A method for synthesizing 2,5-furandicarboxylic acid from fructose via tandem conversion.

By using lignin/metal oxide-based ruthenium nanoparticle catalysts, and directly using an aqueous system containing humin impurities as raw material, the process of converting fructose to 2,5-furandicarboxylic acid was simplified, solving the problems of cumbersome separation and purification steps and catalyst poisoning, and achieving efficient FDCA production.

CN123106594APending Publication Date: 2026-11-17TIANJIN UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202611395891.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for the conversion of fructose to 2,5-furandicarboxylic acid involve cumbersome separation and purification steps and the problem of impurities poisoning the catalyst, resulting in high production costs and low yields. Traditional ruthenium-based catalysts also have limited catalytic performance.

Method used

Using lignin/metal oxide-based ruthenium nanoparticle catalysts, and directly using an aqueous system containing humin impurities as raw material, the directional conversion of 5-hydroxymethylfurfural to 2,5-furandicarboxylic acid is achieved through pyrolysis of the supported ruthenium nanoparticles, simplifying the process steps and improving catalytic activity.

Benefits of technology

A highly efficient process for converting fructose to 2,5-furandicarboxylic acid was achieved, simplifying the production process, improving the conversion rate and yield of FDCA, significantly enhancing industrial production efficiency, and demonstrating excellent selective catalytic performance of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106594A_ABST
    Figure CN123106594A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of biomass chemical technology, and specifically relates to a method for synthesizing 2,5-furandicarboxylic acid (FDCA) from fructose through a series of conversions. This invention connects two stages in series: fructose dehydration to prepare HMF and HMF oxidation to prepare FDCA. Utilizing a provided lignin / metal oxide-based ruthenium particle catalyst, a highly efficient series conversion from fructose to FDCA is achieved. Furthermore, the crude HMF product generated in the first stage (containing 17% humin impurities) is used directly in the subsequent oxidation reaction without purification. Both HMF conversion and FDCA yield reach high levels, with the FDCA yield reaching up to 99%. This invention overcomes many difficulties in traditional FDCA preparation processes, such as cumbersome purification operations and difficult solvent recovery, providing a green and feasible solution for the economical preparation of biomass-based FDCA.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of biomass chemical technology, and specifically relates to a method for synthesizing 2,5-furandicarboxylic acid by tandem conversion of fructose as a raw material. It also relates to the catalyst required for the tandem conversion process and its preparation method. Background Technology

[0002] 2,5-Furfurandicarboxylic acid (FDCA) is an important bio-based platform compound. Its structure is highly similar to that of petroleum-based terephthalic acid, and it is widely considered a key monomer for the synthesis of bio-based polyesters, polyamides, and pharmaceutical intermediates, showing significant development potential in the field of green chemistry. 5-Hydroxymethylfurfural (HMF), as a direct precursor of FDCA, can be prepared from hexoses such as fructose through dehydration. Therefore, the route of converting fructose into FDCA via HMF intermediates has become a major research hotspot in the field of high-value utilization of biomass.

[0003] The preparation of FDCA from fructose as the starting material mainly involves two core reaction stages: the first stage is the acid-catalyzed dehydration of fructose to generate HMF, and the second stage is the further oxidation of HMF to obtain the target product FDCA. However, this process faces significant technical and economic challenges: if the HMF-containing dehydrated product generated in the first stage is separated and purified, it involves complex operations such as extraction and distillation, resulting in a cumbersome process and a significant increase in overall energy consumption and product preparation costs; if the separation and purification steps are omitted and the crude HMF is directly used for oxidation, byproducts such as humin generated during the dehydration process will remain in the system. These impurities can poison the catalyst or interfere with the reaction pathway, leading to a significant decrease in the yield of FDCA. Therefore, how to effectively suppress the adverse effects of impurities such as humin on subsequent oxidation while avoiding cumbersome separation and purification is the key bottleneck to achieving efficient fructose conversion to FDCA.

[0004] Furthermore, catalysts, as key components in the oxidation of HMF to FDCA, have become an important entry point for solving the aforementioned technical challenges. Currently, catalytic systems for preparing FDCA from fructose are mainly divided into two categories: homogeneous catalysts and heterogeneous catalysts. Homogeneous catalysts (patents CN119264084A, CN111194311A, CN113004232A, etc.) are mostly soluble metal salts and inorganic acids and bases. Although they have high reactivity, they are difficult to recover and suffer from problems such as difficult product separation, the generation of large amounts of saline wastewater, and severe environmental pollution, making large-scale application difficult. Heterogeneous catalytic systems, with their advantages of easy catalyst separation and recyclability, have become the mainstream research direction. Among them, ruthenium-based catalysts, due to their excellent bifunctional activation ability, can simultaneously oxidize the hydroxymethyl and aldehyde groups of HMF, achieving the directional conversion of HMF to FDCA under alkaline or weakly alkaline conditions, making them catalytic materials with high application prospects.

[0005] However, numerous studies have shown that the catalytic performance of ruthenium-based catalysts is highly dependent on the support material. This is because the support not only disperses the noble metal nanoparticles in the actual catalytic process but also modulates the electronic state of the catalytic center through ruthenium site-support interactions, synergistically participating in the oxidation process. Currently, supports used for supporting ruthenium catalytic sites mainly include metal oxides / hydroxides, activated carbon, and carbon nanotubes. Among these, single metal hydroxides such as nickel-manganese hydroxide (CN121781189A) and metal oxides such as MnO are particularly valuable. x (Pal Priyanka, Saravanamurugan Shunmugavel. Enhanced Basicity of MnO x Supported Ru for the Selective Oxidation of HMF to FDCA.[J]. ChemSusChem, 2022, 15(17)), etc., can generate strong metal-support interactions with Ru and enhance oxidation activity. However, the specific surface area of ​​pure metal oxides is limited, and noble metal particles are prone to agglomeration, resulting in severe leaching of metal ions during the reaction process. Carbon supports such as activated carbon and carbon nanotubes have high specific surface areas and can disperse Ru particles. However, the metal-support interaction of carbon supports is relatively weak, and noble metals are easily lost during the reaction process, limiting the cycle life.

[0006] Therefore, developing an integrated method for the efficient preparation of FDCA using fructose as a raw material through tandem conversion, avoiding the complex separation and purification steps of 5-hydroxymethylfurfural and humin, and simultaneously solving the problem of limited catalytic conversion activity of traditional ruthenium-based catalysts, is of great significance for promoting the green and economical preparation of FDCA. Summary of the Invention

[0007] To address the above technical problems, this invention proposes a method for synthesizing 2,5-furandicarboxylic acid by tandem conversion of fructose as a raw material.

[0008] The technical solution provided by this invention is as follows:

[0009] This invention provides a method for synthesizing 2,5-furandicarboxylic acid from fructose via a series of conversions. The method can be divided into two stages. The first stage is not significantly different from the traditional method for preparing 5-hydroxymethylfurfural from fructose. Specifically, fructose is used as the initial raw material, and a dehydration reaction is carried out in an organic solvent-water mixed solvent system under acid catalysis. After the reaction, the organic solvent is removed by rotary evaporation to obtain an aqueous phase system containing 5-hydroxymethylfurfural and humin byproducts. The key improvement of this invention lies in the second stage. This invention directly uses this aqueous phase system as the raw material without any purification or impurity removal treatment. A lignin / metal oxide-based ruthenium nanoparticle catalyst is used to catalytically oxidize 5-hydroxymethylfurfural in the aqueous phase system to obtain 2,5-furandicarboxylic acid. In other words, the most significant innovation of this invention is the provision of a novel catalytic system. This catalyst is obtained by pyrolyzing lignin with soluble manganese and cobalt salts under nitrogen protection, followed by reduction of ruthenium nanoparticles. This catalyst enables the directional conversion of 5-hydroxymethylfurfural to 2,5-furandicarboxylic acid even with humin impurities.

[0010] As a preferred embodiment, the present invention provides a method for synthesizing 2,5-furandicarboxylic acid by tandem conversion of fructose as a raw material, which specifically includes the following steps:

[0011] Step 1: Using fructose as the initial raw material, fructose is added to an organic solvent-water mixture, and hydrochloric acid is added to carry out a dehydration reaction to obtain a reaction solution containing 5-hydroxymethylfurfural and humin as byproducts;

[0012] The mass-to-volume ratio of fructose to the organic solvent-water mixture is 1 g: 15~100 mL, the volume ratio of organic solvent to water in the organic solvent-water mixture is 3~5:1, the amount of hydrochloric acid added is 8~12 mmol / L, the temperature of the dehydration reaction is 100~150 ℃, and the reaction time is 4~8 h;

[0013] Step 2: Remove the organic solvent from the reaction solution obtained in Step 1 by rotary evaporation to obtain an aqueous system containing 5-hydroxymethylfurfural and humin byproducts;

[0014] Step 3: Add lignin / metal oxide-based ruthenium nanoparticle catalyst to the aqueous system containing 5-hydroxymethylfurfural and humin byproducts obtained in Step 2, introduce oxygen, and carry out catalytic oxidation reaction under pressure to oxidize 5-hydroxymethylfurfural to 2,5-furandicarboxylic acid.

[0015] The organic solvent is selected from at least one of acetone, butanone, and tetrahydrofuran; the mass ratio of the catalyst to 5-hydroxymethylfurfural in the aqueous system is 2-4:1; and the catalytic oxidation conditions are: reaction temperature 110-140 °C, oxygen pressure 2-6 bar, reaction time 3-8 h, and no alkali.

[0016] Furthermore, the present invention also provides a method for preparing the lignin / metal oxide-based ruthenium nanoparticle catalyst, specifically comprising the following steps:

[0017] (1) The lignin is thoroughly mixed with soluble manganese salt and soluble cobalt salt, and then heated to 400-500 °C under nitrogen protection at a heating rate of 2-5 °C / min to obtain the lignin / metal oxide composite carrier.

[0018] The mass ratio of lignin to soluble manganese salt and soluble cobalt salt is 1~3:5~7:0.7~0.9;

[0019] (2) The lignin / metal oxide composite support prepared in (1) is immersed in an aqueous solution containing ruthenium compound. Under the action of a reducing agent, ruthenium is reduced to nanoparticles and loaded onto the lignin / metal oxide composite support. After washing and drying, the lignin / metal oxide-based ruthenium nanoparticle catalyst is obtained.

[0020] In the above preparation method, preferably, the lignin in (1) is selected from at least one of alkali lignin, enzymatic hydrolyzed lignin, sulfate lignin, and organic solvent lignin;

[0021] Preferably, the soluble manganese salt is selected from at least one of manganese nitrate, manganese sulfate, and manganese chloride.

[0022] Preferably, the soluble cobalt salt is selected from at least one of cobalt nitrate, cobalt sulfate, and cobalt chloride.

[0023] Preferably, the ruthenium-containing compound in (2) is ruthenium trichloride, the mass ratio of ruthenium trichloride to the composite carrier is 1:15~35, the reducing agent is selected from at least one of formaldehyde, sodium borohydride, and hydrogen, and the molar ratio of ruthenium trichloride to the reducing agent is 1:2500~2800.

[0024] Preferably, the reduction temperature described in (2) is 85~95 ℃.

[0025] Furthermore, the application of the lignin / metal oxide-based ruthenium nanoparticle catalyst prepared by the above-described method of this invention in the synthesis of 2,5-furandicarboxylic acid is also a key area of ​​protection for this invention. This application can involve using fructose or pure 5-hydroxymethylfurfural as the initial raw material, employing the catalyst for catalytic oxidation to synthesize 2,5-furandicarboxylic acid. In actual industrial production, fructose is the most preferred and inexpensive raw material for the preparation of 2,5-furandicarboxylic acid. If fructose is used directly as the starting point, adding the catalyst of this invention during the catalytic oxidation stage can still achieve a high conversion rate even with impurities such as humic acid. In addition, if pure 5-hydroxymethylfurfural is used directly as the raw material to produce 2,5-furandicarboxylic acid, the catalyst of this invention can also exhibit excellent oxidation effects. Therefore, the catalytic oxidation of the above two raw materials for the preparation of 2,5-furandicarboxylic acid falls within the technical scope protected by this invention.

[0026] Preferably, when 2,5-furandicarboxylic acid is synthesized from crude product containing 5-hydroxymethylfurfural and humin byproduct obtained by dehydration of pure 5-hydroxymethylfurfural or fructose, the mass ratio of the catalyst to 5-hydroxymethylfurfural is 2~4:1; when 2,5-furandicarboxylic acid is synthesized from fructose, the mass ratio of the catalyst to fructose is 3~5:1.

[0027] The present invention has the following advantages and effects compared with the prior art:

[0028] (1) This invention connects two stages in series: the dehydration of fructose to prepare 5-hydroxymethylfurfural (HMF) and the oxidation of HMF to prepare 2,5-furandicarboxylic acid (FDCA). Although there have been reports on continuous reactions of the two stages, the most critical innovation of this invention is that, on the one hand, in the entire continuous operation process, especially after the first stage reaction, there is no need for cumbersome steps such as purification and impurity removal. Instead, the crude product mixed with aqueous phase containing humin impurities (about 17%) and HMF is used directly as raw material for subsequent oxidation reactions, which greatly simplifies the process steps and effectively reduces production costs. On the other hand, even without the previous purification and impurity removal operations, the crude product is used directly as raw material. After catalysis by the catalyst of this invention, the HMF conversion rate and FDCA yield both reach a high level, with the FDCA yield reaching up to 99%, which significantly improves the industrial production efficiency of FDCA.

[0029] (2) This invention provides a novel support system for ruthenium nanoparticle catalysts. The catalyst is prepared by loading ruthenium nanoparticles onto a lignin-manganese and cobalt metal oxide composite support. The catalyst exhibits excellent selective catalytic effect in the process of catalyzing the conversion of HMF to FDCA. Compared with the FDCA yield of lignin-monometal oxide support (67%~81%), it is increased by 18%~32%, and compared with the FDCA yield of other biomass carbon-based metal oxide support catalysts (21%~56%), it is increased by 1~4 times. Moreover, the catalytic activity is significantly better than catalysts supported by other metal oxides or noble metal nanoparticles (51%~80%). Attached Figure Description

[0030] Figure 1 The XRD pattern of the lignin / metal oxide-based ruthenium nanoparticle catalyst prepared in Example 1 of this invention;

[0031] Figure 2 The Mn2p XPS spectrum of the lignin / metal oxide-based ruthenium nanoparticle catalyst prepared in Example 1 of this invention is shown below.

[0032] Figure 3 The Co2p XPS spectrum of the lignin / metal oxide-based ruthenium nanoparticle catalyst prepared in Example 1 of this invention;

[0033] Figure 4 The image shows the Ru3p XPS spectrum of the lignin / metal oxide-based ruthenium nanoparticle catalyst prepared in Example 1 of this invention. Detailed Implementation

[0034] To enable those skilled in the art to better understand the present invention, specific embodiments will now be described in further detail. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the scope of the invention.

[0035] Example 1

[0036] This embodiment provides a lignin / metal oxide-based ruthenium nanoparticle catalyst, which is prepared using the following method:

[0037] (1) Mix enzymatically hydrolyzed lignin, manganese nitrate and cobalt nitrate in a mass ratio of 1:7:0.7, place them in a tube furnace, and heat them to 400 °C at a heating rate of 2 °C / min under the protection of nitrogen atmosphere. Hold the temperature for 2 h and cool naturally to room temperature to obtain lignin / metal oxide composite carrier.

[0038] (2) Take 0.5 g of the lignin / metal oxide composite carrier obtained in (1), add it to 25 mL of deionized water, add 0.05 mmol of ruthenium trichloride, heat to 90 °C, slowly add 10 mL of 37% formaldehyde solution, stir the reaction for 3 h, after the reaction is completed, wash with deionized water 3 times, dry in a vacuum oven at 60 °C for 12 h to obtain the lignin / metal oxide-based ruthenium nanoparticle catalyst (named Ru / LM).

[0039] Figure 1 The image shows the X-ray diffraction (XRD) pattern of the lignin / metal oxide-based ruthenium nanoparticle catalyst prepared in this embodiment. The XRD pattern shows that the prepared catalyst bulk exhibits typical Mn3O4 diffraction characteristics, indicating that the bulk phase of the catalyst is dominated by the Mn3O4 crystalline phase. No independent diffraction peaks belonging to Co or Ru species were observed, indicating that these two elements exist in the Mn3O4 substrate in a highly dispersed amorphous, nanocluster, or lattice-doped form.

[0040] Figure 2 , Figure 3 , Figure 4 The images show the Mn 2p, Co 2p, and Ru 3p XPS spectra of the lignin / metal oxide-based ruthenium nanoparticle catalyst, respectively. The XPS spectra further reveal the chemical states of the elements on the catalyst surface. Figure 2 and 3 The high-resolution spectral fitting results of Mn 2p and Co 2p show that both Mn and Co exist in oxidized form. Mn is mainly in a mixed state of +2 and +3 valence, while Co is mainly in the +2 valence oxidized state. In addition, the Ru 3p spectrum shows that Ru is in a mixed valence state of zero valence and oxidized state on the catalyst surface.

[0041] The above characterization results show that the present invention has successfully prepared a ruthenium nanoparticle catalyst supported on a lignin / manganese oxide / cobalt oxide composite support.

[0042] Comparative Example 1

[0043] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that, in the preparation of this comparative example, only manganese nitrate was added instead of cobalt nitrate in (1), and the mass ratio of enzymatically hydrolyzed lignin to manganese nitrate was 1:7.7.

[0044] Comparative Example 2

[0045] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that, in the preparation of this comparative example, only cobalt nitrate was added instead of manganese nitrate in (1), and the mass ratio of enzymatically hydrolyzed lignin to cobalt nitrate was 1:7.7.

[0046] Comparative Example 3

[0047] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that, in the preparation of the catalyst in this comparative example, the mass ratio of enzymatic hydrolysis of lignin: manganese nitrate: cobalt nitrate in (1) is 1.5:7:0.7.

[0048] Comparative Example 4

[0049] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that, in the preparation of the catalyst in this comparative example, the mass ratio of enzymatic hydrolysis of lignin: manganese nitrate: cobalt nitrate in (1) is 0.5:7:0.7.

[0050] Comparative Example 5

[0051] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that, in the preparation of the catalyst in this comparative example, the mass ratio of enzymatic hydrolysis of lignin: manganese nitrate: cobalt nitrate in (1) is 1:10.5:0.7.

[0052] Comparative Example 6

[0053] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that, in the preparation of this comparative example, the mass ratio of enzymatic hydrolysis of lignin: manganese nitrate: cobalt nitrate in (1) is 1:3.5:0.7.

[0054] Comparative Example 7

[0055] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that, in the preparation of this comparative example, the mass ratio of enzymatic hydrolysis of lignin: manganese nitrate: cobalt nitrate in (1) is 1:7:1.05.

[0056] Comparative Example 8

[0057] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that, in the preparation of this comparative example, the mass ratio of enzymatic hydrolysis of lignin: manganese nitrate: cobalt nitrate in (1) is 1:7:0.35.

[0058] Comparative Example 9

[0059] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that in the preparation of this comparative example, glucose is used instead of enzymatic hydrolysis of lignin in (1).

[0060] Comparative Example 10

[0061] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that in the preparation of this comparative example, alginate is used instead of enzymatic hydrolysis of lignin in (1).

[0062] Comparative Example 11

[0063] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that, in the preparation of the catalyst in this comparative example, vitamin C is used instead of enzymatic hydrolysis of lignin in (1).

[0064] Comparative Example 12

[0065] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that, in the preparation of the catalyst in this comparative example, ferric nitrate is used instead of cobalt nitrate in (1), that is, the mass ratio of enzymatically hydrolyzed lignin: manganese nitrate: ferric nitrate is 1:7:0.7.

[0066] Comparative Example 13

[0067] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that, in the preparation of the catalyst in this comparative example, nickel nitrate is used instead of cobalt nitrate in (1), that is, the mass ratio of enzymatic hydrolysis of lignin: manganese nitrate: nickel nitrate is 1:7:0.7.

[0068] Comparative Example 14

[0069] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that the catalyst in this comparative example was prepared at a pyrolysis temperature of 300 °C in (1).

[0070] Comparative Example 15

[0071] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that the catalyst in this comparative example was prepared at a pyrolysis temperature of 600 °C in (1).

[0072] Comparative Example 16

[0073] This comparative example provides a lignin / metal oxide-based palladium nanoparticle catalyst. The only difference from Example 1 is that, in the preparation of this comparative example, (2) chloropalladium acid is used instead of ruthenium trichloride.

[0074] Comparative Example 17

[0075] This comparative example provides a lignin / metal oxide-based platinum nanoparticle catalyst. The only difference from Example 1 is that, in the preparation of this comparative example, (2) chloroplatinic acid is used instead of ruthenium trichloride.

[0076] Comparative Example 18

[0077] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that, in the preparation of this comparative example, the amount of ruthenium trichloride added in (2) is 0.075 mmol.

[0078] Comparative Example 19

[0079] This comparative example provides a lignin / metal oxide-based ruthenium nanoparticle catalyst. The only difference from Example 1 is that, in the preparation of this comparative example, the amount of ruthenium trichloride added in (2) is 0.025 mmol.

[0080] Comparative Example 20

[0081] This comparative example provides a lignin / metal oxide catalyst. The only difference from Example 1 is that in this comparative example, only the lignin / metal oxide composite support is prepared as a catalyst according to the method described in (1) of Example 1, and ruthenium nanoparticles are not loaded.

[0082] Comparative Example 21

[0083] The optimal Co-N3 / RuSCCs catalyst was prepared according to the method described in patent CN121360606A and the journal article “Spacing-matching enabled spatiallypaired Co-SA / Ru-NC catalysts for room temperature tandem oxidation of HMF at industrial-level concentration (Appl. Catal. B: Environ. (2026) 399 : 127159)”.

[0084] Comparative Example 22

[0085] In this comparative example, the Pt / Mn with the best performance was prepared according to the method described in patent CN116003355A and the journal article “Unlocking the Production of Biomass-Derived Plastic Monomer 2,5-Furandicarboxylic Acid at Industrial-Level Concentration (ACS Catal. (2024) 14 (23): 17510–17524)”. 10 Co1O x -VC catalyst.

[0086] Application Example 1

[0087] The catalysts prepared in the above embodiments and comparative examples were applied to the synthesis of 2,5-furandicarboxylic acid. Specifically, this application example provides a method for preparing 2,5-furandicarboxylic acid by tandem conversion of fructose as a raw material, the steps of which are as follows:

[0088] Step 1: Using fructose as the initial raw material, fructose, acetone-water mixed solvent, and hydrochloric acid were added to the reactor and the fructose dehydration reaction was carried out at 120℃ for 6 h to obtain a reaction solution containing 5-hydroxymethylfurfural. The yield of 5-hydroxymethylfurfural was 83%.

[0089] The mass-volume ratio of fructose to the mixed solvent is 1 g:~100 mL, the volume ratio of acetone to water in the acetone-water mixed solvent is 4:1, and the amount of hydrochloric acid added is 10 mmol / L.

[0090] Step 2: Remove the acetone from the reaction solution obtained in Step 1 by rotary evaporation to obtain an aqueous system containing 5-hydroxymethylfurfural, which contains 83% 5-hydroxymethylfurfural and 17% humin impurities.

[0091] Step 3: Add the catalysts prepared in each example and comparative example to the aqueous system containing 5-hydroxymethylfurfural obtained in Step 2. The mass ratio of catalyst to 5-hydroxymethylfurfural in the aqueous system is 4:1. Introduce 3 bar of oxygen into the phase reaction system and carry out the catalytic oxidation reaction at 130 °C for 6 h (without alkali) to oxidize 5-hydroxymethylfurfural to 2,5-furandicarboxylic acid.

[0092] The content of 2,5-furandicarboxylic acid in the products obtained by different catalysts was determined by high performance liquid chromatography. The results showed that the conversion rate of 5-hydroxymethylfurfural was >99%, and the specific yields of 2,5-furandicarboxylic acid are shown in Table 1 below.

[0093] The yield of 2,5-furandicarboxylic acid in this invention was calculated according to the following method:

[0094] FDCA yield (%) = n FDCA / n HMF ×100%, n FDCA n is the amount of FDCA actually produced in the reaction. HMF It is the amount of HMF in the solution to be tested before the oxidation reaction begins.

[0095] Table 1. Yields of fructose to 2,5-furandicarboxylic acid catalyzed by different catalysts Group number FDCA yield (%) Group number FDCA yield (%) Example 1 99 Comparative Example 11 56 Comparative Example 1 67 Comparative Example 14 32 Comparative Example 2 81 Comparative Example 15 61 Comparative Example 3 44 Comparative Example 16 51 Comparative Example 4 61 Comparative Example 17 80 Comparative Example 5 83 Comparative Example 18 68 Comparative Example 6 68 Comparative Example 19 36 Comparative Example 7 71 Comparative Example 20 19 Comparative Example 8 69 Comparative Example 21 16 Comparative Example 9 21 Comparative Example 22 56 Comparative Example 10 37

[0096] As shown in Table 1, the ruthenium catalyst supported on a lignin / metal oxide-based ternary composite support prepared by lignin, manganese nitrate and cobalt nitrate in Example 1 of the present invention exhibits the best catalytic performance in the reaction of fructose tandem conversion to FDCA, with the highest FDCA yield reaching 99%.

[0097] Compared to the embodiments, the catalysts prepared in Comparative Examples 1-22 showed significantly reduced effectiveness in the catalytic oxidation of HMF to FDCA. Specifically, in Comparative Examples 1-2, the catalyst support was prepared by adding only one of the metal salts, manganese nitrate or cobalt nitrate, to create a lignin-to-a single metal oxide composite catalyst support. Even after loading ruthenium nanoparticles, the catalytic performance of the catalyst was significantly lower than when both metals were used together, with FDCA yields of 67% and 81%, respectively. This indicates a significant synergistic effect between Mn and Co metal oxides as supports, which is beneficial for improving the conversion efficiency of FDCA.

[0098] In Comparative Examples 3-8 of this invention, the proportions of each component in the support during catalyst preparation were adjusted. Experimental data showed that the amount of lignin added had the most significant impact on the catalytic effect of FDCA synthesis. Specifically, in Comparative Examples 3-4, when the amount of lignin added was high, the FDCA yield was only 44%, and when the amount of lignin added was too low, the FDCA yield was only 61%. This phenomenon may be due to the following: excessive lignin leads to excessive carbon layer encapsulation of Mn-Co oxides, weakening the electronic interaction between Ru and the support, and simultaneously causing pore blockage, hindering mass transfer from HMF and intermediates to the active sites. Insufficient lignin addition, on the other hand, makes Ru nanoparticles prone to aggregation; Mn-Co oxides lose their carbon skeleton dispersion, resulting in low specific surface area, easy sintering, and insufficient exposure of active sites. Furthermore, comparative examples 5-8 show that the content of the two metal oxide supports also directly affects the catalytic effect. Mn and Co generate a significant bimetallic synergistic effect in the oxidation of HMF to FDCA through redox cycles. Deviating from the optimal metal ratio will lead to a decrease in electron transfer efficiency, which will reduce the reaction efficiency of the rate-limiting step in the oxidation process, and consequently reduce the selectivity of FDCA.

[0099] In Comparative Examples 9-11 of this invention, commonly used biomass molecules such as glucose, alginic acid, and vitamin C were used instead of lignin as carbon-based precursors. However, the experimental results showed that although the prepared catalysts could achieve FDCA conversion to a certain extent, the catalytic effect was very poor, with FDCA yields ranging from only 21% to 56%. It is speculated that the reason for this result may be the uniqueness of lignin. Unlike natural small-molecule carbon-based components such as glucose, alginic acid, and vitamin C, lignin is an amorphous aromatic polymer compound associated with cellulose and hemicellulose in plant lignified tissues. It is rich in various types of active groups such as aromatic groups, phenolic hydroxyl groups, alcoholic hydroxyl groups, and carbon-based conjugated double bonds. After pyrolysis and composite metal oxides, it is more conducive to the loading of ruthenium nanoparticles, providing more loading active sites for metal oxides and ruthenium nanoparticles. Therefore, the catalytic effect of the catalyst prepared with lignin as a carbon-based support is significantly better than that of traditional small-molecule bio-carbon sources.

[0100] In Comparative Examples 12-13 and 16-17 of the present invention, Fe and Ni oxides were used instead of cobalt oxides and combined with manganese oxides as metal oxide support components. The results showed that neither manganese iron oxide nor manganese nickel oxide could achieve the synergistic catalytic effect of manganese cobalt oxide catalyst. Similarly, Pd and Pt could not replace the efficient catalytic function of Ru in this reaction.

[0101] Furthermore, in Comparative Examples 14-15 of the present invention, the catalyst support was pyrolyzed at different temperatures. The results show that the pyrolysis temperature has a decisive influence on the catalyst performance. When pyrolyzed at 300 °C, the catalytic yield of FDCA was only 32%, possibly due to insufficient carbonization of lignin and incomplete crystal structure of the metal oxide. At 600 °C, excessive graphitization and sintering and agglomeration of metal particles also significantly reduced the catalyst activity, resulting in an FDCA yield of 61%. In Comparative Example 20, without ruthenium metal nanoparticles, the catalyst support was used directly as the catalyst, and the FDCA yield was only 19%. This indicates that the catalyst support itself has almost no activity in catalyzing the oxidation of HMF to FDCA, further confirming that the ruthenium nanoparticles in the catalyst provided by the present invention are an indispensable key active component in this tandem conversion reaction.

[0102] Furthermore, the inventors prepared catalyst products of Comparative Example 21 and Comparative Example 22 according to existing technology. The catalyst obtained in Comparative Example 21 achieved a maximum HMF conversion rate of 94% in the catalytic reaction, but the FDCA yield was only 16%, and it exacerbated the condensation of humin. This indicates that the existing cobalt-ruthenium dual-site catalyst, in the crude HMF system containing humin impurities in this invention, not only has severely insufficient oxidation activity but also promotes the condensation of byproducts, failing to meet the requirements of alkali-free oxidation catalysis in the tandem process. The catalyst in Comparative Example 22 achieved a 99% HMF conversion rate and a 56% FDCA yield, proving that the catalyst does indeed have certain activity under alkali-free conditions, but the FDCA yield is far lower than that of this invention, also making it difficult to achieve efficient tandem conversion of fructose to FDCA.

[0103] The above are merely preferred embodiments of the present invention and do not limit the scope of the patent. All equivalent changes and modifications made within the scope of the present invention should still fall within the scope of the present invention.

Claims

1. A method for synthesizing 2,5-furandicarboxylic acid from fructose via a series of conversions, comprising using fructose as the initial raw material, carrying out a dehydration reaction in an organic solvent-water mixed solvent system, and after the reaction, removing the organic solvent by rotary evaporation to obtain an aqueous phase system containing 5-hydroxymethylfurfural and humin as byproducts, characterized in that... Using the aqueous system as raw material, 2,5-furandicarboxylic acid was prepared by catalytic oxidation reaction using lignin / metal oxide-based ruthenium nanoparticle catalyst; The organic solvent is selected from at least one of acetone, butanone, and tetrahydrofuran; The lignin / metal oxide-based ruthenium nanoparticle catalyst is obtained by mixing lignin with soluble manganese salt and soluble cobalt salt, pyrolyzing the mixture under nitrogen protection, and then reducing the ruthenium nanoparticles loaded on it.

2. The method as described in claim 1, characterized in that, The mass-to-volume ratio of fructose to the organic solvent-water mixture is 1 g: 15~100 mL, and the volume ratio of organic solvent to water in the organic solvent-water mixture is 3~5:

1. The dehydration reaction is carried out under hydrochloric acid catalysis, and the amount of hydrochloric acid added is 8~12 mmol / L. The temperature of the dehydration reaction is 100~150 ℃, and the reaction time is 4~8 h.

3. The method as described in claim 1, characterized in that, The mass ratio of the catalyst to 5-hydroxymethylfurfural in the aqueous system containing 5-hydroxymethylfurfural and humin byproducts is 2-4:

1. The catalytic oxidation conditions are: reaction temperature 110-140 °C, oxygen pressure 2-6 bar, reaction time 3-8 h, and no alkali.

4. A method for preparing a lignin / metal oxide-based ruthenium nanoparticle catalyst, characterized in that, The steps include the following: (1) The lignin is thoroughly mixed with soluble manganese salt and soluble cobalt salt, and then heated to 400-500 °C under nitrogen protection at a heating rate of 2-5 °C / min to obtain the lignin / metal oxide composite carrier. The mass ratio of lignin to soluble manganese salt and soluble cobalt salt is 1~3:5~7:0.7~0.9; (2) The lignin / metal oxide composite support prepared in (1) is immersed in an aqueous solution containing ruthenium compound. Under the action of a reducing agent, ruthenium is reduced to nanoparticles and loaded onto the lignin / metal oxide composite support. After washing and drying, the lignin / metal oxide-based ruthenium nanoparticle catalyst is obtained.

5. The preparation method according to claim 4, characterized in that, (1) The lignin mentioned is selected from at least one of alkali lignin, enzymatic hydrolyzed lignin, sulfate lignin, and organic solvent lignin; The soluble manganese salt is selected from at least one of manganese nitrate, manganese sulfate, and manganese chloride; The soluble cobalt salt is selected from at least one of cobalt nitrate, cobalt sulfate, and cobalt chloride.

6. The preparation method according to claim 4, characterized in that, (2) The ruthenium-containing compound is ruthenium trichloride, the mass ratio of ruthenium trichloride to the composite carrier is 1:15~35, the reducing agent is selected from at least one of formaldehyde, sodium borohydride and hydrogen, and the molar ratio of ruthenium trichloride to the reducing agent is 1:2500~2800.

7. The preparation method according to claim 4, characterized in that, The reduction temperature described in (2) is 85~95 ℃.

8. The application of the lignin / metal oxide-based ruthenium nanoparticle catalyst prepared by the method according to any one of claims 4 to 7 in the synthesis of 2,5-furandicarboxylic acid, characterized in that, The application uses pure fructose or 5-hydroxymethylfurfural as the initial raw material and the catalyst to carry out a catalytic oxidation reaction to synthesize 2,5-furandicarboxylic acid.

9. The application as described in claim 8, characterized in that, When 2,5-furandicarboxylic acid is synthesized using pure 5-hydroxymethylfurfural as the initial raw material, the mass ratio of the catalyst to 5-hydroxymethylfurfural is 2~4:

1.

10. The application as described in claim 8, characterized in that, When 2,5-furandicarboxylic acid is synthesized from fructose as the initial raw material, the mass ratio of the catalyst to fructose is 3~5:1.

Citation Information

Patent Citations

  • Process for preparing 2,5-furandicarboxylic acid

    CN111194311A

  • One-pot two-step method for preparing FDCA from carbohydrate compound

    CN113004232A

  • Method for preparing 2, 5-furandicarboxylic acid from fructose

    CN119264084A

  • Preparation method of cobalt-ruthenium double-site catalyst and application of cobalt-ruthenium double-site catalyst in synthesis of 2, 5-furandicarboxylic acid

    CN121360606A

  • Precious metal ruthenium monatomic supported catalyst as well as preparation method and application thereof

    CN121781189A