A preparation process for tricalcium phosphate for suspension polymerization and modified tricalcium phosphate

By modifying tricalcium phosphate microparticles and coupling them with amphiphilic polymers, the problem of unsatisfactory dispersion in suspension polymerization was solved, and the preparation of polymer microspheres with uniform particle size was achieved, thus improving the dispersion effect of suspension polymerization.

CN123106951APending Publication Date: 2026-11-17JIANGYIN XINGYU CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610973227.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-01
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the prior art, dispersants prepared using tricalcium phosphate as a matrix do not have ideal dispersion effects in suspension polymerization, making it difficult to obtain polymer microspheres with uniform particle size.

Method used

Tricalcium phosphate microparticles were modified using a carboxysilane coupling agent and then coupled with an amphiphilic polymer to prepare modified tricalcium phosphate microparticles as a dispersant. The microparticles were then activated in a buffer solution at a specific pH value and EDC and NHS were added. The mixture was then further mixed with the amphiphilic polymer to form a stable dispersion system.

Benefits of technology

High molecular microspheres with good transparency, good particle sphericity, and uniform particle size were prepared, which improved the dispersion effect of suspension polymerization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a process for preparing tricalcium phosphate for suspension polymerization, comprising the following steps: S10: modifying tricalcium phosphate microparticles with a carboxysilane coupling agent; S20: dispersing the carboxylated tricalcium phosphate microparticles in a buffer solution with a pH of 5.5-6.5, and adding EDC and NHS to the buffer solution; the ratio of the total mass of EDC and NHS to the mass of the carboxylated porous tricalcium phosphate microparticles is (1-10):100, and the molar ratio of EDC to NHS is 1:(0.9-1.2); S30: dispersing the first and second amphiphilic polymers in a dispersant, and then adding the activated dispersion obtained in S20 dropwise; both the first and second amphiphilic polymers are composed of sequentially connected hydrophobic segments, hydrophilic segments, and terminal amino groups, and the length of the hydrophilic segment of the first amphiphilic polymer is greater than the length of the hydrophilic segment of the second amphiphilic polymer. The suspension dispersion system using tricalcium phosphate as a dispersant of this invention is easy to prepare polymer microspheres with good transparency, good particle sphericity, and uniform particle size. This invention also discloses a modified tricalcium phosphate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymerization reaction technology, specifically to a preparation process of tricalcium phosphate for suspension polymerization and a modified tricalcium phosphate. Background Technology

[0002] Suspension polymerization is a method of free radical polymerization in which monomer droplets are suspended in water. The suspension polymerization system mainly consists of monomers, oil-soluble initiators, dispersants and water. The dispersants are divided into water-soluble polymers (such as polyvinyl alcohol and gelatin) and non-water-soluble inorganic powders (such as calcium carbonate and talc).

[0003] The main functions of dispersants are: 1. To reduce surface tension and help monomers disperse into droplets; 2. To protect and prevent particle aggregation. When the polymerization conversion rate reaches 20%~30%, the monomers become polymer / monomer solution particles (which tend to aggregate). Dispersants adsorb onto the particle surface, thus preventing aggregation.

[0004] Some researchers have modified tricalcium phosphate to prepare high-performance dispersants; however, the dispersion effect of dispersants prepared with tricalcium phosphate as the matrix is ​​still not ideal. Summary of the Invention

[0005] One of the objectives of this invention is to overcome the deficiencies in the prior art and provide a process for preparing tricalcium phosphate for suspension polymerization. The tricalcium phosphate microparticles obtained by this process are used as a dispersant for suspension polymerization, which is beneficial for obtaining polymer microspheres with uniform particle size.

[0006] To achieve the above-mentioned technical effects, the technical solution of the present invention is as follows: a preparation process of tricalcium phosphate for suspension polymerization, comprising the following steps: S10: Tricalcium phosphate microparticles are modified with a carboxylsilane coupling agent to obtain carboxylated tricalcium phosphate microparticles; S20: Disperse carboxylated tricalcium phosphate microparticles in a buffer solution with a pH of 5.5-6.5, add EDC and NHS to the buffer solution to obtain an activated carboxylated tricalcium phosphate microparticle dispersion; The ratio of the total mass of EDC and NHS to the mass of the carboxylated porous tricalcium phosphate microparticles is (1~10):100, and the molar ratio of EDC to NHS is 1:(0.9~1.2). S30: After dispersing the first and second amphiphilic polymers in a polymer dispersant, the activated carboxylated tricalcium phosphate microparticle dispersion obtained in S20 is added dropwise. Both the first and second amphiphilic polymers are composed of sequentially connected hydrophobic segments, hydrophilic segments, and terminal amino groups. The length of the hydrophilic segment of the first amphiphilic polymer is greater than the length of the hydrophilic segment of the second amphiphilic polymer.

[0007] Furthermore, the pH value of the buffer solution can be selected from points 5.5, 5.6, 5.7, 5.8, 5.9, 6, 6.1, 6.2, 6.3, 6.4, and 6.5, or a range of two of the above points as the maximum and minimum values. The ratio of the total mass of EDC and NHS to the mass of the carboxylated porous tricalcium phosphate microparticles can be selected from points 1:100, 2:100, 3:100, 4:100, 5:100, 6:100, 7:100, 8:100, 9:100, and 10:100, or a range of two of the above points as the maximum and minimum values. The molar ratio of EDC to NHS can be selected from points 1:0.9, 1:1, 1:1.1, and 1:1.2, or a range of two of the above points as the maximum and minimum values.

[0008] In a preferred embodiment, the hydrophobic segment is selected from at least one of polylactic acid segments, polytrimethylene carbonate segments, and polycaprolactone segments, and the hydrophilic segment is selected from at least one of polyethylene glycol segments and polyacrylic acid segments.

[0009] In a preferred embodiment, the hydrophobic segments of the first and second amphiphilic polymers are both polycaprolactone segments, and the hydrophilic segments of the first and second amphiphilic polymers are both polyethylene glycol segments.

[0010] A preferred embodiment is that the molecular weight of the polycaprolactone segment of the first amphiphilic polymer is 7~11kDa, and the molecular weight of the polycaprolactone segment of the second amphiphilic polymer is 12~15kDa.

[0011] Furthermore, the molecular weight of the polycaprolactone segment of the first amphiphilic polymer can be selected as 7k, 8k, 9k, 10k, 11kDa or a range of the above two values ​​as the maximum and minimum values, and the molecular weight of the polycaprolactone segment of the second amphiphilic polymer can be selected as 12k, 13k, 14k, 15kDa or a range of the above two values ​​as the maximum and minimum values.

[0012] A preferred embodiment is that the molecular weight of the polyethylene glycol segment of the first amphiphilic polymer is 4-5 kDa, and the molecular weight of the polyethylene glycol segment of the second amphiphilic polymer is 3-4.8 kDa.

[0013] Furthermore, the molecular weight of the polyethylene glycol segment of the first amphiphilic polymer can be selected as 4k, 5kDa, or a range of the two values ​​as the maximum and minimum values, and the molecular weight of the polyethylene glycol segment of the second amphiphilic polymer can be selected as 3k, 3.6k, 4.2k, 4.8kDa, or a range of the two values ​​as the maximum and minimum values.

[0014] In a preferred embodiment, in S10, the mass ratio of the carboxylated tricalcium phosphate microparticles to the carboxysilane coupling agent is 100:(0.5~2).

[0015] Furthermore, the mass ratio of the carboxylated tricalcium phosphate microparticles to the carboxysilane coupling agent can be selected as a point value of 100:0.5, 100:1, 100:1.5, or 100:2, or as an interval value between the two points mentioned above, representing the maximum and minimum values.

[0016] In a preferred embodiment, the mass ratio of the carboxylated tricalcium phosphate microparticles to the first amphiphilic polymer in S30 is 100:(0.1~0.2).

[0017] Furthermore, the mass ratio of the carboxylated tricalcium phosphate microparticles and the first amphiphilic polymer in S30 can be selected as a point value of 100:0.1, 100:0.14, 100:0.18, or 100:0.2, or as an interval value of the above two point values ​​as the maximum and minimum values.

[0018] The preferred embodiment is that the mass ratio of the first amphiphilic polymer and the second amphiphilic polymer in S30 is 1:(2~3).

[0019] Furthermore, the mass ratio of the first amphiphilic polymer and the second amphiphilic polymer in S30 can be selected as a point value of 1:2, 1:2.2, 1:2.4, 1:2.6, 1:2.8, or 1:3, or two of the above point values ​​as an interval between the maximum and minimum values.

[0020] A preferred embodiment is that the carboxysilane coupling agent is at least one selected from triethoxysilylpropylmaleamic acid and carboxylated polyethylene glycol silane.

[0021] The second objective of this invention is to provide a modified tricalcium phosphate, which is prepared by the above-mentioned process for preparing tricalcium phosphate for suspension polymerization.

[0022] The advantages and beneficial effects of this invention are as follows: Modified tricalcium phosphate microparticles are obtained by coupling tricalcium phosphate microparticles with a first amphiphilic polymer and a second amphiphilic polymer. The suspension dispersion system using these microparticles as a dispersant can easily prepare polymer microspheres with good transparency, good particle sphericity, and uniform particle size. Detailed Implementation

[0023] The specific embodiments of the present invention will be further described below with reference to examples. These examples are only used to more clearly illustrate the technical solutions of the present invention and should not be construed as limiting the scope of protection of the present invention.

[0024] Examples and Comparative Examples 1. Examples 1, 2, and 3 concerning whether porous tricalcium phosphate microparticles are only modified with carboxyl groups, whether the carboxyl-modified porous tricalcium phosphate microparticles are coupled with amphiphilic polymers, and whether the lengths of the hydrophilic segments of the amphiphilic polymers are equal. Example 1

[0025] Preparation of porous tricalcium phosphate microparticles in Example 1: Add 200 mL of calcium carbonate aqueous suspension with a solid content of 90 g / L to the reaction vessel, stir thoroughly, heat to 50 °C, and slowly add 1 mol / L phosphoric acid aqueous solution to carry out the reaction. Control the amount of phosphoric acid aqueous solution added so that the Ca:P atomic ratio in the reaction solution is 1.7. After the addition is completed, age at 50 °C for 3 h, cool to room temperature, filter, and dry to obtain porous tricalcium phosphate microparticles.

[0026] Carboxyl modification of porous tricalcium phosphate microparticles in Example 1: S01: Mix 900 parts of deionized water, 100 parts of anhydrous ethanol, and 15 parts of silane coupling agent (Changfu Chemical Company's carboxysilane coupling agent model LNA33), then add glacial acetic acid dropwise until the pH of the mixture reaches 4.5. Stir the mixture at room temperature for 30 minutes. S02: Add 100 parts of porous tricalcium phosphate microparticles to the mixture obtained from 1000 parts of S01, and heat the system to 60℃ and stir for 2 hours; SO3: The product obtained by centrifuging SO2 was washed 2-3 times, kept at 110℃ for 1 hour, dried under vacuum, and then ground to obtain 101 carboxylated porous tricalcium phosphate microparticles.

[0027] The coupling process of carboxyl-modified porous tricalcium phosphate microparticles with amphiphilic polymers in Example 1: S10: Wash the carboxylated porous tricalcium phosphate microparticles twice with MES buffer (MES is 2-morpholine ethanesulfonic acid) by centrifugation, and then dry them under vacuum at low temperature; S20: Disperse 100 parts of the carboxylated porous tricalcium phosphate microparticles obtained from S10 in 1000 parts of MES buffer (pH 6), and add a total of 5 parts of EDC and NHS mixture (molar ratio of EDC to NHS is 1:1, EDC is 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide, and NHS is N-hydroxysuccinimide). Stir at room temperature for 30 min to obtain the activation solution. S30: Dissolve 0.15 parts of the first amphiphilic polymer PCL(10k)-PEG(5k)-NH2 (Chinese name: polycaprolactone(10K)-polyethylene glycol(5K)-amino) and 0.38 parts of the second amphiphilic polymer PCL(14k)-PEG(4k)-NH2 (Chinese name: polycaprolactone(14K)-polyethylene glycol(4K)-amino) in 5 parts of DMSO (Chinese name: dimethyl sulfoxide), and slowly add it dropwise to the activation solution obtained in S20, and stir for 12 hours; S40: The solid product obtained from S30 was washed successively with MES buffer, PBS buffer (pH 7.4), and anhydrous ethanol, and then freeze-dried under vacuum at 40°C to obtain modified tricalcium phosphate microparticles for polymerization.

[0028] Comparative Example 1 The preparation process of the porous tricalcium phosphate microparticles in Comparative Example 1 is the same as that in Example 1.

[0029] Comparative Example 2 The preparation process and carboxyl modification of the porous tricalcium phosphate microparticles in Comparative Example 2 were the same as those in Example 1.

[0030] Comparative Example 3 The preparation process and carboxyl modification of the porous tricalcium phosphate microparticles in Comparative Example 3 were the same as those in Example 1. The coupling process of the carboxyl modified porous tricalcium phosphate microparticles and the amphiphilic polymer in Comparative Example 3 was based on Example 1, except that in S30: 0.53 parts of the amphiphilic polymer PCL(10k)-PEG(5k)-NH2 were dissolved in 5 parts of DMSO and slowly added dropwise to the activation solution obtained in S20, and stirred for 12 hours.

[0031] The performance of the polymer-modified tricalcium phosphate microparticles obtained in Example 1 and Comparative Example 3, the completely unmodified porous tricalcium phosphate microparticles of Comparative Example 1, and the carboxylated porous tricalcium phosphate microparticles of Comparative Example 2 were tested. The test process is as follows: Step 1: Dissolve 0.35g of benzoyl peroxide in 350g of styrene monomer and transfer it into a 2L reactor; A mixture of 35g deionized water and 17.5g acrylic acid was introduced into the above reaction vessel. The reaction temperature was 95℃, the stirring speed was 750rpm, and the prepolymerization was carried out for 1 hour. Step 2: Adjust the stirring speed to 350 rpm, add 3.5 g of benzoyl peroxide to the above reaction vessel, and add 1050 g of deionized water containing 1.26 g of sample as the continuous phase for suspension polymerization; set the temperature of suspension polymerization to 95℃, the stirring speed to 450 rpm, and polymerize for 6 h. After cooling to room temperature, observe the performance of the product beads.

[0032] The test results for Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3 are as follows:

[0033] Compared to Comparative Examples 1, 2, and 3, the improved performance of Example 1 may be due to the fact that during the stirring of the suspension polymerization system, the fluid inside the reactor is in a turbulent state. The dispersion of the monomer in the aqueous phase is affected by both the turbulent force that causes droplet dispersion and the viscous force that prevents droplet dispersion by the dispersant. Modifying tricalcium phosphate with two amphiphilic polymers of different hydrophilic segment lengths helps to slow down the rate of change of viscous force during the reaction process, thereby improving the uniformity of the polymer microsphere size.

[0034] 2. Examples 1, 2, 3, and 4 regarding the types of hydrophobic segments in amphiphilic polymers. Example 2

[0035] The preparation process of porous tricalcium phosphate microparticles and the carboxyl modification of porous tricalcium phosphate microparticles in Example 2 are the same as those in Example 1. The coupling process of carboxyl modified porous tricalcium phosphate microparticles and amphiphilic polymers in Example 2 is based on Example 1, except that in S30: 0.15 parts of the first amphiphilic polymer PLA(10k)-PEG(5k)-NH2 and 0.38 parts of the second amphiphilic polymer PLA(14k)-PEG(4k)-NH2 are dissolved in 5 parts of DMSO and slowly added dropwise to the activation solution obtained in S20 and stirred for 12 hours.

[0036] Example 3

[0037] The preparation process of porous tricalcium phosphate microparticles and the carboxyl modification of porous tricalcium phosphate microparticles in Example 3 are the same as those in Example 1. The coupling process of carboxyl modified porous tricalcium phosphate microparticles and amphiphilic polymers in Example 3 is based on Example 1, except that in S30: 0.15 parts of the first amphiphilic polymer PLA (10k)-PEG (5k)-NH2 and 0.38 parts of the second amphiphilic polymer PCL (14k)-PEG (4k)-NH2 are dissolved in 5 parts of DMSO and slowly added dropwise to the activation solution obtained in S20 and stirred for 12 hours.

[0038] Example 4

[0039] The preparation process of porous tricalcium phosphate microparticles and the carboxyl modification of porous tricalcium phosphate microparticles in Example 4 are the same as those in Example 1. The coupling process of carboxyl modified porous tricalcium phosphate microparticles and amphiphilic polymers in Example 4 is based on Example 1, except that in S30: 0.15 parts of the first amphiphilic polymer PCL(10k)-PEG(5k)-NH2 and 0.38 parts of the second amphiphilic polymer PLA(14k)-PEG(4k)-NH2 (Chinese name polylactic acid(10K)-polyethylene glycol(4k)-amino) are dissolved in 5 parts of DMSO and slowly added dropwise to the activation solution obtained in S20, and stirred for 12 hours.

[0040] The test results for Examples 2, 3, and 4 are as follows:

[0041] Compared with Examples 2, 3, and 4, the performance improvement of Example 1 may be due to the fact that the preferred hydrophobic segment type is beneficial to enhance the hydrophobicity of the oil phase and reduce the diffusion of styrene monomers into the aqueous phase, thereby maintaining the stability of styrene droplets and reducing the occurrence of some excessively small microspheres due to secondary nucleation of a small amount of monomers in the aqueous phase.

[0042] 3. Examples 1, 5, 6, and 7 concerning the molecular weight of the hydrophilic segments of amphiphilic polymers. Example 5

[0043] The preparation process and carboxyl modification of the porous tricalcium phosphate microparticles in Example 5 are the same as in Example 1. The coupling process of the carboxyl-modified porous tricalcium phosphate microparticles and the amphiphilic polymer in Example 5 is based on Example 1, except for S30: Dissolve 0.15 parts of the first amphiphilic polymer PCL(10k)-PEG(7k)-NH2 and 0.38 parts of the second amphiphilic polymer PCL(14k)-PEG(4k)-NH2 in 5 parts of DMSO, and slowly add the S20 activation solution dropwise, stirring for 12 hours.

[0044] Example 6

[0045] The preparation process and carboxyl modification of the porous tricalcium phosphate microparticles in Example 6 are the same as in Example 1. The coupling process of the carboxyl-modified porous tricalcium phosphate microparticles and the amphiphilic polymer in Example 6 is based on Example 1, except for S30: Dissolve 0.15 parts of the first amphiphilic polymer PCL(10k)-PEG(5k)-NH2 and 0.38 parts of the second amphiphilic polymer PCL(14k)-PEG(2.5k)-NH2 in 5 parts of DMSO, and slowly add the S20 activation solution dropwise, stirring for 12 hours.

[0046] Example 7

[0047] The preparation process and carboxyl modification of the porous tricalcium phosphate microparticles in Example 7 are the same as in Example 1. The coupling process of the carboxyl-modified porous tricalcium phosphate microparticles and the amphiphilic polymer in Example 7 is based on Example 1, except for S30: Dissolve 0.15 parts of the first amphiphilic polymer PCL(10k)-PEG(7k)-NH2 and 0.38 parts of the second amphiphilic polymer PCL(14k)-PEG(2.5k)-NH2 in 5 parts of DMSO, and slowly add the S20 activation solution dropwise, stirring for 12 hours.

[0048] The test results for Examples 5, 6, and 7 are as follows:

[0049] The beads from Examples 5, 6, and 7 all exhibited high transparency, were free of haze, and contained no air bubbles. The beads from Examples 5, 6, and 7 also showed good sphericity.

[0050] Data from Examples 1, 5, 6, and 7 show that using the optimal molecular weight of the hydrophilic segments is beneficial for preparing polystyrene microspheres with uniform particle size.

[0051] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A process for preparing tricalcium phosphate for suspension polymerization, characterized in that, Includes the following steps: S10: Tricalcium phosphate microparticles are modified with a carboxylsilane coupling agent to obtain carboxylated tricalcium phosphate microparticles; S20: Disperse carboxylated tricalcium phosphate microparticles in a buffer solution with a pH of 5.5-6.5, add EDC and NHS to the buffer solution to obtain an activated carboxylated tricalcium phosphate microparticle dispersion; The ratio of the total mass of EDC and NHS to the mass of the carboxylated porous tricalcium phosphate microparticles is (1~10):100, and the molar ratio of EDC to NHS is 1:(0.9~1.2). S30: After dispersing the first and second amphiphilic polymers in a polymer dispersant, the activated carboxylated tricalcium phosphate microparticle dispersion obtained in S20 is added dropwise. Both the first and second amphiphilic polymers are composed of sequentially connected hydrophobic segments, hydrophilic segments, and terminal amino groups. The length of the hydrophilic segment of the first amphiphilic polymer is greater than the length of the hydrophilic segment of the second amphiphilic polymer.

2. The preparation process of tricalcium phosphate for suspension polymerization according to claim 1, characterized in that, The hydrophobic segment is selected from at least one of polylactic acid segment, polytrimethylene carbonate segment, and polycaprolactone segment, and the hydrophilic segment is selected from at least one of polyethylene glycol segment and polyacrylic acid segment.

3. The preparation process of tricalcium phosphate for suspension polymerization according to claim 2, characterized in that, The hydrophobic segments of both the first and second amphiphilic polymers are polycaprolactone segments, and the hydrophilic segments of both polymers are polyethylene glycol segments.

4. The preparation process of tricalcium phosphate for suspension polymerization according to claim 3, characterized in that, The molecular weight of the polycaprolactone segment of the first amphiphilic polymer is 7~11 kDa, and the molecular weight of the polycaprolactone segment of the second amphiphilic polymer is 12~15 kDa.

5. The preparation process of tricalcium phosphate for suspension polymerization according to claim 4, characterized in that, The first amphiphilic polymer has a polyethylene glycol segment with a molecular weight of 5-6 kDa, and the second amphiphilic polymer has a polyethylene glycol segment with a molecular weight of 3-4.8 kDa.

6. The preparation process of tricalcium phosphate for suspension polymerization according to claim 1, characterized in that, In S10, the mass ratio of the carboxylated tricalcium phosphate microparticles to the carboxysilane coupling agent is 100:(0.5~2).

7. The preparation process of tricalcium phosphate for suspension polymerization according to claim 6, characterized in that, The mass ratio of the carboxylated tricalcium phosphate microparticles to the first amphiphilic polymer in S30 is 100: (0.1~0.2).

8. The preparation process of tricalcium phosphate for suspension polymerization according to claim 7, characterized in that, The mass ratio of the first amphiphilic polymer and the second amphiphilic polymer in S30 is 1:(2~3).

9. The preparation process of tricalcium phosphate for suspension polymerization according to claim 1, characterized in that, The carboxysilane coupling agent is at least one selected from triethoxysilylpropylmaleamic acid and carboxylated polyethylene glycol silane.

10. A modified tricalcium phosphate, prepared by the process for preparing tricalcium phosphate for suspension polymerization according to any one of claims 1 to 9.