A hydrocarbon wax and its preparation method

By using chromium coordination catalysts to catalyze ethylene polymerization, the problems of inaccurate melting point control and high energy consumption in the preparation of traditional hydrocarbon waxes have been solved, enabling the preparation of high-purity hydrocarbon waxes that meet the precise melting point requirements of specific application scenarios.

CN123106957APending Publication Date: 2026-11-17SHANGHAI INST OF ORGANIC CHEM CHINESE ACAD OF SCI
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510635748.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional methods for preparing hydrocarbon waxes suffer from problems such as inaccurate melting point control, insufficient product purity, complex processes, and high energy consumption, making it difficult to meet the precise requirements of specific application scenarios.

Method used

High-purity hydrocarbon waxes were prepared by catalyzing the polymerization of ethylene under specific conditions using chromium coordination catalysts and co-catalysts. The melting point was precisely controlled by adjusting the reaction temperature, pressure, and solvent selection.

Benefits of technology

A hydrocarbon wax with a narrow melting point range and high purity was prepared to meet specific application requirements. The process is simple and has low energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005406603220000021
    Figure BDA0005406603220000021
  • Figure BDA0005406603220000022
    Figure BDA0005406603220000022
  • Figure BDA0005406603220000031
    Figure BDA0005406603220000031
Patent Text Reader

Abstract

This invention discloses a hydrocarbon wax and its preparation method. Specifically, it has the following characteristics: (a) a white powder, free from visible mechanical impurities; inorganic content <100ppm; metal content <10ppm; (b) a peak melting temperature T. pm (c) Number-average molecular weight is 600-4000 g / mol, and molecular weight distribution is <3; (d) Temperature T for 5% thermal weight loss. d5 ≥300℃; and / or (e) solubility in alkanes: at >90℃, solubility ≥8 g / 100 mL.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the fields of petrochemicals and fine chemicals. Specifically, this invention relates to a hydrocarbon wax and its preparation method. Background Technology

[0002] Hydrocarbon wax is a type of hydrocarbon wax composed of high-carbon straight-chain alkanes (usually C46-244-3 ...54-344-354-344-354-344-354-344 20 To C 40 + Hydrocarbon waxes are solid mixtures of hydrocarbons, characterized by high melting points, high hardness, and good chemical stability, and are widely used in candle manufacturing, packaging materials, coatings, inks, cosmetics, and hot melt adhesives. Traditional methods for preparing hydrocarbon waxes mainly include crude oil distillation, Fischer-Tropsch synthesis, and natural mineral wax refining. However, these methods suffer from problems such as inaccurate melting point control, insufficient product purity, complex processes, and high energy consumption. For example, hydrocarbon waxes prepared by traditional methods have a wide melting point range (typically 60-100℃ or higher), making it difficult to meet the precise melting point requirements of specific applications; simultaneously, the products often contain impurities such as branched alkanes and cycloalkanes, affecting their performance and application effects.

[0003] Therefore, there is an urgent need in this field to develop hydrocarbon waxes with higher purity, simpler processes, and lower energy consumption, as well as their preparation methods, to meet the precise melting point requirements of specific scenarios. Summary of the Invention

[0004] One object of the present invention is to provide a high-purity hydrocarbon wax with a narrow melting point range.

[0005] Another object of the present invention is to provide a method for preparing high-purity hydrocarbon wax.

[0006] In a first aspect of the invention, a hydrocarbon wax is provided, having the following characteristics:

[0007] (a) White powder, free from visible mechanical impurities; inorganic content <100ppm; metal content <10ppm;

[0008] (b) Peak melting temperature T pm The temperature is 90-110℃, the enthalpy of melting is ≥180J / g, and the bimodal integral area ratio (A / B) is not less than 3;

[0009] (c) Number-average molecular weight is 600-4000 g / mol, and molecular weight distribution is <3;

[0010] (d) Temperature T at which thermal weight loss is 5% d5 ≥300℃; and / or

[0011] (e) Solubility in alkanes: Solubility ≥8 g / 100 mL at >90 °C.

[0012] In another preferred embodiment, the hydrocarbon wax has a melting point of 90-105°C.

[0013] In another preferred embodiment, the number-average molecular weight of the hydrocarbon wax is 600-2000 g / mol, more preferably 650-1500 g / mol.

[0014] In another preferred embodiment, the molecular weight distribution is <2.5.

[0015] In another preferred embodiment, the molecular chain of the hydrocarbon wax contains carbon-carbon double bonds, and the carbon-carbon double bonds are terminal double bonds.

[0016] In another preferred embodiment, the alkane is a high-boiling-range alkane, preferably a high-boiling-range petroleum ether, heptane, or octane.

[0017] In another preferred embodiment, the hydrocarbon wax exhibits a 5% thermal weight loss at temperature T. d5 ≥330℃.

[0018] In a second aspect of the present invention, a method for preparing the hydrocarbon wax described in the first aspect of the present invention is provided, comprising the following steps:

[0019] In the presence of a catalyst and a co-catalyst, ethylene undergoes a catalytic polymerization reaction to obtain the aforementioned hydrocarbon wax;

[0020] The catalyst is obtained by reacting the ligand represented by Formula I with a chromium compound:

[0021]

[0022] Wherein, R1 is selected from C1-C10 straight-chain alkyl, preferably C3-C8 straight-chain alkyl; R2 is selected from the group consisting of H and C1-C4 alkyl.

[0023] In another preferred embodiment, R2 is selected from the group consisting of H, methyl, ethyl, n-propyl, and n-butyl.

[0024] In another preferred embodiment, the catalyst is prepared by the following method:

[0025] Under inert gas protection, equimolar amounts of chromium compound and ligand are placed in solvent 1 and stirred for 10-60 minutes. After removing solvent 1 under reduced pressure, solvent 2 is added to prepare a catalyst solution, which is then directly used for the catalytic polymerization of ethylene.

[0026] The ligand has the structure shown in Formula I:

[0027]

[0028] Wherein, R1 is selected from C1-C10 straight-chain alkyl, preferably C3-C8 straight-chain alkyl; R2 is selected from the group consisting of H and C1-C4 alkyl.

[0029] In another preferred embodiment, the solvent 1 is selected from the group consisting of ether solvents, aromatic solvents, or combinations thereof; preferably tetrahydrofuran, anhydrous diethyl ether, or toluene.

[0030] In another preferred embodiment, the solvent 2 is selected from the group consisting of aromatic solvents, C6-C10 alkane solvents, or combinations thereof, preferably toluene or hexane.

[0031] In another preferred embodiment, solvent 1 and solvent 2 are not the same.

[0032] In another preferred embodiment, the method for preparing the hydrocarbon wax includes the following steps:

[0033] In the presence of a catalyst and a co-catalyst, ethylene is catalytically polymerized at 20-100°C and 0.5-8.0 MPa ethylene pressure to obtain the aforementioned hydrocarbon wax.

[0034] In another preferred embodiment, the ethylene pressure is 0.5-2.0 MPa.

[0035] In another preferred embodiment, the chromium compound is selected from the group consisting of chromium trichloride, chromium trichloride tetrahydrofuran, p-tolyl chromium dichloride tetrahydrofuran, and benzyl chromium dichloride, or combinations thereof.

[0036] In another preferred embodiment, the molar ratio of the chromium compound to the ligand is 1:(1±0.2).

[0037] In another preferred embodiment, the ligand is selected from the group consisting of:

[0038]

[0039] In another preferred embodiment, the cocatalyst is selected from the group consisting of: dichloroethylaluminum, diethylaluminum chloride, triethylaluminum, triisobutylaluminum, ethylaluminum sesquichloride, butylaluminum sesquichloride, aluminumoxane, or methylaluminoxane.

[0040] In another preferred embodiment, the catalyst is prepared in situ.

[0041] In another preferred embodiment, the molar ratio of the co-catalyst to the catalyst is 100-4000:1; more preferably 100-2000:1; and more preferably 500-1500:1.

[0042] In a third aspect of the invention, a use is provided for the hydrocarbon wax described in the first aspect of the invention as a lubricant, dispersant, release agent, additive, and desensitizer.

[0043] It should be understood that, within the scope of this invention, the above-described technical features of this invention and the technical features specifically described below (such as in the embodiments) can be combined with each other to form new or preferred technical solutions. Due to space limitations, they will not be described in detail here. Attached Figure Description

[0044] Figure 1 The DSC spectrum of the hydrocarbon wax prepared in Example 3 is shown. Detailed Implementation

[0045] Through extensive and in-depth research, the inventors have, for the first time, provided a high-purity hydrocarbon wax with a narrow melting point range of 90-110℃ and its preparation method. The hydrocarbon wax is obtained by catalytic polymerization of ethylene under specific temperature and pressure conditions, with the aid of a chromium coordination catalyst and a co-catalyst. The hydrocarbon wax prepared by this invention has high purity, allows for precise control of the melting point, and reduces energy consumption. Based on these findings, the inventors completed this invention.

[0046] Hydrocarbon wax

[0047] This invention provides a high-purity hydrocarbon wax, specifically, the hydrocarbon wax has the following characteristics:

[0048] (1) White powder, free of visible mechanical impurities; inorganic content <100ppm; metal content <10ppm; indicating that the hydrocarbon wax of the present invention has high purity;

[0049] (2) Peak melting temperature T pm The melting point is 90-110℃, preferably 90-105℃, with a melting enthalpy ≥180J / g; and the bimodal integral area ratio (A / B) is not less than 3; indicating that the alkane wax of the present invention has a narrow melting point range and can precisely control the melting point;

[0050] (3) Temperature T at which thermal weight loss is 5% d5 ≥300℃; optimal temperature T d5 ≥330℃.

[0051] (4) The number-average molecular weight is 600-4000 g / mol, the molecular weight distribution is <3, and the molecular weight distribution is preferably <2.5;

[0052] (5) Solubility in alkanes: >90℃, solubility ≥8g / 100mL.

[0053] The test methods for the above-mentioned characteristics of hydrocarbon waxes are all conventional testing methods well known to those skilled in the art, as detailed below:

[0054] (1) The metal content can be obtained through elemental analysis;

[0055] (2) The content of inorganic matter can be obtained by ash content determination or thermogravimetric analysis;

[0056] (3) The peak melting temperature T of the polymer was obtained by DSC testing. pm and enthalpy of fusion;

[0057] (4) The temperature at which the polymer loses 5% of its thermal weight is obtained by TGA test; the temperature is controlled to rise from room temperature to 600.0℃ while maintaining a heating rate of 10.0℃ / min; nitrogen flow rate: 50.0mL / min and nitrogen is maintained for 1-2 hours before the test begins.

[0058] (5) The number-average molecular weight and molecular weight distribution of the polymer were obtained by GPC testing;

[0059] (6) Solubility test method: Weigh a certain amount of polymer sample and add it to petroleum ether with a boiling range of (90~120)℃. Heat and reflux with stirring until the sample is completely dissolved in petroleum ether and the system is visually clear. Record the amount of sample dissolved and the volume of solvent at this time, in g / 100mL.

[0060] Preparation method of hydrocarbon wax

[0061] The hydrocarbon wax of the present invention is prepared by a metal coordination catalyst catalysis method. However, the specific conditions of this method, such as reactants, solvents, amounts of compounds used, pressure, reaction temperature, and reaction time, are not limited to those explained below. The hydrocarbon wax of the present invention can also be conveniently prepared by optionally combining various synthetic methods described in this specification or known in the art, such combinations can be easily performed by those skilled in the art.

[0062] In the preparation method of this invention, each reaction is typically carried out in an inert solvent at 0-100°C (preferably 20-80°C). The reaction time is typically 0.1-60 h; preferably 0.5-48 h (1-12 h, 1-6 h, 1-2 h). The pressure for catalytic ethylene polymerization can be any pressure within the ethylene pressure range of 0.5-8.0 MPa, but an appropriate reaction pressure can optimize the corresponding catalytic activity; preferably, the ethylene pressure is 0.5-1.0 MPa. Specifically, the method of this invention uses a chromium coordination compound as a catalyst, which, in synergistic effect with a co-catalyst, catalyzes the polymerization of ethylene to obtain hydrocarbon waxes with terminal double bonds. Compared with other conventional methods, the preparation process of the hydrocarbon waxes of this invention is simple, energy-efficient, and allows for precise control of the melting point.

[0063] Specifically, the method for preparing hydrocarbon wax of the present invention includes the following steps:

[0064] In the presence of a catalyst and a co-catalyst, ethylene undergoes a catalytic polymerization reaction to obtain the aforementioned hydrocarbon wax;

[0065] The catalyst is obtained by reacting the ligand represented by Formula I with a chromium compound:

[0066]

[0067] Wherein, R1 is selected from C1-C10 straight-chain alkyl groups, preferably C3-C8 straight-chain alkyl groups; R2 is selected from the group consisting of H and C1-C4 alkyl groups. As used herein, the term "C1-C10 straight-chain alkyl" refers to a saturated aliphatic hydrocarbon group, including a straight-chain group containing 1-10 carbon atoms, preferably an alkyl group containing 3-8 carbon atoms, such as n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, etc.

[0068] The preparation method of the hydrocarbon wax of the present invention further includes adding silica gel or diatomaceous earth, heating and refluxing for 1-2 hours, filtering while hot to remove inorganic matter or metal, and drying to obtain the polyethylene wax.

[0069] In one specific embodiment, the reaction of the present invention is carried out in the presence of an inert gas. The inert gas described in this invention is a commonly used inert gas in the art, such as N2, Ar, etc.

[0070] In one specific embodiment, the catalyst is the chromium catalyst disclosed in patent CN102443082B, or prepared using the method disclosed in patent CN102443082B.

[0071] In one specific embodiment, the molar ratio of the ligand represented by Formula I to the chromium compound in the catalyst is 1:(1±0.2); preferably 1:(1±0.1); more preferably an equimolar ratio.

[0072] In one specific embodiment, the hydrocarbon wax is prepared by the following steps:

[0073] In the presence of a catalyst and a co-catalyst, ethylene is catalytically polymerized at 20-100°C and 0.5-8.0 MPa ethylene pressure to obtain the aforementioned hydrocarbon wax.

[0074] Preferably, the ethylene pressure is 0.5-2.0 MPa.

[0075] Representative examples of cocatalysts include (but are not limited to): dichloroethylaluminum, diethylaluminum chloride, triethylaluminum, triisobutylaluminum, ethylaluminum sesquichloride, butylaluminum sesquichloride, aluminumoxane, or methylaluminoxane.

[0076] In one specific embodiment, the catalyst is prepared by the following method:

[0077] Under inert gas protection, equimolar amounts of chromium compound and ligand are placed in solvent 1 and stirred for 10-60 minutes. After removing solvent 1 under reduced pressure, solvent 2 is added to prepare a catalyst solution of a certain concentration, which is then directly used for the catalytic polymerization of ethylene.

[0078] Solvent 1 and solvent 2 are inert solvents and are not particularly limited, including any saturated aliphatic hydrocarbons, as well as aromatic hydrocarbons and halogenated hydrocarbons. In this invention, solvent 1 is selected from the group consisting of ether solvents, aromatic solvents, or combinations thereof; preferably tetrahydrofuran, anhydrous diethyl ether, and toluene; solvent 2 is selected from the group consisting of aromatic solvents, C6-C10 alkane solvents, or combinations thereof, preferably toluene and hexane. Solvent 1 and solvent 2 may be the same or different. In one embodiment, the solvent used in the ethylene catalytic system is usually the same as the solvent used to prepare the catalyst solution.

[0079] In one specific embodiment, the molar ratio of catalyst to co-catalyst is 100-4000:1; preferably 100-2000:1; more preferably 500-1500:1.

[0080] In one embodiment, the chromium compound is selected from the group consisting of chromium trichloride, chromium trichloride tetrahydrofuran, p-tolyl chromium dichloride tetrahydrofuran, and benzyl chromium dichloride, or combinations thereof.

[0081] use

[0082] The hydrocarbon wax of this invention has a narrow melting point range, which can meet the melting point requirements of specific applications. Furthermore, the hydrocarbon wax of this invention has high purity, is free of visible mechanical impurities, and has low content of inorganic substances, metals, and other impurities; therefore, it can be used as a lubricant, dispersant, mold release agent, additive, and desensitizer.

[0083] Compared with the prior art, the main advantages of the present invention include:

[0084] (1) The hydrocarbon wax provided by the present invention has high purity, is a white powder, and has no visible mechanical impurities; the inorganic content is <100ppm; and the metal content is <10ppm.

[0085] (2) The preparation method of hydrocarbon wax of the present invention is simple and energy-efficient, and can meet the precise requirements of melting point in specific scenarios.

[0086] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Experimental methods in the following embodiments, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. Percentages and parts are by weight unless otherwise stated.

[0087] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as are familiar to those skilled in the art. Furthermore, any methods and materials similar to or equivalent to those described herein may be applied to the methods of this invention. The preferred embodiments and materials described herein are for illustrative purposes only.

[0088] Example 1: Synthesis of ligand L1

[0089]

[0090] Add to a 100 mL Schlenk tube Molecular sieves and Si-Al were used. A Schlenk tube was heated under reduced pressure using an oil pump to remove water from the reaction system. After cooling, furan-2-carboxaldehyde (2.3 g, 23.8 mmol), toluene (50 mL), and n-propylthioethylamine (3.0 g, 25 mmol) were added sequentially. The mixture was heated to 90 °C and reacted for 4 h. NMR spectroscopy was used to monitor the reaction progress. The mixture was filtered through diatomaceous earth, and the solvent was removed under reduced pressure to obtain a dark brown liquid. After the solvent was removed, NMR spectroscopy showed that the product was relatively pure, and the reaction proceeded directly to the next step.

[0091] The imine and methanol (40 mL) were added to a 100 mL round-bottom flask. NaBH4 (1.8 g, 47.4 mmol) was added in portions under ice bath conditions. The mixture was then stirred at room temperature for 1 hour, and the reaction was monitored using NMR. After removing the methanol, anhydrous diethyl ether was added, followed by slow addition of a saturated ammonium chloride aqueous solution while stirring. The mixture was extracted with anhydrous diethyl ether, washed, dried, and distilled under reduced pressure to obtain 3.7 g of a colorless liquid, with a yield of 78%. NMR detection: 1 H NMR (400MHz, CDCl3): δ (ppm) 7.35 (s, 1H), 6.30 (s, 1H), 6.17 (s, 1H), 3.80 (s, 2H), 2.79 (t, 2H), 2.66 (t, 2H), 2.45 (t, 2H), 1.57 (m, 2H), 0.96 (t, 3H).

[0092] Example 2: Synthesis of ligand L3

[0093]

[0094] Add to a 100 mL Schlenk tube Molecular sieves and Si-Al were used. A Schlenk tube was heated under reduced pressure using an oil pump to remove water from the reaction system. After cooling, furan-2-carboxaldehyde (1.85 g, 19.1 mmol), toluene (50 mL), and n-octylthioethylamine (3.8 g, 20 mmol) were added sequentially. The mixture was heated to 90 °C and reacted for 4 h. NMR spectroscopy was used to monitor the reaction progress. The mixture was filtered through diatomaceous earth, and the solvent was removed under reduced pressure to obtain a dark brown liquid. After drying, NMR analysis showed that the product was relatively pure, and the reaction proceeded directly to the next step.

[0095] The imine and methanol (40 mL) were added to a 100 mL round-bottom flask. NaBH4 (1.44 g, 38.1 mmol) was added in portions under ice bath conditions. The mixture was stirred at room temperature for 1 hour, and the reaction was monitored using NMR. After removing the methanol, anhydrous diethyl ether was added, followed by slow addition of a saturated ammonium chloride aqueous solution while stirring. The mixture was extracted with anhydrous diethyl ether, washed, dried, and distilled under reduced pressure to obtain 3.87 g of a yellow liquid, with a yield of 75.4%. NMR detection: 1 H NMR (400MHz, CDCl3): δ (ppm) 7.34 (s, 1H), 6.29 (s, 1H), 6.17 (s, 1H), 3.79 (s, 2H), 2. 79(t,2H),2.66(t,2H),2.46(t,2H),1.55(m,2H),1.41-1.13(br,10H),0.87(t,3H).

[0096] Example 3 High-pressure polymerization reaction

[0097] Weigh equivalent amounts of ligand L1 and chromium trichloride tetrahydrofuran into a stopcock bottle in a glove box, add THF and stir for 10 min, remove THF and then add toluene to prepare a catalyst solution of 1 μmol / mL for later use.

[0098] After drying a 1L stainless steel reactor, purged it with nitrogen and preheated the reactor to about 50°C. Add 450mL of toluene and control the stirring speed at 300rpm. After stirring for 5 minutes, add MMAO (1.88M in toluene) and stir for another 10 minutes. Then add 20µl of catalyst solution and introduce ethylene to bring the pressure inside the reactor to 1.0MPa. Control the temperature inside the reactor at 50°C and allow the polymerization reaction to proceed for 1 hour. After this, cut off the ethylene supply, cool the reaction, release the pressure inside the reactor, quench the reaction, add silica gel or diatomaceous earth to the polymer, and heat under reflux for 1-2 hours. Then filter while hot to remove inorganic or metallic impurities and dry to obtain a white powdered polymer. The specific results are shown in Table 1.

[0099] Example 4

[0100] Example 3 was repeated, except that the solvent was hexane. The specific results are shown in Table 1.

[0101] Example 5

[0102] Example 3 was repeated, except that the co-catalyst was MAO (10% in toluene), and the specific results are shown in Table 1.

[0103] Example 6

[0104] Example 3 was repeated, except that the catalyst was ligand L1 coordinated with p-tolylchromium dichloride tetrahydrofuran in an equimolar amount. The specific results are shown in Table 1.

[0105] Example 7

[0106] Example 3 was repeated, except that the catalyst was equimolarly coordinated with ligand L1 and benzyl chromium dichloride. The specific results are shown in Table 1.

[0107] Example 8

[0108] Example 3 was repeated, except that the ethylene pressure was 0.5 MPa. The specific results are shown in Table 1.

[0109] Example 9

[0110] Example 3 was repeated, except that the reaction temperature was 70°C, and the specific results are shown in Table 1.

[0111] Examples 10-12

[0112] Example 3 was repeated, except that the catalyst was coordinated with other ligands in equimolar amounts with chromium trichloride tetrahydrofuran. The specific results are shown in Table 1.

[0113] Table 1

[0114]

[0115]

[0116] As can be seen from Table 1, the hydrocarbon wax prepared by this invention has a narrow melting point range, a number-average molecular weight of 650-1500 g / mol, a thermal weight loss temperature of 5% ≥300℃, and a solubility of ≥8 g / 100 mL in alkane solvents.

[0117] Test Example 1: Solubility Test

[0118] The hydrocarbon waxes prepared in Examples 3-12 of this invention were subjected to solubility tests in high-boiling-range petroleum ether (the test methods are as described above), and the results are shown in Table 1. It can be seen that the high-melting-point polyethylene wax of this invention has a solubility ≥8 g / 100 mL in alkane solvents, indicating that the high-melting-point wax of this invention has high solubility and can form a uniform dispersion system in alkane solvents, making it suitable for applications in plastics processing, coatings, inks, hot melt adhesives, cosmetics, and other fields.

[0119] All documents mentioned in this invention are incorporated herein by reference as if each document were individually incorporated by reference. Furthermore, it should be understood that after reading the foregoing teachings of this invention, those skilled in the art can make various alterations or modifications to this invention, and these equivalent forms also fall within the scope defined by the appended claims.

Claims

1. A hydrocarbon wax, characterized in that, It has the following characteristics: (a) White powder, free from visible mechanical impurities; inorganic content <100ppm; metal content <10ppm; (b) Peak melting temperature T pm The temperature is 90-110℃, the enthalpy of melting is ≥180J / g, and the bimodal integral area ratio (A / B) is not less than 3; (c) Number-average molecular weight is 600-4000 g / mol, and molecular weight distribution is <3; (d) Temperature T at which thermal weight loss is 5% d5 ≥300℃; and / or (e) Solubility in alkanes: Solubility ≥8 g / 100 mL at >90 °C.

2. The hydrocarbon wax as described in claim 1, characterized in that, The molecular chain of the hydrocarbon wax contains carbon-carbon double bonds, and the carbon-carbon double bonds are terminal double bonds.

3. The hydrocarbon wax as described in claim 1, characterized in that, The alkane is a high-boiling-range alkane, preferably a high-boiling-range petroleum ether, heptane, or octane.

4. The hydrocarbon wax as described in claim 1, characterized in that, The temperature at which the hydrocarbon wax loses 5% of its thermal weight is T. d5 ≥330℃.

5. A method for preparing the hydrocarbon wax according to claim 1, characterized in that, Includes the following steps: In the presence of a catalyst and a co-catalyst, ethylene undergoes a catalytic polymerization reaction to obtain the aforementioned hydrocarbon wax; The catalyst is obtained by reacting the ligand represented by Formula I with a chromium compound: Wherein, R1 is selected from C1-C10 straight-chain alkyl, preferably C3-C8 straight-chain alkyl; R2 is selected from the group consisting of H and C1-C4 alkyl.

6. The preparation method according to claim 5, characterized in that, The catalyst is prepared by the following method: Under inert gas protection, equimolar amounts of chromium compound and ligand are placed in solvent 1 and stirred for 10-60 minutes. After removing solvent 1 under reduced pressure, solvent 2 is added to prepare a catalyst solution, which is then directly used for the catalytic polymerization of ethylene. The ligand has the structure shown in Formula I: Wherein, R1 is selected from C1-C10 straight-chain alkyl, preferably C3-C8 straight-chain alkyl; R2 is selected from the group consisting of H and C1-C4 alkyl.

7. The preparation method according to claim 6, characterized in that, The chromium compound is selected from the group consisting of chromium trichloride, chromium trichloride tetrahydrofuran, p-tolyl chromium dichloride tetrahydrofuran, and benzyl chromium dichloride, or combinations thereof.

8. The preparation method according to claim 6, characterized in that, The ligands are selected from the following group:

9. The preparation method according to claim 6, characterized in that, The molar ratio of the co-catalyst to the catalyst is 100-4000:1; preferably 100-2000:1; more preferably 500-1500:

1.

10. The use of the hydrocarbon wax according to claim 1, characterized in that, It is used as a lubricant, dispersant, release agent, additive, and desensitizer.

Citation Information

Patent Citations

  • Novel chromium catalyst and application thereof in catalysis of olefin oligomerization and polymerization