A fluorinated polyester polyol, its preparation method and application

By synthesizing fluorinated diols to prepare fluorinated polyester polyols, the problems of insufficient chemical resistance and thermal stability of traditional polyester polyols are solved, and polyurethane adhesives suitable for high-end fields are prepared with excellent thermal stability and chemical inertness.

CN123106370APending Publication Date: 2026-11-17NANTONG GAOMENG NEW MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611348865.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional polyester polyols have shortcomings in chemical resistance and thermal stability, which affect the stability and lifespan of adhesives in certain environments.

Method used

Fluorinated polyester polyols were prepared by designing and synthesizing fluorinated diols as monomers, and then polyurethane adhesives were synthesized by reacting them with isocyanates. The reaction was carried out under mild light conditions and with a specific catalyst to form polyurethane adhesives with high chemical resistance and thermal stability.

Benefits of technology

The improved thermal stability and chemical inertness of polyurethane adhesives make them suitable for high-end applications such as cable insulation materials, battery technology, and aerospace, exhibiting excellent weather resistance and low surface energy properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106370A_ABST
    Figure CN123106370A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of polyester polyol preparation technology, specifically relating to a method for preparing fluorinated polyester polyol and synthesizing polyurethane adhesives therein. The method includes the following steps: S1: synthesizing a fluorinated diol from α,ω-diiodoperfluoroalkane, enol, catalyst, and organic solvent under light irradiation; S2: feeding a diacid, polyol, and fluorinated diol in a certain proportion, and performing esterification and polycondensation to obtain the fluorinated polyester polyol; S3: mixing the prepared fluorinated polyester polyol as component A with a polyisocyanate as component B in a certain proportion to obtain a polyurethane adhesive. This invention designs and synthesizes a fluorinated diol, prepares a fluorinated polyester polyol, and then synthesizes a fluorinated adhesive. The resulting adhesive exhibits excellent thermal stability, maintaining stable properties over a wider temperature range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of adhesive technology, specifically to a fluorinated polyester polyol, its preparation method, and its application in the preparation of polyurethane adhesives. Background Technology

[0002] Fluorine atoms have small radii, lone pairs of electrons, high electronegativity, low polarizability, and high CF bond energy (540 kJ / mol), resulting in stable polymers. These properties of fluorine make fluoropolymers far superior to other polymers in many aspects, such as excellent water and oil resistance, thermal stability, low surface tension, and corrosion resistance. These properties make fluoropolymers extremely promising for applications in functional coatings, biomedical materials, and surfactants.

[0003] Polyester polyols are important raw materials for the preparation of polyurethanes and have wide applications in adhesives, coatings, and elastomers. However, traditional polyester polyols suffer from poor weather resistance or chemical resistance due to limitations in their chemical structure. In certain environments, adhesives may fail due to chemical corrosion or temperature changes, affecting the stability and lifespan of the material. Therefore, developing a fluorinated polyester polyol with high chemical resistance and thermal stability is particularly important, providing potential applications for polyurethane adhesives in specific fields. Summary of the Invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the limitations of the chemical structure of traditional polyester polyols, such as insufficient chemical resistance and thermal stability, and to provide a method for preparing fluorinated polyester polyols and a method for preparing polyurethane adhesives. Specifically, the method involves designing and synthesizing a fluorinated diol as a monomer to prepare polyester polyols, thereby obtaining fluorinated polyester polyols, which are then synthesized with isocyanates to form polyurethane adhesives.

[0005] The first objective of this invention is to provide a fluorinated diol with the following structural formula: , Where n = 1-6, m = 2-4; n and m are integers.

[0006] The method for preparing the fluorinated diol includes the following steps: S1: α,ω-diiodoperfluoroalkane, enol, catalyst halogen salt and organic solvent are mixed and reacted under light to obtain a reaction solution; S2: Perform column chromatography on the reaction solution in step S1 to obtain the fluorinated diol.

[0007] In one embodiment of the present invention, after mixing in step S1, a deoxygenation treatment is performed, the deoxygenation treatment including the introduction of an inert gas.

[0008] In step S1, the α,ω-diiodoperfluoroalkane is one or more of 1,6-diiodoperfluorohexane, 1,4-diiodoperfluorobutane, and 1,8-diiodoperfluorooctane.

[0009] Preferably, the α,ω-diiodoperfluoroalkane is 1,6-diiodoperfluorohexane.

[0010] In one embodiment of the present invention, in step S1, the enol is one or more of 3-buten-1-ol, 4-penten-1-ol, and 5-hexen-1-ol; preferably, the enol is 5-hexen-1-ol.

[0011] In one embodiment of the present invention, in step S1, the catalyst is a halogen salt, selected from sodium iodide, sodium chloride, and sodium bromide; preferably, the catalyst is sodium iodide.

[0012] In one embodiment of the present invention, in step S1, the organic solvent is selected from one or more of dimethylacetamide, acetone, tetrahydrofuran, dimethyl carbonate and acetonitrile; preferably, the organic solvent is acetone.

[0013] In one embodiment of the present invention, in step S1, the wavelength of the illumination is 373-403 nm; preferably, the wavelength of the illumination is 403 nm.

[0014] In one embodiment of the present invention, in step S2, the column chromatography eluent is petroleum ether / ethyl acetate = 20~4 / 1 by volume. Preferably, the ratio of petroleum ether to ethyl acetate is 10 / 1.

[0015] In one embodiment of the present invention, after step S2, the prepared fluorinated diol is subjected to 1H NMR and 1C NMR standards.

[0016] The principle of this invention is as follows: when the catalyst is irradiated with visible light, it absorbs energy and undergoes intramolecular single electron transfer, which combines with the terminal iodine of α,ω-diiodoperfluoroalkane to form a bonded electron donor-acceptor complex. Under mild conditions, a free radical intermediate is generated, which then undergoes addition with the terminal double bond of the enol to form a fluorinated diol with hydroxyl groups at both ends.

[0017] The second objective of this invention is to provide a method for preparing fluorinated polyester polyols, comprising the following steps: feeding fluorinated diols, diacids, and polyols in a certain proportion, and carrying out esterification and polycondensation reactions to obtain fluorinated polyester polyols.

[0018] In one embodiment of the present invention, the dicarboxylic acid is one or more of glutaric acid, adipic acid, and azelaic acid; preferably, the dicarboxylic acid is adipic acid.

[0019] In one embodiment of the present invention, the polyol is one or more of 1,4-butanediol, 2-methyl-1,3-propanediol, diethylene glycol, and glycerol; preferably, the polyol is 2-methyl-1,3-propanediol or diethylene glycol.

[0020] In one embodiment of the present invention, the esterification reaction is carried out by introducing nitrogen gas at 145-155 °C. o React under stirring for 1-2 hours, aiming for a water output of 45%-55% of the theoretical value. Continue heating to 156-190°C. o React at C for 1.5-2 hours, aiming for an output flow rate of 80%-90% of the theoretical value, then continue heating to 191-230°C. o The C reaction takes 1.5-2 hours, requiring the effluent flow rate to reach 91%-100% of the theoretical value; the polycondensation reaction is carried out under vacuum at 230-240°C. o Pre-polymerize at -0.02 MPa for about 0.5-1 hour, then gradually reduce the vacuum to -0.09 MPa, and then pump for 10-15 minutes.

[0021] A third objective of this invention is to provide a polyurethane adhesive comprising component A and component B, wherein component A comprises the aforementioned fluorinated polyester polyol, and component B comprises a polyisocyanate, wherein the mass ratio of component A to component B is 1:1 to 1.4.

[0022] The preparation method of the above-mentioned polyurethane adhesive includes the following steps: mixing component A and component B in a mass ratio of 1:1 to 1.4 to prepare the polyurethane adhesive.

[0023] In one embodiment of the present invention, the polyisocyanate is one or both of 4,4'-methylene bis(phenyl isocyanate) (MDI) and toluene-2,4-diisocyanate (TDI); preferably, the polyisocyanate is MDI.

[0024] In one embodiment of the present invention, the mass ratio of component A to component B is preferably 1:1.2.

[0025] By means of the above-described solution, the present invention has at least the following advantages: This invention introduces fluorine atoms into the preparation of polyester polyols from a small molecule design perspective, based on the characteristics of fluorine (high electronegativity, low polarizability, small van der Waals radius (1.32 Å)) and C−F bonds (485 kJ mol). −1Fluorinated polyester polyols may exhibit unique properties, such as excellent thermal stability, chemical inertness, weather resistance, low surface energy, and unique electrical properties. Therefore, the polyurethane adhesives prepared from them can be applied in some unique high-end fields, such as cable insulation materials, adhesives used as electrodes in battery technology, solar cell coatings, and aerospace. Simultaneously, the synthesis of fluorinated diol monomers is carried out under room temperature and light irradiation, with mild reaction conditions and simple operation. Attached Figure Description

[0026] Figure 1 The fluorinated diol monomer A in Example 1 of this invention 1 1H NMR test results.

[0027] Figure 2 The 1,6-diiodoperfluorohexane monomer in Example 1 of this invention 1 F NMR test results.

[0028] Figure 3 The fluorinated diol monomer A in Example 1 of this invention 1 F NMR test results.

[0029] Figure 4 This is the GPC effluent curve of the polyester polyol in Example 2 of the present invention.

[0030] Figure 5 This is the GPC effluent curve of the polyester polyol in Example 3 of the present invention. Detailed Implementation

[0031] The following embodiments are provided to better understand the present invention and are not limited to the preferred embodiments described. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.

[0032] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.

[0033] Unless otherwise specified, the temperature in the embodiments of the present invention is room temperature or ambient temperature; room temperature or ambient temperature refers to 25±1℃.

[0034] The chemical reagents involved in this invention are as follows: 1,6-Diiodoperfluorohexane (98%, TCI); 5-Hexen-1-ol (97%, Aladdin); Sodium iodide (99%, TCI); Acetone (AR, Qiangsheng); Petroleum ether (AR, Qiangsheng); Ethyl acetate (AR, Qiangsheng); Adipic acid (99%, Aladdin); 2-Methyl-1,3-propanediol (99%, Alfa Aesar); Diethylene glycol (98%, Aladdin).

[0035] The detection method involved in this invention is as follows: 1. Fluorinated diol monomer A 1 The 1H NMR spectra were obtained using a Bruker 300 MHz nuclear magnetic resonance (NMR) instrument. The tests were performed at room temperature (25 °C) with CDCl3 as the deuterated reagent and tetramethylsilane (TMS) as the internal standard.

[0036] 2. Molecular weight of polyester polyols ( M n,GPC ) and molecular weight distribution index ( Ð The molecular weight was determined using a TOSOH HLC-8320 gel permeation chromatography (GPC) system equipped with a differential refractive index detector (TOSOH). The instrument used a Waters 2414 refractive index detector and a TSKgel Super AWM-H column (4.6 mm ID * 15 cm * 2). The molecular weight range was 10. 3 Up to 10 6 g / mol. Tetrahydrofuran was used as the eluent at a flow rate of 0.35 mL / min. GPC samples were injected using a TOSOH plus autosampler, with PMMA purchased from TOSOH as the standard.

[0037] 3. The peel force of the composite film was measured by a computer-controlled electronic universal testing machine (CMT6202). Example 1

[0038] A method for preparing a fluorinated diol monomer A includes the following steps: dissolving a mixture of monomers 1,6-diiodoperfluorohexane (0.25 mol), 5-hexen-1 alcohol (0.60 mol), and sodium iodide (0.25 mol) in 250 mL of acetone, and adding the solution to a three-necked flask equipped with a clean stir bar, then purging with nitrogen to maintain an inert environment. Subsequently, the flask is placed under a purple LED light source (λ). max =403nm, 29.7mW*cm -2The mixture was placed on a stirrer surrounded by a ring, and the reaction temperature was controlled to approximately room temperature using circulating water cooling and an electric fan. After the specified reaction time, the reaction was stopped, the solvent was removed by rotary evaporation, and the product was then purified by column chromatography (ethyl acetate / petroleum ether = 1 / 10 (volume ratio)) to obtain a colorless oily liquid (169.4 g, 90.1%), characterized by 1H NMR and fluorine NMR. Figure 1 and 3 As shown, the synthesis of fluorinated diol monomer A was successfully confirmed. Example 2

[0039] A method for preparing a fluorinated polyester polyol includes the following steps: adipic acid (1.00 mol), methyl propylene glycol (0.65 mol), diethylene glycol (0.35 mol), and the fluorinated diol monomer A (0.20 mol) prepared in Example 1 are added to a reaction apparatus, nitrogen gas is introduced, and the mixture is reacted at 155 °C. o The reaction was stirred at C for 2 hours, and then the temperature was increased to 190°C. o C, react for 2 hours, and finally raise the temperature to 230°C. o React at C for 2 hours. Then, pre-polymerization is carried out under vacuum to -0.02 MPa for 1 hour, and the vacuum is gradually reduced to -0.09 MPa for 15 minutes. The material is then cooled and discharged to obtain fluorinated polyester polyol FPP. 1500 .like Figure 4 As shown, the molecular weight of the polyester polyol is 1500, the hydroxyl value of the polyester polyol is 130~140mgKOH / g, and the viscosity is 5000mPa·s.

[0040] A polyurethane adhesive is prepared using the aforementioned fluorinated polyester polyol, comprising separately packaged component A and separately packaged component B MDI, wherein component A is 100g of fluorinated polyester polyol FPP. 1500 The second component, consisting of 120g MDI, was mixed to prepare a fluorinated polyurethane adhesive. The adhesive was then subjected to a film-coating test, as shown in Table 1. After high-temperature cooking, the peel strength of the composite film remained above 4N, with some even reaching above 6N. This indicates that the introduction of fluorine atoms into the polyester polyol synthesized in this invention effectively improves the thermal stability of the adhesive.

[0041]

[0042] Adipic acid (1.00 mol), methyl propylene glycol (0.40 mol), and diethylene glycol (0.8 mol) were added to the reaction apparatus to synthesize fluorine-free polyester polyol PP. 1500 The molecular weight is 1500; then FPP 1500 and PP 1500The mixture was separately mixed with diphenylmethane diisocyanate (MDI) at a mass ratio of 1:1.4 to form a 15×10cm film, which was then cured at 50 °C for 72 h.

[0043] Samples with a width of 0.4 cm were prepared using a dumbbell-shaped sample preparation machine and aged in an oven at 150 ℃ for 48 h. Tensile strength tests were performed on the samples before and after baking using a universal testing machine. The test results are shown in Table 2. It can be seen that the tensile strength of FPP samples increased significantly before and after high-temperature baking. 1500 The tensile strength and elongation at break of the MDI samples did not change significantly, with a decrease of less than 5%. However, the PP samples showed no significant changes. 1500 The tensile strength of the MDI sample decreased from 30.22 MPa to 22.59 MPa, a reduction of 25.4%, and the elongation at break decreased from 338.1% to 302.5%, a reduction of 10.5%. This indicates that introducing fluorine atoms into the polyurethane backbone can give the product a higher glass transition temperature (T0). g It has good high-temperature resistance and is suitable for applications requiring high strength and heat resistance.

[0044]

[0045] Example 3 A method for preparing a fluorinated polyester polyol includes the following steps: adipic acid (1.00 mol), methyl propylene glycol (0.30 mol), diethylene glycol (0.6 mol), and monomer A (0.30 mol) obtained in Example 1 are added to a reaction apparatus, nitrogen gas is introduced, and the mixture is reacted at 150 °C. o The reaction was stirred at C for 2 hours, and then the temperature was increased to 190°C. o The reaction was carried out at C for 2.5 hours, and finally the temperature was increased to 225°C. o React at C for 2 hours. Then, pre-polymerization is carried out under vacuum to -0.02 MPa for 1 hour, and the vacuum is gradually reduced to -0.09 MPa for 15 minutes. The material is then cooled and discharged to obtain fluorinated polyester polyol FPP. 2000 ,like Figure 5 As shown, the molecular weight of the polyester polyol is 2000. The hydroxyl value of the polyester polyol was tested to be 120~130 mgKOH / g, and the viscosity was 8000 mPa·s.

[0046] A polyurethane adhesive is prepared using the aforementioned fluorinated polyester polyol, comprising separately packaged component A and separately packaged component B MDI, wherein component A is 100g of fluorinated polyester polyol FPP. 2000The second component, consisting of 120g MDI, was mixed to prepare a fluorinated polyurethane adhesive. The adhesive was then subjected to a film-coating test, as shown in Table 3. After high-temperature cooking, the peel strength of the composite film remained above 4N, indicating that the introduction of fluorine atoms into the polyester polyol synthesized in this invention effectively improves the thermal stability of the adhesive.

[0047]

[0048] Adipic acid (1.00 mol), methyl propylene glycol (0.50 mol), and diethylene glycol (0.7 mol) were added to the reaction apparatus to synthesize fluorine-free polyester polyol PP. 2000 The molecular weight is 2000. Then FPP 2000 and PP 2000 The mixture was separately mixed with diphenylmethane diisocyanate (MDI) at a mass ratio of 1:1.4 to form a 15×10cm film, which was then cured at 50 °C for 72 h.

[0049] Samples with a width of 0.4 cm were prepared using a dumbbell-shaped sample preparation machine and aged in an oven at 150 ℃ for 48 h. Tensile strength tests were performed on the samples before and after baking using a universal testing machine. The test results are shown in Table 4. It can be seen that the tensile strength of FPP samples increased significantly before and after high-temperature baking. 2000 The tensile strength and elongation at break of the MDI samples did not change significantly, with a decrease of less than 5%. However, the PP samples showed no significant changes. 2000 The tensile strength of the MDI sample decreased from 33.27 MPa to 25.51 MPa, a reduction of 23.3%, and the elongation at break decreased from 342.4% to 310.1%, a reduction of 9.43%. This indicates that introducing fluorine atoms into the polyurethane backbone can give the product a higher glass transition temperature (T0). g It has good high-temperature resistance and can be used in applications requiring high strength and heat resistance.

[0050]

[0051] The above description is merely a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

Claims

1. A method for preparing a fluorinated diol, characterized in that, Includes the following steps: S1: α,ω-diiodoperfluoroalkane, enol and catalyst are added to an organic solvent, wherein the catalyst is a halogen salt. After deoxygenation and sealing, the mixture is placed under light conditions to react and obtain a reaction solution. S2: Perform column chromatography on the reaction solution in step S1 to obtain the fluorinated diol; The structural formula of the fluorinated diol is as follows: , Where n = 1-6, m = 2-4; n and m are integers.

2. The method for preparing a fluorinated diol according to claim 1, characterized in that, The α,ω-diiodoperfluoroalkane is one or more of 1,6-diiodoperfluorohexane, 1,4-diiodoperfluorobutane, and 1,8-diiodoperfluorooctane. And / or, the enol is one or more of 3-buten-1-ol, 4-penten-1-ol, and 5-hexen-1-ol; And / or, the catalyst is a halogen salt, selected from sodium iodide, sodium chloride, and sodium bromide; And / or, the organic solvent is selected from one or more of dimethylacetamide, acetone, tetrahydrofuran, dimethyl carbonate, and acetonitrile.

3. The method for preparing a fluorinated diol according to any one of claims 1-2, characterized in that, After mixing in step S1, a deoxygenation treatment is performed, which includes introducing an inert gas; and / or, the wavelength of the light irradiation is 373-403 nm; and / or, in step S2, the column chromatography eluent is petroleum ether / ethyl acetate at a volume ratio of 20-4 / 1.

4. A fluorinated diol, characterized in that, The fluorinated diol is obtained by the preparation method according to any one of claims 1-3.

5. A method for preparing a fluorinated polyester polyol, characterized in that, Includes the following steps: Fluorinated polyester polyol is prepared by feeding dicarboxylic acid, polyol and fluorinated diol in a certain proportion and carrying out esterification and polycondensation reactions; the fluorinated diol is obtained by the preparation method according to any one of claims 1-3.

6. The preparation method according to claim 5, characterized in that: The dicarboxylic acid is one or more of glutaric acid, adipic acid, and azelaic acid; and / or the polyol is one or more of 1,4-butanediol, 2-methyl-1,3-propanediol, diethylene glycol, and glycerol.

7. The preparation method according to any one of claims 5-6, characterized in that: The esterification reaction is carried out by introducing nitrogen gas at 145-155 °C. o React under stirring for 1-2 hours, aiming for a water output of 45%-55% of the theoretical value. Continue heating to 156-190°C. o React at C for 1.5-2 hours, aiming for an output flow rate of 80%-90% of the theoretical value, then continue heating to 191-230°C. o The C reaction takes 1.5-2 hours, requiring the effluent flow rate to reach 91%-100% of the theoretical value; the polycondensation reaction is carried out under vacuum at 230-240°C. o Pre-polymerize at -0.02 MPa for about 0.5-1 hour, then gradually reduce the vacuum to -0.09 MPa, and then pump for 10-15 minutes.

8. The application of the fluorinated polyester polyol obtained by the preparation method according to any one of claims 5-7, characterized in that: The fluorinated polyester polyol is used to prepare polyurethane adhesives.

9. A polyurethane adhesive, characterized in that: It includes component A and component B, wherein component A comprises a fluorinated polyester polyol and component B comprises a polyisocyanate, and the mass ratio of component A to component B is 1:1 to 1.4; the fluorinated polyester polyol is a fluorinated polyester polyol obtained by the preparation method according to any one of claims 5-7.

10. A method for preparing a polyurethane adhesive according to claim 9, characterized in that: Component A and component B are mixed in a mass ratio of 1:1 to 1.4 to prepare a polyurethane adhesive.