Dy,Yb,Gd,Tb]NbO4 powder, n-SiC, and n-Ga2O3 were mixed with a 1:1 volume ratio of anhydrous ethanol and butanone as a solvent. Add 3 wt% PVB as a binder, 2 wt% DOP as a plasticizer, and 1 wt% triethanolamine as a dispersant to the total powder mass, and stir evenly to obtain a mud-phase slurry. Mix the flake SiC powder with a mixed solvent of anhydrous ethanol and methyl ethyl ketone, add 2 wt% PVB as a binder and 1 wt% triethanolamine as a dispersant to the total powder mass, and stir evenly to obtain a brick-phase slurry. Use a casting molding method to cast the brick-phase slurry and mud-phase slurry separately to obtain a thickness of approximately 0.12 mm. The green body consists of a brick phase green strip with a thickness of approximately 0.05 mm and a clay phase green strip with a thickness of approximately 0.05 mm. After cutting the brick and clay phase green strips, they are layered alternately with two layers of brick phase green strip and one layer of clay phase green strip, with a brick:clay volume ratio of approximately 70%:30%, resulting in a total thickness of 1.9 mm. The laminated body is placed in a muffle furnace and heated from room temperature to 600℃ at a rate of 1℃ / min, holding for 3 hours to completely remove organic additives. The unbleached green body is then placed in a graphite mold coated with a release agent and placed in a vacuum hot-pressing sintering furnace with a vacuum degree ≤10. -2 The temperature was increased to 1850℃ at 10℃ / min, and an axial pressure of 35MPa was applied. The temperature and pressure were maintained for 2 hours, and then the coating was cooled to room temperature in the furnace. Finally, the coating was heat-treated at 750℃ for 2 hours to obtain the SiC / [Y,Dy,Yb,Gd,Tb]NbO4 microwave absorbing coating.

[0036] Table 1 shows the specific performance of the biomimetic structure microwave absorbing coatings prepared by the casting method in Examples 1-5:

[0037] Figure 1 This is a schematic diagram of the internal structure of the biomimetic absorbing coating protected in this application. Figure 2The reflection loss curves of the coating in Example 1 in the 2-18 GHz frequency band are shown, and its absorption bandwidth (≤-5 dB) reaches 8.9 GHz in the 8-18 GHz band. The microwave absorption performance of the coatings in Examples 1-5 was measured at 1200℃, and the fracture toughness was measured at room temperature. As can be seen from Table 1, the biomimetic structure microwave absorbing coatings prepared by the above steps, with a thickness of 1.5-2.0 mm, tested at 1200℃, all exhibited absorption bandwidth (≤-5 dB) above 8 GHz, minimum reflection loss <-10 dB, and fracture toughness generally above 7 MPa·m. 1 / 2 The above demonstrates that the biomimetic structure absorbing coating in this application possesses excellent microwave absorption performance, toughness, and high-temperature resistance.

[0038] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

[0039] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A biomimetic structure microwave absorbing coating, characterized in that, It consists of a brick phase, which comprises 50%-80% by volume of oriented sheet-like SiC powder, and a binder phase, which comprises 20%-50% by volume. Both the brick phase and the binder phase are layered structures, and the two phases are alternately layered to form a coating.

2. The biomimetic structure absorbing coating according to claim 1, characterized in that: The binder mud phase consists of 80%-90% RE n It consists of NbO4 powder, 5%-10% mechanical reinforcement phase and 5%-10% microwave absorption reinforcement phase.

3. The biomimetic structure absorbing coating according to claim 2, characterized in that: RE n NbO4 powder, n is an integer from 1 to 5, RE n It represents n different rare earth elements, and each rare earth element is in an equimolar ratio or a near equimolar ratio. A near equimolar ratio means that the mole fraction of each rare earth element does not exceed 5%.

4. The biomimetic structure absorbing coating according to claim 2, characterized in that: RE is selected from Y, Gd, Tb, Dy, Ho, Er, Tm, Yb, or Lu.

5. The biomimetic structure absorbing coating according to claim 2, characterized in that: The mechanical reinforcement phase is selected from at least one of silicon carbide, aluminum oxide, and yttrium-stabilized zirconium oxide; the microwave absorption reinforcement phase is selected from at least one of titanium dioxide, cerium oxide, and gallium oxide.

6. The biomimetic structure absorbing coating according to claim 1 or 2, characterized in that: The aspect ratio of the flake-shaped SiC powder is 10:1 to 100:1, and the characteristic length is 5-100 μm.

7. The biomimetic structure absorbing coating according to claim 2, characterized in that: The average particle size of the mechanically enhanced phase and the microwave-absorbing enhanced phase is 20-100 nm.

8. A method for preparing a biomimetic structure microwave absorbing coating, used to prepare the biomimetic structure microwave absorbing coating according to any one of claims 1-7, characterized in that: include: Step 1: Prepare the powder for the binding mud phase, then mix it evenly with the solvent to obtain the mud phase slurry; Step 2: Mix the flake SiC powder with the solvent evenly to obtain the brick phase slurry; Step 3: The brick phase slurry and the clay phase slurry are cast into brick phase green belts and clay phase green belts respectively using the casting molding method; The brick phase green body and the clay phase green body are alternately layered in a manner of one layer of brick phase and one layer of clay phase, so that the volume ratio of brick phase to clay phase is 50%-80%:20%-50%, to obtain a laminated green body; after the laminated green body is debonded, it is hot-pressed and sintered to form a ceramic coating. Step 4: Heat treat the coating at 650-850℃ for 1-2 hours to obtain a coating with a thickness of 1.5-2mm.

9. The biomimetic structure absorbing coating according to claim 8, characterized in that: Step 1 includes: weighing n rare earth oxides and niobium pentoxide powder in equimolar or near-equimolar ratios, mixing and ball milling them, drying the slurry, sieving it, and pressing it into a green body; heating the green body to 1400-1600℃ at a rate of 3-5℃ / min and holding it at that temperature for 4-10 hours to form a pre-sintered ceramic block, which is then crushed and ball-milled to obtain RE with an average particle size of 0.5-2μm. n NbO4 powder, E n NbO4 powder, mechanically reinforcing phase powder, and microwave-absorbing reinforcing phase powder are mixed evenly with solvent, and binder, plasticizer, and dispersant are added and stirred evenly to obtain mud-phase slurry.

10. The biomimetic structure absorbing coating according to claim 8, characterized in that: In step 2: the flake SiC powder is mixed with a solvent, and a binder and dispersant are added and stirred evenly to obtain a brick phase slurry.